Cesium-doped bismuth vanadate material as well as preparation method and application thereof
By doping cesium ions in bismuth vanadate and preparing cesium doped bismuth vanadate thin films by electrodeposition method, the problem of poor stability of bismuth vanadate photoanode was solved, and its photoelectrochemical performance and water oxidation capacity were significantly improved, thus achieving Excellent performance in the preparation of hydrogen by photoelectro-catalytic decomposition of water.
Patent Information
- Application Number
- CN202411265087.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
AI Technical Summary
Due to the problems of carrier recombination, slow water oxidation kinetics and poor stability, bismuth vanadate photoanode limits its application in photoelectrochemical decomposition of water to prepare hydrogen.
By doping cesium ions into bismuth vanadate, the cesium doped bismuth vanadate film was prepared by electrodeposition method to improve its photoelectrochemical properties and PEC water oxidation properties, including dissolution in potassium iodide, bismuth nitrate pentahydrate and cesium hydroxide monohydrate. After adjusting the pH value, mixing the benzenequinone solution for electrodeposition, calcining and immersion of the alkaline solution to form a cesium-doped bismuth vanadate material.
The photocurrent density and electrochemical activity area are significantly improved, the conductivity and water oxidation reaction capacity are enhanced, so that cesium-doped bismuth vanadate materials show excellent performance in photoelectro-catalyzed decomposition of water to produce hydrogen.
Smart Images

Figure HDA0005036899080000011 
Figure HDA0005036899080000012 
Figure HDA0005036899080000013
Abstract
Description
Technical Field
[0001] The invention belongs to the field of photoelectrochemical (PEC) water decomposition to prepare hydrogen, and specifically relates to a cesium-doped bismuth vanadate material and a preparation method and application thereof. Background Art
[0002] As a clean and renewable energy source, hydrogen is gaining more and more attention. Among the many methods of hydrogen production, the method of producing hydrogen by photoelectrochemical decomposition of water has attracted much attention due to its pollution-free and low energy consumption.
[0003] Bismuth vanadate (BiVO4) has become the preferred photoanode material due to its suitable band gap (about 2.4eV), non-toxic and cheap raw materials, and high photoelectric conversion efficiency. However, the practical application of BiVO4 photoanode is hampered by defects such as serious carrier recombination, slow water oxidation kinetics, and poor stability on the surface of BiVO4. Summary of the invention
[0004] In order to solve the above problems of the prior art, the present invention provides a cesium-doped bismuth vanadate material and a preparation method and application thereof. The cesium-doped bismuth vanadate material has excellent photoelectrochemical properties and PEC water oxidation properties.
[0005] The present invention is achieved through the following technical solutions:
[0006] The present invention provides a cesium-doped bismuth vanadate material, which is Cs-doped BiVO4.
[0007] Preferably, in terms of molar percentage, the doping amount of Cs is 1% to 10% of the molar amount of BiVO4.
[0008] The present invention provides a method for preparing the cesium-doped bismuth vanadate material, comprising the following steps:
[0009] (1) dissolving potassium iodide, bismuth nitrate pentahydrate and cesium hydroxide monohydrate in water, adjusting the pH value to 1 to 3, to obtain solution A; dissolving p-benzoquinone in anhydrous ethanol to obtain solution B;
[0010] (2) mixing solution A and solution B to obtain an electrodeposition precursor solution;
[0011] (3) using an electrodeposition precursor solution to perform electrodeposition to obtain a cesium-doped bismuth oxide iodide film;
[0012] (4) adding solution C dropwise onto the cesium-doped bismuth iodide oxide film, and then calcining; wherein the solution C is a dimethyl sulfoxide solution of acetylacetonate;
[0013] (5) The calcined product is immersed in an alkaline solution to obtain a cesium-doped bismuth vanadate film.
[0014] Preferably, in solution A, the molar ratio of cesium hydroxide monohydrate to bismuth nitrate pentahydrate is (1-10):100.
