Method for purifying and regenerating waste iron phosphate and battery-grade iron phosphate
Through two acid-soluble crystallization operations and phosphorus replenishment of phosphorus in the phosphorus solution, the iron-phosphorus ratio is adjusted, and the iron-phosphorus ratio in waste lithium iron-phosphate batteries is solved, and low-cost and efficient iron phosphate recycling is achieved, meeting battery-grade standards.
Patent Information
- Application Number
- CN202411199847.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art is difficult to effectively recycle iron phosphate in waste lithium iron phosphate batteries, resulting in the iron-phosphorus ratio not meeting the requirements and the process cost is high, which limits the application scope of recycling products.
Using two acid-soluble crystallization operations, the iron-phosphorus ratio is adjusted through the first high-temperature crystallization and the second phosphorus acid solution to achieve the production of battery-grade iron phosphate, and the pH value is adjusted through water to avoid the use of alkali and reduce acid The consumption of acid is improved.
Iron phosphate products with an iron-phosphorus ratio in the range of 0.96 to 1 were achieved, which reduced process costs, increased yield and added value of iron phosphate, and met the impurity content requirements of battery-grade standards.
Smart Images

Figure CN119038509A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery material technology, and in particular to a method for purifying and regenerating waste iron phosphate and battery-grade iron phosphate. Background Art
[0002] With the rapid development of the economy, energy and environmental issues have become the focus of people's attention. In recent years, a large number of retired lithium iron phosphate batteries have appeared, and the number is showing a rapid growth trend. The harmful parts of retired lithium iron phosphate batteries will cause serious pollution after entering the environment. Recycling waste lithium iron phosphate batteries not only solves environmental problems, but also brings certain economic benefits. In addition, the safety hazards such as fire and explosion caused by waste lithium iron phosphate should not be underestimated. Therefore, recycling waste lithium iron phosphate batteries is imminent.
[0003] The existing recycling of lithium iron phosphate from waste lithium iron phosphate batteries generally uses an acid solution and a combined oxidant to leach lithium from lithium iron phosphate waste. However, the iron phosphate after lithium extraction often does not meet the requirements due to the impurity content and Fe:P ratio, so it is discarded as residue. For example, a document discloses a new oxidation leaching method for waste lithium iron phosphate, which uses the inherent oxidation / reduction characteristics of LCO and LFP to recover lithium, cobalt, iron, phosphorus and other elements. Although this method effectively reduces the consumption of chemicals, its final product types cannot meet the requirements of the iron phosphate field, thereby limiting the application scope of the recycled products.
[0004] However, if you want the iron phosphate after lithium extraction to meet the Fe:P ratio requirements, it often requires a more complicated process with high costs, while the market price of iron phosphate is relatively low. From the perspective of actual production, the iron phosphate after lithium extraction is usually discarded as residue. Therefore, it is urgent to provide an iron phosphate purification process that can meet the Fe:P ratio requirements and impurity content requirements while maintaining a low cost. Summary of the invention
[0005] In view of this, the present application provides a method for purifying and regenerating waste iron phosphate, battery-grade iron phosphate. The method can obtain an iron phosphate product with an iron-phosphorus ratio (Fe:P, molar ratio) that meets the requirements. During the operation, two different acid dissolution and crystallization operations are used to adjust the iron-phosphorus ratio in the system to finally obtain battery-grade iron phosphate (i.e., Fe:P is in the range of 0.96 to 1), and avoids the use of alkali to adjust the pH, significantly reducing the acid consumption, and the acid recycling rate is very high, achieving low-cost production.
[0006] In a first aspect, the present application provides a method for purifying and regenerating waste iron phosphate, comprising the following steps: S100, obtaining waste iron phosphate, dissolving the waste iron phosphate with an acid solution, filtering, and obtaining a waste solution; S200, diluting the waste solution with water (adjusting the pH), performing high-temperature crystallization (first recrystallization), filtering, and obtaining a first iron phosphate filter residue and a filtrate, wherein the contents of Fe and P in the first iron phosphate filter residue do not meet the product content requirements (i.e., Fe:P is not within the range of 0.96 to 1); S300, adding the first iron phosphate filter residue to a phosphoric acid solution for cleaning and phosphorus supplementation (second recrystallization), filtering, and obtaining a second iron phosphate filter residue; S400, calcining the second iron phosphate filter residue to obtain battery-grade iron phosphate (Fe:P=0.96 to 1).
[0007] Waste iron phosphate includes the ferrophosphorus slag remaining after recovering lithium from the positive electrode waste of waste lithium iron phosphate batteries, and also includes the ferrophosphorus slag remaining after recovering lithium from unqualified lithium iron phosphate batteries or eliminated positive electrode waste of lithium iron phosphate batteries.
