Tungsten trioxide semiconductor nanowire material and preparation method thereof

The preparation of tungsten trioxide nanowires using a hydrothermal synthesis method with cationic surfactants and inorganic small molecules solves the problem of complicated synthesis steps in existing technologies, achieves controllable and uniform nanowire size, and improves the production efficiency and performance of the material.

CN119038607APending Publication Date: 2024-11-29ZHEJIANG LANTI SEMICON TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411274494.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In existing technologies, the synthesis steps of tungsten trioxide semiconductor nanowire materials are complex and difficult to mass-produce.

Method used

A hydrothermal synthesis method was adopted, using cationic surfactants as structure-directing agents and inorganic small molecules as metal oxide precursors. By controlling the hydrothermal temperature and time, the preparation process was simplified, and the size of tungsten trioxide nanowires could be precisely controlled.

Benefits of technology

Tungsten trioxide semiconductor nanowires with controllable and uniform size were successfully synthesized, simplifying the preparation process, reducing costs, and improving the yield and performance stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038607A_ABST
    Figure CN119038607A_ABST
Patent Text Reader

Abstract

The invention provides a tungsten trioxide semiconductor nanowire material and a preparation method thereof.The preparation method of the tungsten trioxide semiconductor nanowire material comprises the following steps that a cationic surface active agent is added into an organic solvent, and an organic solution containing the cationic surface active agent is prepared; tungsten chloride is added into the organic solution containing the cationic surface active agent, and a reaction solution is prepared; heating the reaction solution for hydrothermal reaction; and centrifuging, washing and drying in vacuum. According to the method, the synthesis efficiency of the tungsten trioxide nanowire and the size uniformity of the nanowire are effectively improved, the optical, photoelectric and electrical properties of a tungsten trioxide semiconductor nanowire material are improved, and the method has wide application prospects in the fields of heterogeneous catalysis, gas sensing and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nano materials and preparation, and specifically relates to a tungsten trioxide semiconductor nanowire material and a preparation method. Background Art

[0002] One-dimensional nanomaterials are a new type of nanomaterials with high specific surface area, abundant reactive sites and fast electron transfer characteristics. They can effectively promote the adsorption, desorption and transfer of guest molecules. They have important applications in catalytic reactions, energy conversion and storage, and can be used to prepare gas sensors. Resistive sensors based on semiconductor metal oxides are inexpensive, simple in structure, sensitive and fast in response, and easy to mass produce. Therefore, they have become the most important type of sensor in gas sensors and a research hotspot. The preparation of low-dimensional metal oxides can make full use of the rich defects and sensitization properties of the crystal planes unique to metal oxides, increase the adsorbed oxygen concentration and effectively reduce the activation energy of surface reactions, thereby further improving the performance of gas sensors.

[0003] In the prior art, the synthesis steps of tungsten trioxide semiconductor nanowire materials are complicated, often requiring large equipment and manual operation, and are difficult to produce on a large scale. Summary of the invention

[0004] In view of the above-mentioned technical defects in the prior art, the technical problem to be solved by the present invention is to provide a tungsten trioxide semiconductor nanowire material and a preparation method. Through the hydrothermal synthesis method, cationic surfactants are used as structure directing agents, and inorganic small molecules are used as metal oxide precursors. After the hydrothermal reaction, the hydrothermal temperature and time are simply adjusted to achieve precise control of the size of the tungsten trioxide nanowires.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] The present invention provides a method for preparing a tungsten trioxide semiconductor nanowire material, comprising the following steps:

[0007] Step A: adding a cationic surfactant into an organic solvent to prepare an organic solution containing the cationic surfactant;

[0008] Step B: adding tungsten chloride to the organic solution containing the cationic surfactant to prepare a reaction solution;

[0009] Step C: heating the reaction solution to perform a hydrothermal reaction;

[0010] Step D: centrifuging, washing, and vacuum drying to obtain the tungsten trioxide semiconductor nanowire material.