[0015] Preferably, the molar ratio of bismuth nitrate pentahydrate to potassium iodide in solution A is 1:(8-12); and the molar ratio of p-benzoquinone to bismuth nitrate pentahydrate in the electrodeposition precursor solution is (20-25):4.
[0016] Preferably, the electrodeposition time is 3 to 8 minutes.
[0017] Preferably, the concentration of vanadyl acetylacetonate in solution C is 0.06M to 0.2M.
[0018] Preferably, the calcination temperature is 400-500° C. and the calcination time is 1-3 hours.
[0019] Preferably, the alkaline solution is potassium hydroxide solution.
[0020] The present invention also provides the use of the cesium-doped bismuth vanadate material or the cesium-doped bismuth vanadate film obtained by the preparation method as a photoanode in photoelectrocatalytic water decomposition to produce hydrogen.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention provides a cesium-doped bismuth vanadate material. Compared with bismuth vanadate, the photocurrent density of the cesium-doped bismuth vanadate is significantly improved. This is because Cs replaces the position of V, thereby causing lattice distortion, improving light absorption performance, and generating more carriers.
[0023] The present invention also provides a simple and effective method for doping cesium ions into the bismuth vanadate bulk phase, wherein the ions Cs are doped into an electrodeposition precursor solution and uniformly doped into the bismuth vanadate bulk phase by an electrodeposition method, and the obtained cesium-doped bismuth vanadate photoanode film exhibits excellent PEC water oxidation performance.
[0024] The semicircle radius fitted by the electrochemical impedance diagram of the cesium-doped bismuth vanadate material provided by the present invention is smaller than the fitted circle radius of bismuth vanadate, indicating that doping with Cs can significantly improve the conductivity of the BiVO4 photoanode. -1) tested the photoanode voltammetric curves of cesium-doped bismuth vanadate and bismuth vanadate, and obtained the electrochemically active areas (ECSA) of the two photoanodes. The results showed that the ECSA value of the Cs-BiVO4 photoanode was greatly improved compared with that of the BiVO4 photoanode. And according to the relevant formula, a linear fitting graph of the relationship between the current difference Δj and the scanning rate was made, and its slope was roughly equal to the ECSA value. A significant increase in ECSA is conducive to the occurrence of water oxidation reaction. Therefore, the electrochemical impedance, electrochemical active area and other photoelectrochemical properties of the cesium-doped bismuth vanadate material provided by the present invention are better than those of undoped bismuth vanadate, showing excellent PEC water oxidation performance, and can be used as a photoanode for photoelectrocatalytic water decomposition to produce hydrogen. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 The BiVO4 thin film photoanode in Comparative Example 1 of the present invention and the cesium-doped BiVO4 thin film photoanode in Example 1 were subjected to 100 mW cm-2 electrolysis in 0.5 M Na2SO4 electrolyte. -2 Schematic diagram of the linear sweep voltammetry curve measured under light intensity.
[0027] Figure 2 The BiVO4 thin film photoanode in Comparative Example 1 of the present invention and the cesium-doped BiVO4 thin film photoanode in Example 1 were subjected to 100 mW cm-2 electrolysis in 0.5 M Na2SO4 electrolyte. -2 Electrochemical impedance spectroscopy (EIS) plots measured under light intensity.
[0028] Figure 3 The electrochemical active area ECSA diagram of the BiVO4 thin film photoanode in comparative example 1 of the present invention and the cesium-doped BiVO4 thin film photoanode in embodiment 1 was measured in 0.5M Na2SO4 electrolyte.
[0029] Figure 4 The cesium-doped BiVO4 thin film photoanode of Examples 1 to 4 of the present invention is in a 0.5M Na2SO4 electrolyte at 100mW cm -2 Schematic diagram of the linear sweep voltammetry curve measured under light intensity.
[0030] Figure 5The cesium-doped BiVO4 thin film photoanode electrodeposition of Example 1 of the present invention for 8 min and the cesium-doped BiVO4 thin film photoanode electrodeposition of Example 6 for 5 min in 0.5 M Na2SO4 electrolyte at 100 mW cm -2 Schematic diagram of the linear sweep voltammetry curve measured under light intensity.