[0008] The present application adopts the method of coordinated two acid dissolutions and temperature rise recrystallizations to adjust the iron-phosphorus ratio in steps, and obtains an iron phosphate product that meets the requirements, that is, first dissolve using an acid solution such as hydrochloric acid, sulfuric acid, etc., and adjust the pH using water, and then crystallize at high temperature. After the first crystallization, the first iron phosphate filter residue is obtained. At this time, the iron-phosphorus ratio cannot meet the product requirements, so phosphoric acid is continued to be used for secondary dissolution and high-temperature crystallization. The phosphoric acid solution not only provides a stable environment and acidic conditions for the precipitation and crystallization of iron phosphate, but also plays the role of further adjusting the phosphorus content in the crystal. The method in the present application also greatly reduces the amount of acid added in the traditional method. This is because the synthesis of traditional iron phosphate products is usually one-step acid addition and alkali is added to adjust the pH. The introduction of alkali consumes acid and causes acid waste. The present application changes the pH of the solution by adding water, avoiding the use of alkali, and also avoiding the introduction of alkali impurities. Moreover, since water is used to adjust the pH, the filtrate can realize the recycling of acid only through a simple evaporation step, and the recycling rate of acid is very high. After two recrystallizations and roasting, iron phosphate that meets the requirements of the iron-phosphorus ratio can be obtained. It can be seen that the method of the present application takes into account reducing the consumption of the acid solution, helping to reduce costs and obtaining iron phosphate products that meet the requirements, and the iron phosphate yield is high, which increases the added value of waste lithium iron phosphate products.
[0009] In some embodiments, in step S100, at least one of the following conditions is met: Condition A: the liquid-to-solid ratio of waste iron phosphate and acid solution is 18 ml / g to 22 ml / g; Condition B: the pH value of the acid solution is -2 to 1.5; preferably, the pH value of the acid solution is 0 to 0.5; Condition C: the acid solution is selected from at least one of hydrochloric acid solution, sulfuric acid solution or nitric acid solution. The present application uses the above-mentioned type and pH range of acid solution to dissolve waste iron phosphate, and when the liquid-to-solid ratio of waste iron phosphate and acid solution is also in a suitable range, it is conducive to the efficient dissolution of waste iron phosphate.
[0010] Furthermore, in some embodiments, in step S100, the use of a strong acid (such as at least one of a hydrochloric acid solution, a sulfuric acid solution or a nitric acid solution) can not only achieve a good dissolution effect, but also requires a lower acid concentration. A low concentration of strong acid is beneficial for reducing the amount of water used in the subsequent pH regulation process using water, and the high recrystallization time will also be reduced accordingly, thereby reducing energy consumption.
[0011] In some embodiments, in step S200, diluting the waste solution with water includes: diluting the waste solution with water to a pH value of 0.7 to 2.5. Preferably, the waste solution is diluted with water to a pH value of 0.9 to 1.5. The present application uses water dilution to adjust the pH value of the solution, which not only avoids the use of alkali, but also allows the acid to be recycled through a simple evaporation step, thereby reducing acid consumption and improving acid utilization. In particular, the pH value of the waste solution is regulated within the above range to prevent Fe in the solution. 3+ Hydrolysis generates Fe(OH)3, which avoids affecting the iron-phosphorus ratio in the product and increases the yield of the iron phosphate (i.e., the first iron phosphate residue) obtained by the first recrystallization.
[0012] In some embodiments, in step S200, the conditions for high temperature crystallization are: temperature: 70°C to 110°C, time: 3h to 6h. The present application adopts high temperature crystallization in step S200. At a higher temperature, the solubility of iron phosphate decreases, which can increase the precipitation amount of iron phosphate.
[0013] In some embodiments, step S200 further includes adding an oxidant during the dilution process of the waste solution, wherein the oxidant includes hydrogen peroxide, wherein the mass concentration of the hydrogen peroxide is 25wt% to 30wt%, and the amount of hydrogen peroxide is: 2ml to 4ml of hydrogen peroxide for every 10g of waste iron phosphate. 2+ Oxidized to Fe 3+, avoiding affecting the iron-phosphorus ratio in subsequent products, and the appropriate type of oxidant takes into account the improvement of product yield. In this process, 5g of waste iron phosphate only consumes 1-2mL H2O2 in each cycle reaction process, which greatly reduces the consumption of oxidants compared to traditional methods.