[0011] Preferably, the cationic surfactant is one or more of cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, dodecyltrimethylammonium bromide, octadecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide and dodecyltrimethylammonium bromide.

[0012] Preferably, the organic solvent is one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol.

[0013] Preferably, the mass ratio of the cationic surfactant to the organic solvent is 1:(0.2-1), and more preferably 1:(0.3-0.6).

[0014] Preferably, the mass ratio of the tungsten chloride to the organic solvent is 1:(1-6), and more preferably 1:(2-4).

[0015] Preferably, the hydrothermal reaction conditions are 160-220° C. for 12-24 h.

[0016] Further preferably, a method for preparing a tungsten trioxide semiconductor nanowire material comprises the following steps:

[0017] Step A, adding a cationic surfactant to an organic solvent and mixing them evenly, stirring at room temperature for 10-20 minutes to obtain an organic solution containing a cationic surfactant;

[0018] Step B, adding tungsten chloride to the organic solution containing the cationic surfactant, stirring for 10-20 minutes until it is completely dissolved, to obtain a reaction solution;

[0019] Step C, transferring the reaction solution into a polytetrafluoroethylene bottle and sealing it with a cover; then placing the polytetrafluoroethylene bottle containing the reaction solution into a hydrothermal kettle and tightening it with a cover; placing it in an oven, adjusting the oven temperature between 160-220° C., and performing a hydrothermal reaction for 12-24 hours;

[0020] Step D, centrifuging the product obtained by the hydrothermal reaction in step C, washing it with ethanol, and then vacuum drying it at 35-55° C. to obtain a tungsten trioxide semiconductor nanowire material.

[0021] The present invention also provides a tungsten trioxide semiconductor nanowire material, which is prepared by the above method. Preferably, the width of the tungsten trioxide semiconductor nanowire material is 20-50nm; the length is greater than 0.5μm, preferably greater than 5μm, and more preferably 5-20μm.

[0022] The present invention has the following beneficial effects compared with the prior art:

[0023] First, the present invention successfully synthesized size-controllable and uniform tungsten trioxide semiconductor nanowire materials by precisely controlling the amount of cationic surfactant and the conditions of the hydrothermal reaction. Thanks to this process, the prepared nanowire materials have high adjustability and stability in both width and length.

[0024] Secondly, due to the adsorption and guiding effect of the cationic surfactant on the surface of the crystal grains, the morphology of the nanowires can be effectively controlled, ensuring the high purity and structural integrity of the material. In addition, the method of the present invention simplifies the traditional preparation process, reduces the reaction complexity and cost, and improves the yield of the material.

[0025] Finally, the prepared tungsten trioxide semiconductor nanowire material showed excellent performance stability in application, was suitable for a variety of nanotechnology fields, and showed broad industrial application potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0027] Figure 1 This is a scanning electron microscope image of the tungsten trioxide nanowires provided in Example 1 of the present invention;

[0028] Figure 2 This is a scanning electron microscope image of tungsten trioxide nanowires provided in Example 2 of the present invention;

[0029] Figure 3 This is a scanning electron microscope image of tungsten trioxide nanowires provided in Example 3 of the present invention;

[0030] Figure 4 A transmission electron microscope image of tungsten trioxide nanowires provided in Example 4 of the present invention;

[0031] Figure 5 A transmission electron microscope image of tungsten trioxide nanowires provided in Example 5 of the present invention;

[0032] Figure 6 This is a scanning electron microscope image of tungsten trioxide nanowires provided in Example 6 of the present invention;

[0033] Figure 7 The concentration gradient response curve and concentration-response value curve of the tungsten trioxide nanowires provided in Example 4 of the present invention to ozone gas;

[0034] Figure 8The concentration gradient response curve and concentration-response value curve of tungsten trioxide nanowires to ozone gas provided in known literature;

[0035] Fig. 9 This is a scanning electron microscope image of tungsten trioxide nanowires provided in comparative example 2 of the present invention. DETAILED DESCRIPTION

[0036] Below, by referring to exemplary embodiments, technical problems, technical solutions and advantages of the present invention are explained in detail. The exemplary embodiments described below are only used to explain the present invention and cannot be interpreted as limiting the present invention. It can be understood by those skilled in the art that, unless otherwise defined, all terms (including technical terms and scientific terms) used herein have the same meaning as the general understanding of those of ordinary skill in the field to which the present invention belongs. It should also be understood that those terms such as those defined in general dictionaries should be understood to have a meaning consistent with the meaning in the context of the prior art, and unless defined here, will not be interpreted with an idealized or overly formal meaning.