[0031] Figure 6 X-ray diffraction (XRD) patterns of the photoanodes of Comparative Example 1 and Example 1 are shown.
[0032] Figure 7 Zhongwei Figure 6 A partial enlarged view of . DETAILED DESCRIPTION
[0033] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0034] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0035] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0036] The method for preparing the cesium-doped bismuth vanadate material of the present invention comprises the following steps:
[0037] (1) dissolving potassium iodide, bismuth nitrate pentahydrate and cesium hydroxide monohydrate in deionized water, and then adding a certain amount of dilute nitric acid to adjust the pH value of the solution to 1-3 to obtain solution A; dissolving p-benzoquinone in anhydrous ethanol to obtain solution B;
[0038] (2) After the two solutions are dissolved, solution A and solution B are mixed evenly and stirred sufficiently to obtain an electrodeposition precursor solution;
[0039] (3) using an electrodeposition precursor solution for electrodeposition, the electrodeposition is carried out in a three-electrode system, with a platinum sheet as a counter electrode, FTO (F-doped SnO2) as a working electrode, and an Ag / AgCl standard electrode as a reference electrode, and the working voltage is set to -0.1 V vs. Ag / AgCl; depositing a layer of iodine bismuth oxide precursor film on the FTO, that is, obtaining a cesium-doped iodine bismuth oxide film;
[0040] (4) dissolving acetylacetonate in dimethyl sulfoxide to obtain solution C;
[0041] (5) adding a C solution dropwise onto the electrodeposited cesium-doped bismuth iodide film, and then transferring the sample to a tube furnace for calcination;
[0042] (6) The calcined product is immersed in an alkaline solution to obtain the target product, cesium-doped bismuth vanadate photoanode film.
[0043] In the above step (1), the molar ratio of cesium hydroxide monohydrate to bismuth nitrate pentahydrate in solution A is (1-10): 100. The molar ratio of bismuth nitrate pentahydrate to potassium iodide is 1: (8-12).
[0044] In the above step (2), in the electrodeposition precursor solution, the molar ratio of p-benzoquinone to bismuth nitrate pentahydrate is (20-25):4.
[0045] The concentration of bismuth nitrate pentahydrate in the solution A is preferably 0.04 M. The concentration of p-benzoquinone in the solution B is preferably 0.23 M.
[0046] In the above step (4), the concentration of vanadyl acetylacetonate in the solution C is 0.06M to 0.2M.
[0047] In the above step (5), the calcination is carried out at 400-500°C for 1-3 hours, and the heating rate of the tube furnace is preferably set to 2°C·min -1 .
[0048] In the above step (6), the alkaline solution is a potassium hydroxide solution, and the vanadium pentoxide remaining on the surface of the film is removed by soaking in the potassium hydroxide solution.
[0049] Comparative Example 1
[0050] Preparation of BiVO4 electrode
[0051] Dissolve 3.3200gKI and 0.9701g Bi(NO3)3·5H2O in 50ml deionized water, then add a certain amount of dilute HNO3 to adjust the pH value of the solution to 1.7, and mark this solution as solution A; weigh 0.4973g p-benzoquinone and dissolve it in 20mL anhydrous ethanol, and after it is completely dissolved, slowly add it to solution A to obtain an electrodeposition precursor solution.
[0052] The electrodeposition was carried out using a three-electrode system, with a platinum sheet as the counter electrode, FTO (F-doped SnO2) as the working electrode, and an Ag / AgCl standard electrode as the reference electrode. The working voltage was set to -0.1 V vs. Ag / AgCl. The BiIO film was deposited using an electrochemical workstation for 8 min. The deposited BiIO film was rinsed with deionized water and anhydrous ethanol, respectively, and then dried for later use.