[0014] In some embodiments, in step S300, the pH value of the phosphoric acid solution is 0.5 to 3, and the amount of the phosphoric acid solution is: 200 ml to 400 ml of the phosphoric acid solution is used for every 10 g of waste iron phosphate. During the secondary recrystallization process, phosphoric acid with a pH value of 0.5 to 3 is used for high-temperature cleaning and phosphorus supplementation, which can not only provide an acid environment that satisfies the crystallization, but also provide sufficient phosphorus content, which is conducive to obtaining a final product with an iron-phosphorus ratio that meets the requirements.
[0015] In some embodiments, in step S300, during the cleaning and phosphorus supplementation, the first iron phosphate filter residue is subjected to secondary recrystallization. Preferably, the conditions for cleaning and phosphorus supplementation are: cleaning temperature: 70°C to 110°C, number of cleanings: 2 to 3 times, single cleaning time: 1h to 2h, total cleaning time: 3h to 6h. During the cleaning and phosphorus supplementation process, only 2-3 cleanings are required to obtain a product with an iron-phosphorus ratio that meets the requirements, which reduces the number of cleanings, avoids the loss of iron phosphate due to cleaning, and improves the iron phosphate yield.
[0016] In this process, the temperature of the first recrystallization and the second recrystallization are both 70-110°C. If the temperature is too low, the iron phosphate cannot be recrystallized. If the temperature is too high, water evaporates quickly, so that the pH value of the solution cannot meet the requirements of recrystallization.
[0017] In some embodiments, the filtrate in step S200 is heated and evaporated to a pH value of -2 to 1.5, and step S100 is repeated to dissolve the waste iron phosphate. That is, when the filtrate in step S200 is evaporated to the pH range of the original solution (i.e., the acid solution), the waste iron phosphate is dissolved again. It can be seen that the acid used in the process of dissolving the waste iron phosphate in this application can be recycled and the recovery rate is very high.
[0018] In a second aspect, the present application provides battery-grade iron phosphate prepared by any one of the methods of the first aspect above.
[0019] In the present application, two high-temperature crystallizations are used. In the first, waste ferric phosphate is dissolved with acids such as sulfuric acid, hydrochloric acid, and nitric acid. The first high-temperature crystallization is performed at an appropriate pH to adjust the iron-phosphorus ratio for the first time. Then, phosphoric acid is used to dissolve phosphorus. The second high-temperature crystallization is performed at an appropriate pH to adjust the iron-phosphorus ratio for the second time. Through two high-temperature crystallizations, and the two high-temperature crystallizations use different process methods, an ferric phosphate product that meets the iron-phosphorus ratio requirements can be obtained, and the ferric phosphate yield is relatively high.
[0020] The method of the present application uses a smaller amount of acid than the traditional method to dissolve the iron ions and phosphate ions in the waste iron phosphate, obtain a suitable waste solution, and then adjust the pH value of the waste solution to a suitable range by water. On the one hand, adjusting the pH value with water is conducive to the recycling of the acid solution, and the absence of the addition of alkali will significantly reduce the acid consumption, which is conducive to saving process costs, and on the other hand, other impurity ions will not be introduced; the appropriate pH range can also avoid the hydrolysis of trivalent iron ions in the solution to generate Fe(OH)3, so that the iron and phosphorus contents in the first iron phosphate filter residue are appropriate, which is conducive to the subsequent process of cleaning and phosphorus supplementation for the second recrystallization, and a product that meets the iron-phosphorus ratio requirements is obtained, and the yield of iron phosphate obtained by the first recrystallization is relatively high. The acid dissolution combined with the two recrystallizations is conducive to impurity removal, thereby obtaining a battery-grade iron phosphate with a high yield and an impurity content that meets industry requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0022] Figure 1 The figure is a schematic diagram of the process flow of the method for purifying and regenerating waste iron phosphate in the present application. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0024] Method for purifying and regenerating waste iron phosphate
[0025] See also Figure 1 , including the following steps:
[0026] S100, obtaining waste iron phosphate, dissolving the waste iron phosphate with an acid solution (such as a hydrochloric acid solution, a sulfuric acid solution, or a nitric acid solution) (such as dissolving at room temperature), filtering, and obtaining a waste solution;
[0027] S200, diluting the waste solution with water (adding water to adjust the pH), performing high temperature crystallization (heating crystallization, i.e., the first high temperature crystallization), filtering, and obtaining a first iron phosphate filter residue and a filtrate;
[0028] S300, adding the first iron phosphate filter residue to a phosphoric acid solution (dilute phosphoric acid) for washing and phosphorus supplementation (i.e., second high-temperature crystallization), filtering, and obtaining a second iron phosphate filter residue;
[0029] S400, calcining the second iron phosphate filter residue (600°C-800°C) to obtain battery-grade iron phosphate.