[0037] A method for preparing a tungsten trioxide semiconductor nanowire material comprises the following steps:

[0038] Step A, adding a cationic surfactant to an organic solvent and mixing them uniformly, stirring at room temperature for 10-20 minutes, to obtain an organic solution containing the cationic surfactant; the mass ratio of the cationic surfactant to the organic solvent is 1:(0.2-1); the cationic surfactant is one or more of hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, dodecyltrimethylammonium bromide, octadecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide and dodecyltrimethylammonium bromide; the organic solvent is one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol; the main function of this step is to ensure that the cationic surfactant is uniformly distributed in the solvent, so as to provide a stable reaction environment in the subsequent chemical reaction.

[0039] Step B, adding tungsten chloride to the organic solution containing the cationic surfactant, stirring for 10-20 minutes until completely dissolved, to prepare a reaction solution; the mass ratio of the tungsten chloride to the organic solvent in the organic solution containing the cationic surfactant is 1:(1-6); adding tungsten chloride to the organic solution containing the cationic surfactant prepared in step A, stirring until completely dissolved, to prepare a reaction solution. The key to this step is to ensure that the tungsten chloride is in full contact with the surfactant in the solution to form a uniform precursor solution. The complete dissolution of tungsten chloride is the basis for the synthesis of tungsten trioxide nanowires, and affects the growth and morphology of tungsten trioxide nanowires in the subsequent hydrothermal reaction.

[0040] Step C, transfer the reaction solution to a polytetrafluoroethylene bottle and seal it with a cover; then place the polytetrafluoroethylene bottle containing the reaction solution in a hydrothermal kettle and tighten it with a cover; place it in an oven, adjust the oven temperature between 160-220°C, and perform a hydrothermal reaction for 12-24 hours; the purpose of this step is to generate tungsten trioxide nanowires through a hydrothermal reaction. Specifically, the prepared reaction solution is transferred to a polytetrafluoroethylene bottle and sealed with a cover to ensure the airtightness of the reaction system. Subsequently, the sealed polytetrafluoroethylene bottle is placed in a hydrothermal kettle and the lid is tightened to ensure that there is no gas or liquid leakage during the hydrothermal reaction, thereby maintaining a high temperature and high pressure environment inside the system. The hydrothermal kettle is placed in an oven and the temperature is adjusted to 160-220°C, so that the reaction is carried out at high temperature for 12-24 hours. This hydrothermal reaction process is the key to the growth of tungsten trioxide nanowires. The adjustment of reaction temperature and time can directly affect the length and width of the nanowires. By precisely controlling these parameters, the size and morphology of the nanowires can be easily adjusted so that the final product has a uniform size distribution.

[0041] Step D, centrifuge the product obtained by the hydrothermal reaction in step C, wash it with ethanol, and then vacuum dry it at 35-55°C to obtain a tungsten trioxide semiconductor nanowire material. In this step, the product generated after the hydrothermal reaction in step C is separated from the solid by centrifugation to remove the reaction residue. Subsequently, the separated product is washed with ethanol to remove impurities remaining on the surface. Then, the washed product is placed in a vacuum environment at 35-55°C for drying, and finally a pure tungsten trioxide semiconductor nanowire material is obtained. Through this method, the present invention can effectively control the size and morphology of tungsten trioxide nanowires. By adjusting the amount of cationic surfactant and the temperature and time of the hydrothermal reaction, a nanowire material with a width of 20-50nm and a length of at least 5μm is synthesized. The obtained tungsten trioxide semiconductor nanowire material has the characteristics of controllable and uniform size, which significantly improves the uniformity and practicality of the material, so that it exhibits higher performance stability in application.