[0053] Weigh 0.2g of vanadium acetylacetonate and dissolve it in 4mL of dimethyl sulfoxide. Add 100μL of vanadium acetylacetonate solution to each deposited BiIO film, transfer it to a tube furnace for calcination, set the calcination temperature to 450℃, and heat it at a rate of 2℃ / min for 2 hours. After calcination, remove the residual vanadium pentoxide on the surface with 1M sodium hydroxide solution, and rinse it with deionized water and anhydrous ethanol to finally obtain a BiVO4 thin film photoelectrode.
[0054] Example 1
[0055] Dissolve 3.3200gKI, 0.9701g Bi(NO3)3·5H2O, and 0.0034g CsOH·H2O in 50ml deionized water, then add a certain amount of dilute HNO3 to adjust the pH value of the solution to 1.7, and mark this solution as solution A; weigh 0.4973g p-benzoquinone and dissolve it in 20mL anhydrous ethanol, and after it is completely dissolved, slowly add it to solution A to obtain an electrodeposition precursor solution.
[0056] The electrodeposition was carried out using a three-electrode system, with a platinum sheet as the counter electrode, FTO (F-doped SnO2) as the working electrode, and an Ag / AgCl standard electrode as the reference electrode. The working voltage was set to -0.1 V vs. Ag / AgCl. The cesium-doped BiIO film was deposited using an electrochemical workstation for 8 min. The deposited cesium-doped BiIO film was rinsed with deionized water and anhydrous ethanol, respectively, and then dried for later use.
[0057] Weigh 0.2g of vanadium acetylacetonate and dissolve it in 4mL of dimethyl sulfoxide. Add 100μL of vanadium acetylacetonate solution to each cesium-doped BiIO film after deposition, transfer it to a tube furnace for calcination, set the calcination temperature to 450℃, and heat it at a rate of 2℃ / min for 2 hours. After calcination, remove the residual vanadium pentoxide on the surface with 1M sodium hydroxide solution, and rinse it with deionized water and anhydrous ethanol to finally obtain a cesium-doped BiVO4 thin film photoelectrode.
[0058] Example 2
[0059] Dissolve 3.3200gKI, 0.9701g Bi(NO3)3·5H2O, and 0.01g CsOH·H2O in 50ml deionized water, then add a certain amount of dilute HNO3 to adjust the pH value of the solution to 1.7, and mark this solution as solution A; weigh 0.4973g p-benzoquinone and dissolve it in 20mL anhydrous ethanol, and after it is completely dissolved, slowly add it to solution A to obtain an electrodeposition precursor solution.
[0060] The electrodeposition was carried out using a three-electrode system, with a platinum sheet as the counter electrode, FTO (F-doped SnO2) as the working electrode, and an Ag / AgCl standard electrode as the reference electrode. The working voltage was set to -0.1 V vs. Ag / AgCl. The cesium-doped BiIO film was deposited using an electrochemical workstation for 8 min. The deposited cesium-doped BiIO film was rinsed with deionized water and anhydrous ethanol, respectively, and then dried for later use.
[0061] Weigh 0.2g of vanadium acetylacetonate and dissolve it in 4mL of dimethyl sulfoxide. Add 100μL of vanadium acetylacetonate solution to each cesium-doped BiIO film after deposition, transfer it to a tube furnace for calcination, set the calcination temperature to 450℃, and heat it at a rate of 2℃ / min for 2 hours. After calcination, remove the residual vanadium pentoxide on the surface with 1M sodium hydroxide solution, and rinse it with deionized water and anhydrous ethanol to finally obtain a cesium-doped BiVO4 thin film photoelectrode.
[0062] Example 3
[0063] Dissolve 3.3200gKI, 0.9701g Bi(NO3)3·5H2O, and 0.0168g CsOH·H2O in 50ml deionized water, then add a certain amount of dilute HNO3 to adjust the pH value of the solution to 1.7, and mark this solution as solution A; weigh 0.4973g p-benzoquinone and dissolve it in 20mL anhydrous ethanol, and after it is completely dissolved, slowly add it to solution A to obtain an electrodeposition precursor solution.