[0030] The filtrate in step S200 is heated and evaporated to a pH value of -2 to 1.5, and step S100 is repeated to dissolve the waste iron phosphate.
[0031] The present application adopts the method of acid dissolution combined with two high-temperature crystallizations to prepare battery-grade iron phosphate that meets product requirements. Specifically, two different acid dissolution high-temperature crystallizations are used to control the pH of each crystallization process, thereby achieving the regulation of the iron-phosphorus ratio, and no alkali is added to adjust the pH in the entire process, which is not only conducive to the recycling of the acid solution, but also significantly reduces the consumption of the acid solution. Heating recrystallization (high-temperature recrystallization) further reduces the demand for the acid solution.
[0032] The synergistic cooperation of the two acid dissolution and high-temperature recrystallization processes can not only obtain iron phosphate with a suitable Fe:P value, but also a low impurity content. The product is battery-grade FePO4 and its yield is also high.
[0033] In this process, further, in the first acid dissolution crystallization process, the use of strong acid can not only achieve a good dissolution effect, but also in the subsequent process of using water to control the pH, the amount of water used is small, the high recrystallization time will be correspondingly reduced, and the energy consumption is reduced.
[0034] In some embodiments, in step S100, at least one of the following conditions is met: Condition A: the liquid-to-solid ratio of waste iron phosphate and acid solution is 18 ml / g to 22 ml / g, Condition B: the pH value of the acid solution is -2 to 1.5, and Condition C: the acid solution is selected from at least one of hydrochloric acid solution, sulfuric acid solution, or nitric acid solution. Exemplarily, the liquid-to-solid ratio of waste iron phosphate and acid solution is 18 ml / g, 18.5 ml / g, 19 ml / g, 19.5 ml / g, 20 ml / g, 20.5 ml / g, 21 ml / g, 21.5 ml / g, 22 ml / g, or a value in the range of any two of these values. Exemplarily, the pH value of the acid solution is -2, -1.5, -1.0, -0.5, 0, 0.3, 0.5, 0.8, 1.0, 1.3, 1.5, or a value in the range of any two of these values.
[0035] In some embodiments, in step S200, diluting the waste solution with water includes: diluting the waste solution with water to a pH value of 0.7 to 2.5. In the present application, if too little water is added, the pH value is too low, and the iron phosphate cannot be precipitated during the temperature rise crystallization process. If too much water is added, the pH value is too high, and a large amount of Fe(OH)3 will be generated. Adjusting the pH to a range of 0.7 to 2.5 avoids Fe 3+Hydrolysis generates a large amount of Fe(OH)3, and is more conducive to obtaining products with a suitable iron-phosphorus ratio and an increase in yield. Exemplarily, the waste dissolution solution is diluted with water to a pH value of 0.7, 0.8, 0.9, 1, 1.3, 1.5, 1.8, 2, 2.3, 2.5 or a value within the range of any two of these values. Further preferably, the waste dissolution solution is diluted with water to a pH value of 0.9 to 1.5. Within this range, no white precipitate is generated during the water addition process, and the filter residue yield obtained after the first temperature increase crystallization is good, which provides a higher possibility for subsequent phosphorus supplementation by phosphate to obtain a product iron phosphate that meets the requirements and has a high yield.
[0036] In some embodiments, in step S200, the conditions for high temperature crystallization are: temperature: 70°C to 110°C, time: 3h to 6h. For example, the temperature is 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, or a value in the range of any two of these values. For example, the time is 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, or a value in the range of any two of these values.
[0037] In some embodiments, step S200 also includes adding an oxidant during the dilution process of the waste solution, wherein the oxidant includes hydrogen peroxide, the mass concentration of the hydrogen peroxide is 25wt% to 30wt%, and the amount of hydrogen peroxide is: 2ml to 4ml of the hydrogen peroxide for every 10g of the waste iron phosphate. Selecting a suitable amount of oxidant can reduce the Fe in the lithium iron phosphate waste. 2+ Effectively oxidized. Exemplarily, the mass concentration of hydrogen peroxide is 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt% or a value within the range consisting of any two of these values.