[0042] The present invention provides a new method for preparing tungsten trioxide semiconductor nanowire materials, using a cationic surfactant with a small molecular weight as a template to guide the formation of tungsten trioxide nanowires during the hydrothermal reaction process. Specifically, the cationic surfactant is first dissolved in an organic solvent, and a stable solution environment is formed by precisely controlling the stirring time and temperature. Subsequently, tungsten chloride is added to the solution to ensure that it is fully dissolved to generate a uniform reaction solution. In the hydrothermal reaction stage, tungsten chloride is gradually hydrolyzed to generate tungsten trioxide grains. Since these initially generated grains have more lattice defects, the cationic surfactant coordinates with these grains and adsorbs on the surface of the grains, thereby guiding these grains to aggregate and crystallize in a specific direction, and finally forming a nanowire structure. By precisely controlling the temperature and time of the hydrothermal reaction, the size of the nanowire can be effectively adjusted. Finally, centrifugal separation and ethanol washing are used to remove the reaction residues, and then vacuum drying is performed to obtain a tungsten trioxide semiconductor nanowire material with uniform size and stable performance. The preparation method of the present invention is simple and efficient, and the prepared nanowire material has excellent size control and uniformity, showing good practicality and broad application prospects.

[0043] Embodiment 1:

[0044] A method for preparing a tungsten trioxide semiconductor nanowire material comprises the following steps:

[0045] Step A, dissolving 100 mg of hexadecyltrimethylammonium bromide in 60 ml of anhydrous ethanol, stirring at room temperature for 15 min until completely dissolved, to obtain an organic solution containing a cationic surfactant;

[0046] Step B, adding 100 mg of solid tungsten chloride to the above solution containing the cationic surfactant, stirring for 10 minutes to obtain a light yellow transparent solution (i.e., reaction solution);

[0047] Step C, transfer the above light yellow transparent solution into a polytetrafluoroethylene bottle and seal it with a cover; put the polytetrafluoroethylene bottle containing the reaction solution into a hydrothermal kettle and tighten it with a cover; place the hydrothermal kettle containing the reaction solution in an oven, adjust the oven temperature at 160° C., and react for 18 hours;

[0048] Step D, centrifuging the product obtained by the hydrothermal reaction to obtain a powder product, washing the powder product with ethanol, and then vacuum drying it at 40° C. for 24 hours to obtain a tungsten trioxide semiconductor nanowire material.

[0049] See also Figure 1 The obtained tungsten trioxide semiconductor nanowire material has a uniform linear morphology, a nanowire length of 0.5-1 μm, and a width of 50 nm.

[0050] Embodiment 2:

[0051] A method for preparing a tungsten trioxide semiconductor nanowire material comprises the following steps:

[0052] Step A, dissolving 95 mg of dodecyltrimethylammonium bromide in 50 ml of anhydrous isopropanol, stirring at room temperature for 15 min until completely dissolved, to obtain an organic solution of a cationic surfactant;

[0053] Step B, adding 120 mg of solid tungsten chloride to a solution containing a cationic surfactant, stirring for 10 minutes to obtain a light yellow transparent solution (i.e., a reaction solution);

[0054] Step C, transferring the obtained light yellow transparent solution into a polytetrafluoroethylene bottle and sealing it with a cover; placing the polytetrafluoroethylene bottle containing the reaction solution into a hydrothermal kettle and tightening it with a cover; placing the hydrothermal kettle containing the reaction solution in an oven, adjusting the oven temperature at 180° C., and reacting for 20 hours;

[0055] Step D, centrifuging the product obtained by the hydrothermal reaction to obtain a powder product, washing the powder product with ethanol, and then vacuum drying it at 40° C. for 24 hours to obtain a tungsten trioxide semiconductor nanowire material.