[0064] The electrodeposition was carried out using a three-electrode system, with a platinum sheet as the counter electrode, FTO (F-doped SnO2) as the working electrode, and an Ag / AgCl standard electrode as the reference electrode. The working voltage was set to -0.1 V vs. Ag / AgCl. The cesium-doped BiIO film was deposited using an electrochemical workstation for 8 min. The deposited cesium-doped BiIO film was rinsed with deionized water and anhydrous ethanol, respectively, and then dried for later use.
[0065] Weigh 0.2g of vanadium acetylacetonate and dissolve it in 4mL of dimethyl sulfoxide. Add 100μL of vanadium acetylacetonate solution to each cesium-doped BiIO film after deposition, transfer it to a tube furnace for calcination, set the calcination temperature to 450℃, and heat it at a rate of 2℃ / min for 2 hours. After calcination, remove the residual vanadium pentoxide on the surface with 1M sodium hydroxide solution, and rinse it with deionized water and anhydrous ethanol to finally obtain a cesium-doped BiVO4 thin film photoelectrode.
[0066] Example 4
[0067] Dissolve 3.3200gKI, 0.9701gBi(NO3)3·5H2O, and 0.0336gCsOH·H2O in 50ml of deionized water, then add a certain amount of dilute HNO3 to adjust the pH value of the solution to 1.7, and mark this solution as solution A; weigh 0.4973g of p-benzoquinone and dissolve it in 20mL of anhydrous ethanol, and after it is completely dissolved, slowly add it to solution A to obtain an electrodeposition precursor solution.
[0068] The electrodeposition was carried out using a three-electrode system, with a platinum sheet as the counter electrode, FTO (F-doped SnO2) as the working electrode, and an Ag / AgCl standard electrode as the reference electrode. The working voltage was set to -0.1 V vs. Ag / AgCl. The cesium-doped BiIO film was deposited using an electrochemical workstation for 8 min. The deposited cesium-doped BiIO film was rinsed with deionized water and anhydrous ethanol, respectively, and then dried for later use.
[0069] Weigh 0.2g of vanadium acetylacetonate and dissolve it in 4mL of dimethyl sulfoxide. Add 100μL of vanadium acetylacetonate solution to each cesium-doped BiIO film after deposition, transfer it to a tube furnace for calcination, set the calcination temperature to 450℃, and heat it at a rate of 2℃ / min for 2 hours. After calcination, remove the residual vanadium pentoxide on the surface with 1M sodium hydroxide solution, and rinse it with deionized water and anhydrous ethanol to finally obtain a cesium-doped BiVO4 thin film photoelectrode.
[0070] Example 5
[0071] Dissolve 3.3200gKI, 0.9701gBi(NO3)3·5H2O, and 0.0034gCsOH·H2O in 50ml of deionized water, then add a certain amount of dilute HNO3 to adjust the pH value of the solution to 1.7, and mark this solution as solution A; weigh 0.4973g of p-benzoquinone and dissolve it in 20mL of anhydrous ethanol, and after it is completely dissolved, slowly add it to solution A to obtain an electrodeposition precursor solution.
[0072] The electrodeposition was carried out using a three-electrode system, with a platinum sheet as the counter electrode, FTO (F-doped SnO2) as the working electrode, and an Ag / AgCl standard electrode as the reference electrode. The working voltage was set to -0.1 V vs. Ag / AgCl. The cesium-doped BiIO film was deposited using an electrochemical workstation for 8 min. The deposited cesium-doped BiIO film was rinsed with deionized water and anhydrous ethanol, respectively, and then dried for later use.
[0073] Weigh 0.03g of vanadium acetylacetonate and dissolve it in 2mL of dimethyl sulfoxide. Add 100μL of vanadium acetylacetonate solution to each cesium-doped BiIO film after deposition, transfer it to a tube furnace for calcination, set the calcination temperature to 450℃, and heat it at a rate of 2℃ / min for 2 hours. After calcination, remove the residual vanadium pentoxide on the surface with 1M sodium hydroxide solution, and rinse it with deionized water and anhydrous ethanol to finally obtain a cesium-doped BiVO4 thin film photoelectrode.