[0038] In some embodiments, in step S300, the pH value of the phosphoric acid solution is 0.5 to 3, and the amount of the phosphoric acid solution is: for every 10g of waste iron phosphate, 200ml to 400ml of phosphoric acid solution is used. In the present application, the first iron phosphate residue does not meet the iron-phosphorus ratio range of the battery-grade standard FePO4, and the phosphoric acid solution under suitable conditions is continued to be crystallized at high temperature to obtain an iron phosphate product that meets the industry requirements, that is, the ratio of iron and phosphorus in the first iron phosphate residue is adjusted by phosphoric acid, and a stable crystallization environment and acidic conditions are provided to obtain a product that meets the iron-phosphorus ratio requirements, and the pH value of the phosphoric acid solution is in the above range, which is more conducive to improving the yield of the product and obtaining a suitable iron-phosphorus ratio. Exemplarily, the pH value of the phosphoric acid solution is 0.5, 0.8, 1, 1.5, 1.8, 2, 2.5, 2.8, 3 or a value within the range composed of any two of these values.
[0039] In some embodiments, in step S300, when washing and replenishing phosphorus, the first iron phosphate filter residue is subjected to secondary recrystallization, and the conditions for washing and replenishing phosphorus are: washing temperature: 70°C to 110°C, number of washings: 2 to 3 times, single washing time: 1h to 2h, total washing time: 3h to 6h. Exemplarily, the washing temperature is 70°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C or a value in the range of any two of these values. Exemplarily, the single washing time is 1h, 1.3h, 1.5h, 1.8h, 2h or a value in the range of any two of these values. Exemplarily, the total washing time is 3h, 4h, 5h, 6h or a value in the range of any two of these values, and the total washing time is the product of the single washing time and the number of washings.
[0040] The following are possible implementations
[0041] The residue (i.e., waste iron phosphate) after lithium is recovered from waste lithium iron phosphate (for example, leaching by FeCl3 solution, high pressure oxygen leaching, calcination and dilute acid dissolution, etc.) is added to an acid solution (HCl, H2SO4, H3PO4, HNO3, pH = -2 to 1.5), and dissolved for 6 to 24 hours at room temperature, preferably, for 6 to 12 hours. After the dissolution is completed, the solution is filtered, and the residue is collected for the next dissolution. Water is added to the filtrate to adjust the pH to 0.7 to 2.5, and hydrogen peroxide (1 to 2 ml for every 5 g of waste iron phosphate) can be added. Then, the solution is placed in a water bath and heated (70 to 110° C.) for recrystallization. The crystallization aging time is 3-6h. After the aging time is over, filtration is performed. At this time, the contents of Fe and P in the filter residue do not meet the product content requirements. It is necessary to use dilute phosphoric acid for cleaning and phosphorus supplementation, and perform secondary recrystallization. The pH of phosphoric acid is 0.5-3, and the cleaning temperature is (70-110°C) for 2-3 times, each cleaning is 1-2h, and the total cleaning time is 3-6h. After cleaning, calcination is performed at a calcination temperature of 600-800°C for 1-3h to obtain an iron phosphate product. The iron-phosphorus content and iron-phosphorus ratio in the product meet the requirements (product requirements Fe: 35.7-36.7%, phosphorus: 20.0-21.1, iron-phosphorus ratio 0.96-1).
[0042] The filtrate needs to be concentrated by evaporation to evaporate the added water. When the pH of the solution is the same as before adding water, the evaporation is stopped and the solution is circulated again.
[0043] The waste iron phosphate residue remaining after lithium recovery from waste lithium iron phosphate in the art can be purified by the method provided by this process to obtain a product with an iron-phosphorus ratio that meets the requirements. This process does not limit the source of the waste iron phosphate residue. For example, the waste iron phosphate residue can be obtained by leaching with FeCl3 solution, high-pressure oxygen leaching, calcination and dilute acid dissolution, etc.
[0044] The benefits of this process:
[0045] 1. By adding water to change the pH of the solution, the use of alkali is avoided, and the introduction of alkali impurities is also avoided. It is worth noting that since water is used to adjust the pH, the acid can be recycled through a simple evaporation step. Since no alkali is used to adjust the pH, the acid consumption is greatly reduced and the acid recovery rate is very high.
[0046] 2. Reduce the use of H2O2. In this process, an oxidant is added to remove the residual Fe 2+ Transformed Fe 3+ , and obtain a product that meets the iron-phosphorus ratio requirements.
[0047] 3. The filtrate after crystallization filtration can be recycled again by evaporation.
[0048] 4. During the first recrystallization, the pH was adjusted to the range of 0.7-2.5 to avoid Fe 3+ Hydrolysis generates Fe(OH)3, which in turn affects the iron-phosphorus ratio in the product, and the yield of iron phosphate from the first recrystallization is higher.
[0049] 5. During the second recrystallization process, phosphoric acid with a pH of 0.5-3 is used to wash and replenish phosphorus, and the iron-phosphorus ratio is continuously adjusted. This not only can obtain a final product with an iron-phosphorus ratio that meets the requirements, but also reduces the number of washing times, thereby avoiding the loss of iron phosphate during the washing process, and also avoiding the dissolution of iron phosphate, thereby improving its yield.