[0074] Example 6
[0075] Dissolve 3.3200gKI, 0.9701gBi(NO3)3·5H2O, and 0.0034gCsOH·H2O in 50ml of deionized water, then add a certain amount of dilute HNO3 to adjust the pH value of the solution to 1.7, and mark this solution as solution A; weigh 0.4973g of p-benzoquinone and dissolve it in 20mL of anhydrous ethanol, and after it is completely dissolved, slowly add it to solution A to obtain an electrodeposition precursor solution.
[0076] The electrodeposition was carried out using a three-electrode system, with a platinum sheet as the counter electrode, FTO (F-doped SnO2) as the working electrode, and an Ag / AgCl standard electrode as the reference electrode. The working voltage was set to -0.1 V vs. Ag / AgCl. The cesium-doped BiIO film was deposited using an electrochemical workstation for 5 min. The deposited cesium-doped BiIO film was rinsed with deionized water and anhydrous ethanol, respectively, and then dried for later use.
[0077] Weigh 0.2g of vanadium acetylacetonate and dissolve it in 4mL of dimethyl sulfoxide. Add 100μL of vanadium acetylacetonate solution to each cesium-doped BiIO film after deposition, transfer it to a tube furnace for calcination, set the calcination temperature to 450℃, and heat it at a rate of 2℃ / min for 2 hours. After calcination, remove the residual vanadium pentoxide on the surface with 1M sodium hydroxide solution, and rinse it with deionized water and anhydrous ethanol to finally obtain a cesium-doped BiVO4 thin film photoelectrode.
[0078] The electrodes obtained in Examples 1 to 6 and Comparative Example 1 were subjected to photoelectrochemical tests. The electrochemical test used a three-electrode system, with the photoanode as the working electrode, the platinum sheet as the counter electrode, and the Ag / AgCl standard electrode as the reference electrode. 0.5M Na2SO4 was used as the electrolyte solution, and the light source was a 300W xenon headlamp equipped with a 1.5AG filter, with the light intensity set to 100mWcm -2 .
[0079] Figure 1 Schematic diagram of linear sweep voltammetry curves of the BiVO4 thin film photoanode in Comparative Example 1 and the 1% Cs-doped BiVO4 thin film photoanode in Example 1. Figure 1 It can be seen that the photocurrent density generated by the BiVO4 thin film photoanode and the cesium-doped BiVO4 thin film photoanode at 1.23 V vs. RHE is 0.80 mA cm 2 and 1.80 mA cm 2 That is, when the doping amount is 1% Cs, the photocurrent of cesium-doped bismuth vanadate is 2.25 times that of bismuth vanadate without cesium doping, indicating that cesium doping improves the electrochemical properties of bismuth vanadate.
[0080] Figure 2 The electrochemical impedance diagram of the BiVO4 thin film photoanode in comparative example 1 and the 1% Cs-doped BiVO4 thin film photoanode in example 1 is shown in FIG. Figure 2 It can be seen that the semicircle radius of the electrochemical impedance diagram of the cesium-doped BiVO4 thin film photoanode is smaller than that of the electrochemical impedance diagram of the BiVO4 thin film photoanode, indicating that 1% Cs doping can improve the conductivity of the BiVO4 thin film photoanode and reduce the electrochemical impedance.
[0081] Figure 3 The electrochemical active area ECSA diagram of the BiVO4 thin film photoanode in comparative example 1 and the 1% Cs-doped BiVO4 thin film photoanode in example 1 is shown in FIG. Figure 3 It can be seen that doping modification significantly increases the ECSA value of bismuth vanadate, and a larger ECSA value is more conducive to the water oxidation reaction.