[0050] Hereinafter, examples and comparative examples are given to more specifically illustrate the embodiments of the present application. Unless otherwise stated, the parts, percentages and ratios listed are all based on mass.
[0051] The lithium iron phosphate waste in the following examples and comparative examples includes unqualified lithium iron phosphate batteries and discarded lithium iron phosphate batteries. The lithium iron phosphate waste obtained by dismantling unqualified lithium iron phosphate batteries and / or discarded lithium iron phosphate batteries is simply roasted and carbon floated in an inert atmosphere to obtain lithium iron phosphate waste with organic matter and carbon removed.
[0052] Then, the lithium iron phosphate waste is reacted with hydrogen peroxide under acidic conditions to obtain waste iron phosphate and lithium leaching solution. This method is a conventional method in the art and will not be described in detail. Of course, the method for obtaining waste iron phosphate in this application is not limited to this method, and other methods known to those skilled in the art are also possible.
[0053] Example 1
[0054] Add 5g of waste ferric phosphate to 100ml of sulfuric acid solution with pH=0, dissolve it at room temperature of 20℃ for 12h, then filter the solution, collect the residue and continue to dissolve it next time, add water to the filtrate to adjust the pH (adjust to pH 1.5), and add 1ml of H2O2 at the same time. After adding water, put the solution into a water bath, adjust the temperature of the water bath to 110℃, stir and age for 3h (i.e., the first high-temperature crystallization), and then filter to obtain a residue and a filtrate. The residue is 4.6g (excluding crystallization water). At this time, the ratio of Fe to P in the residue is greater than 1, which does not meet the product content requirements.
[0055] The filter residue was placed in 100 ml of dilute phosphoric acid solution (pH 0.5), washed 3 times at 70°C, each time for 1 hour, for a total of 3 hours, i.e., secondary recrystallization. After washing, it was calcined at 600°C for 2 hours to remove crystal water, i.e., the product iron phosphate (Fe: 36.5%, P: 20.8%) met the product requirements. The filtrate was evaporated to remove the added water, to make pH = 0, and then recycled.
[0056] Example 2
[0057] Add 5g of waste ferric phosphate into 100ml of a mixed solution of sulfuric acid and hydrochloric acid at pH = 0.5 (the molar ratio of sulfuric acid to hydrochloric acid is 1:1), dissolve at room temperature 25°C for 6h, then filter the solution, collect the residue and continue to dissolve next time, add water to the filtrate to adjust the pH (adjust to pH 1), and add 1ml of H2O2 at the same time. After adding water, put the solution into a water bath, adjust the temperature of the water bath to 70°C, stir and age for 6h, and then filter to obtain a residue and a filtrate. The residue is 4.5g (excluding crystal water). At this time, the ratio of Fe to P in the residue is greater than 1, which does not meet the product content requirements.
[0058] The filter residue was placed in 100 ml of dilute phosphoric acid solution (pH 1.5), washed twice at 110°C, each time for 2 hours, for a total of 4 hours. After washing, it was calcined at 800°C for 1 hour to remove crystal water, i.e., the product iron phosphate (Fe: 36.1%, P: 20.2%) met the product requirements. The filtrate was evaporated to remove the added water, to make the pH = 0.5, and then recycled.
[0059] Example 3
[0060] Add 5g of waste ferric phosphate to 100ml of a mixed solution of hydrochloric acid and nitric acid at pH = 0.5 (the molar ratio of hydrochloric acid to nitric acid is 3:1), dissolve it at room temperature of 23°C for 10h, then filter the solution, collect the residue and continue to dissolve it next time, add water to the filtrate to adjust the pH (adjust to pH 0.9), and add 1ml of H2O2 at the same time. After adding water, put the solution into a water bath, adjust the temperature of the water bath to 90°C, stir and age it for 4h, and then filter it to obtain a residue and a filtrate. The residue is 4.6g (excluding crystal water). At this time, the ratio of Fe to P in the residue is greater than 1, which does not meet the product content requirements.
[0061] The filter residue was placed in 100 ml of dilute phosphoric acid solution (pH 3), washed 3 times at 90°C, each time for 2 hours, for a total of 6 hours. After washing, it was calcined at 750°C for 2 hours to remove crystal water, i.e., the product iron phosphate (Fe: 36.3%, P: 20.9%) met the product requirements. The filtrate was evaporated to remove the added water, making the pH = 0.5, and then recycled.
[0062] Example 4
[0063] 5g of waste iron phosphate was added to 100ml sulfuric acid solution with pH = 0, and dissolved at room temperature 20℃ for 12h, then the solution was filtered, the residue was collected and dissolved next time, water was added to the filtrate to adjust the pH (adjusted to pH 3), and 1ml H2O2 was added at the same time. During the water addition process, a large amount of white precipitate was found to be generated. Analysis of the precipitate showed that due to the high pH, Fe in the solution 3+ Hydrolysis to form Fe(OH)3 will result in the ratio of Fe to P in the final crystallized iron phosphate not meeting the requirements.
[0064] Example 5
[0065] 5g of waste ferric phosphate was added to 100ml sulfuric acid solution of pH=0, dissolved at room temperature of 20°C for 12h, then the above solution was filtered, the filter residue was collected and continued to dissolve next time, water was added to the filtrate for pH adjustment (adjusting to pH 0.5), and 1ml H2O2 was added simultaneously, after adding water, the above solution was put into a water bath, the water bath temperature was adjusted to 110°C, stirred and aged for 3h, then filtered, filter residue and filtrate were obtained, and it was found during the experiment that only a small amount of ferric phosphate filter residue would precipitate (0.5g, without crystal water being counted) during the crystallization process. The secondary recrystallization process is the same as in Example 2, and will not be repeated here, and the obtained product ferric phosphate, the iron-phosphorus ratio in the product meets the product requirements.
[0066] Comparing Example 4 and Example 5 with Example 1, it can be seen that the appropriate amount of water added can not only reduce the acid consumption and improve the recycling rate of the acid, but also is conducive to obtaining an iron phosphate product that meets the requirements and has a high yield.
[0067] Example 6
[0068] 5 g of waste ferric phosphate was added to a mixed solution of 100 ml of sulfuric acid and hydrochloric acid at pH = 0.5, and dissolved at room temperature of 25°C for 6 hours. Then the solution was filtered, and the residue was collected and dissolved next time. Water was added to the filtrate to adjust the pH (adjusted to pH 1), and 1 ml of H2O2 was added at the same time. After adding water, the solution was placed in a water bath, the temperature of the water bath was adjusted to 70°C, stirred and aged for 6 hours, and then filtered to obtain a residue and a filtrate. At this time, the ratio of Fe to P in the residue was greater than 1, which did not meet the product content requirements.
[0069] The filter residue was put into 100 ml of dilute phosphoric acid solution (pH 3.5) and washed twice at 110°C, with each soaking and washing for 2 hours, for a total of 4 hours. At this time, the ratio of Fe to P was greater than 1, which did not meet the product content requirements. The washing was continued for 7 times (washing conditions were the same as above). At this time, the ratio of Fe to P met the requirements, but the washing process would cause a large loss of iron phosphate.
[0070] Example 7
[0071] Add 5g of waste ferric phosphate to 100ml of a mixed solution of sulfuric acid and hydrochloric acid at pH = 0.5, dissolve at room temperature 25°C for 6h, then filter the solution, collect the residue and continue to dissolve next time, add water to the filtrate (adjust to pH 1), and add 1ml of H2O2 at the same time. After adding water, put the solution into a water bath, adjust the temperature of the water bath to 70°C, stir and age for 6h, and then filter to obtain a residue and a filtrate. At this time, the ratio of Fe to P in the residue is greater than 1, which does not meet the product content requirements.
[0072] The filter residue was put into 100 ml of dilute phosphoric acid solution (pH 0) and washed twice at 110°C, with each soaking and washing for 2 hours, for a total of 4 hours. The iron-to-phosphorus ratio of the obtained iron phosphate met the requirements, but due to the low pH, the iron phosphate dissolved during washing, resulting in a reduced yield.
[0073] In Table 1, the first crystallization refers to the high temperature crystallization in step S200, and the second recrystallization refers to the cleaning and phosphorus replenishment in step S300.
[0074] Table 1
[0075]
[0076] Note: “--” in Table 1 means no relevant data.
[0077] Example 8
[0078] Similar to Example 1, the difference is that the first acid dissolution crystallization process:
[0079] 5 g of waste iron phosphate was added to 100 ml of phosphoric acid solution with pH = 0, and dissolved at room temperature 20°C for 24 hours. The dissolved amount was about half of that in Example 1, and about 35% of the waste was dissolved. The dissolved amount remained almost unchanged as the dissolution time was increased.
[0080] It can be seen that in the first step of the dissolution process, medium-strong acid phosphoric acid is used to dissolve the waste iron phosphate, the dissolution amount is very small, and the dissolution time is very long.