[0082] Figure 4The linear sweep voltammetric curves of BiVO4 doped with different Cs contents in Examples 1-4 are shown in Figure 1. The present invention synthesized BiVO4 photoanode films doped with cesium with contents of 1%, 3%, 5%, and 10%. Figure 4 It can be seen that at 1.23V vs. RHE, the photocurrent density of 1%, 3%, 5%, and 10% cesium-doped BiVO4 films is 1.80mAcm -2 、1.56mAcm -2 , 1.45mAcm -2 , 1.30mAcm -2 , it can be seen that when the doping amount is 1%, the photocurrent density of the photoanode is the best, which is significantly improved compared with other contents. However, the photocurrent density of all doping amounts is greater than that of the undoped bismuth vanadate photoanode film.
[0083] Figure 5 The linear sweep voltammetric curves of 1% Cs-doped BiVO4 electrochemically deposited for 8 min and 5 min in Example 1 and Example 6, respectively. Figure 5 It can be seen that the photocurrent density at 8 min and 5 min of electrodeposition is 1.80 mA cm -2 、0.98mAcm -2 .
[0084] Figure 6 The X-ray diffraction (XRD) patterns of the BiVO4 thin film photoanode in Comparative Example 1 and the 1% Cs-doped BiVO4 thin film photoanode in Example 1 are shown. All diffraction peaks in the figure correspond to the standard card of monoclinic BiVO4 (JCPDS PDF#14-0688) and the standard card of SnO2 (PDF#46-1088). Figure 7 The local magnified image in shows that Cs doping causes a significant change in the relative intensity of the diffraction peaks corresponding to the BiVO4 (-121) and (040) crystal planes. This indicates that Cs doping causes BiVO4 lattice distortion, exposing more (040) crystal planes in BiVO4, thereby improving the carrier separation ability of BiVO4, indicating that Cs forms doping.
Claims
1. A cesium-doped bismuth vanadate material, characterized in that: It is Cs-doped BiVO4.
2. The cesium-doped bismuth vanadate material according to claim 1, characterized in that: In terms of molar percentage, the doping amount of Cs is 1% to 10% of the molar amount of BiVO4.
3. The method for preparing the cesium-doped bismuth vanadate material according to claim 1 or 2, characterized in that: The following steps are involved: (1) dissolving potassium iodide, bismuth nitrate pentahydrate and cesium hydroxide monohydrate in water, adjusting the pH value to 1 to 3, to obtain solution A; dissolving p-benzoquinone in anhydrous ethanol to obtain solution B; (2) mixing solution A and solution B to obtain an electrodeposition precursor solution; (3) using an electrodeposition precursor solution to perform electrodeposition to obtain a cesium-doped bismuth oxide iodide film; (4) adding solution C dropwise onto the cesium-doped bismuth iodide oxide film, and then calcining; wherein the solution C is a dimethyl sulfoxide solution of acetylacetonate; (5) The calcined product is immersed in an alkaline solution to obtain a cesium-doped bismuth vanadate film.
4. The method for preparing the cesium-doped bismuth vanadate material according to claim 3, characterized in that: In solution A, the molar ratio of cesium hydroxide monohydrate to bismuth nitrate pentahydrate is (1-10):
100.
5. The method for preparing the cesium-doped bismuth vanadate material according to claim 3, characterized in that: The molar ratio of bismuth nitrate pentahydrate to potassium iodide in solution A is 1:(8-12); and the molar ratio of p-benzoquinone to bismuth nitrate pentahydrate in the electrodeposition precursor solution is (20-25):
4.
6. The method for preparing the cesium-doped bismuth vanadate material according to claim 3, characterized in that: The electrodeposition time is 3 to 8 minutes.
7. The method for preparing the cesium-doped bismuth vanadate material according to claim 3, characterized in that: The concentration of vanadyl acetylacetonate in solution C is 0.06M to 0.2M.
8. The method for preparing the cesium-doped bismuth vanadate material according to claim 3, characterized in that: The calcination temperature is 400-500° C. and the calcination time is 1-3 hours.
9. The method for preparing the cesium-doped bismuth vanadate material according to claim 3, characterized in that: The alkaline solution is potassium hydroxide solution.