[0081] Example 9
[0082] Similar to Example 1, the difference is that the first acid dissolution crystallization process:
[0083] 5 g of waste iron phosphate was added to 100 ml of phosphoric acid solution with a concentration of 4 mol / L, and dissolved at room temperature of 20°C for 12 h. At this time, the amount of dissolution was the same as in Example 1, and about 75% of the waste was dissolved. After filtration, water was added to adjust the pH (adjusted to pH 1.5). In this embodiment, the amount of water added was about 8 times that in Example 1, and the subsequent crystallization aging process required about 6 h.
[0084] Compared with Example 1, Example 8 requires a higher concentration of phosphoric acid to achieve the same dissolution effect. However, the use of concentrated phosphoric acid will result in a larger amount of water used in the subsequent pH adjustment process, and the aging and crystallization time will be too long.
[0085] Through Examples 8-9, it can be seen that in this process, using a strong acid in the first step of acid dissolution crystallization can achieve better dissolution effect, short dissolution time, high dissolution rate, and in the process of controlling the pH, it will also reduce the amount of water used, while reducing the time and energy consumption of the aging crystallization process.
[0086] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for purifying and regenerating waste iron phosphate, characterized in that: The following steps are involved: S100, obtaining waste iron phosphate, dissolving the waste iron phosphate with an acid solution, filtering, and obtaining a waste solution; S200, diluting the waste material solution with water, performing high temperature crystallization, and filtering to obtain a first iron phosphate filter residue and a filtrate; S300, adding the first iron phosphate filter residue to a phosphoric acid solution for cleaning and phosphorus supplementation, and filtering to obtain a second iron phosphate filter residue; S400, calcining the second iron phosphate residue to obtain battery-grade iron phosphate.
2. The method according to claim 1, characterized in that In step S100, at least one of the following conditions is met: Condition A: the liquid-to-solid ratio of the waste iron phosphate and the acid solution is 18 ml / g to 22 ml / g; Condition B: the pH value of the acid solution is -2 to 1.5; Condition C: The acid solution is selected from at least one of a hydrochloric acid solution, a sulfuric acid solution or a nitric acid solution.
3. The method according to claim 1, characterized in that In step S200, diluting the waste solution with water includes: Diluting the waste solution with water to a pH value of 0.7 to 2.5; Preferably, the waste solution is diluted with water to a pH value of 0.9 to 1.
5.
4. The method according to claim 1, characterized in that In step S200, The conditions for the high temperature crystallization are: Temperature: 70℃ to 110℃; Time: 3h to 6h.
5. The method according to any one of claims 1 to 4, characterized in that: Step S200 also includes adding an oxidant during the dilution process of the waste solution with water; The oxidant includes hydrogen peroxide; The mass concentration of the hydrogen peroxide is 25wt% to 30wt%; The dosage of the hydrogen peroxide is: 2 ml to 4 ml of the hydrogen peroxide for every 10 g of the waste iron phosphate.
6. The method according to claim 1, characterized in that In step S300, the pH value of the phosphoric acid solution is 0.5-3; The usage of the phosphoric acid solution is: for every 10g of the waste iron phosphate, 200ml to 400ml of the phosphoric acid solution is used.
7. The method according to claim 1 or 6, characterized in that: In step S300, during the cleaning and phosphorus supplementation, the first iron phosphate filter residue is subjected to secondary recrystallization; Preferably, the conditions for cleaning and phosphorus supplementation are: Cleaning temperature: 70℃ to 110℃; Cleaning times: 2 to 3 times; Single cleaning time: 1h to 2h; Total cleaning time: 3h to 6h.
8. The method according to claim 1, characterized in that The waste iron phosphate includes the ferrophosphorus slag remaining after lithium is recovered from the positive electrode waste of waste lithium iron phosphate batteries.
9. The method according to claim 1, characterized in that: The filtrate in step S200 is heated and evaporated to a pH value of -2 to 1.5, and step S100 is repeated to dissolve the waste iron phosphate.
10. Battery-grade iron phosphate obtained by the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of battery-grade iron phosphate
CN110482512A
Recovery method of iron phosphate waste
CN112320780A
Method for preparing iron phosphate from lithium extraction slag of waste lithium iron phosphate positive electrode powder and application
CN112499609A
Method for preparing high-purity iron phosphate from lithium iron phosphate battery waste
CN113415793A
Iron phosphate dihydrate and preparation method thereof, iron phosphate, lithium iron phosphate and lithium ion battery
CN114394581A
Cited By
Method for recovering iron phosphate from black powder acid leaching residues of retired lithium iron phosphate batteries
CN121269653A
Method for regenerating battery-grade iron phosphate from waste lithium iron phosphate lithium extraction slag
CN122102081A