[0056] See also Figure 2 The obtained tungsten trioxide semiconductor nanowire material has a uniform linear morphology, the nanowire length is more than 5 μm, and the width is 40 nm.

[0057] Embodiment 3:

[0058] A method for preparing a tungsten trioxide semiconductor nanowire material comprises the following steps:

[0059] Step A, dissolving 150 mg of octadecyltrimethylammonium bromide in 50 ml of anhydrous n-propanol, stirring at room temperature for 15 min until completely dissolved, to obtain an organic solution of a cationic surfactant;

[0060] Step B, adding 150 mg of solid tungsten chloride to a solution containing a cationic surfactant, stirring for 10 minutes to obtain a light yellow transparent solution (i.e., a reaction solution);

[0061] Step C, transferring the obtained light yellow transparent solution into a polytetrafluoroethylene bottle and sealing it with a cover; placing the polytetrafluoroethylene bottle containing the reaction solution into a hydrothermal kettle and tightening it with a cover; placing the hydrothermal kettle containing the reaction solution in an oven, adjusting the oven temperature at 180° C., and reacting for 24 hours;

[0062] Step D, centrifuging the product obtained by the hydrothermal reaction to obtain a powder product, washing the powder product with ethanol, and then vacuum drying it at 40° C. for 24 hours to obtain a tungsten trioxide semiconductor nanowire material.

[0063] See also Figure 3 The obtained tungsten trioxide semiconductor nanowire material has a uniform linear morphology, the nanowire length is more than 10 μm, and the width is 30 nm.

[0064] Embodiment 4:

[0065] A method for preparing a tungsten trioxide semiconductor nanowire material comprises the following steps:

[0066] Step A, dissolving 150 mg of dodecyltrimethylammonium bromide in 50 ml of anhydrous n-propanol, stirring at room temperature for 15 min until completely dissolved, to obtain an organic solution of a cationic surfactant;

[0067] Step B, adding 150 mg of solid tungsten chloride to a solution containing a cationic surfactant, stirring for 10 minutes to obtain a light yellow transparent solution (i.e., a reaction solution);

[0068] Step C, transferring the obtained light yellow transparent solution into a polytetrafluoroethylene bottle and sealing it with a cover; placing the polytetrafluoroethylene bottle containing the reaction solution into a hydrothermal kettle and tightening it with a cover; placing the hydrothermal kettle containing the reaction solution in an oven, adjusting the oven temperature at 180° C., and reacting for 24 hours;

[0069] Step D, centrifuging the product obtained by the hydrothermal reaction to obtain a powder product, washing the powder product with ethanol, and then vacuum drying it at 40° C. for 24 hours to obtain a tungsten trioxide semiconductor nanowire material.

[0070] See also Figure 4 The obtained tungsten trioxide semiconductor nanowire material has a uniform linear morphology, a nanowire length of more than 5 μm, and a width of 20 nm.

[0071] Embodiment 5:

[0072] A method for preparing a tungsten trioxide semiconductor nanowire material comprises the following steps:

[0073] Step A, dissolving 200 mg of hexadecyltrimethylammonium bromide in 50 ml of anhydrous n-butanol, stirring at room temperature for 15 min until completely dissolved, to obtain an organic solution of a cationic surfactant;

[0074] Step B, adding 250 mg of solid tungsten chloride to a solution containing a cationic surfactant, stirring for 10 minutes to obtain a light yellow transparent solution (i.e., a reaction solution);

[0075] Step C, transfer the obtained light yellow transparent solution into a polytetrafluoroethylene bottle and seal it with a cover; put the polytetrafluoroethylene bottle containing the reaction solution into a hydrothermal kettle and tighten it with a cover; place the hydrothermal kettle containing the reaction solution in an oven, adjust the oven temperature at 175° C., and react for 22 hours;

[0076] Step D, centrifuging the product obtained by the hydrothermal reaction to obtain a powder product, washing the powder product with ethanol, and then vacuum drying it at 40° C. for 24 hours to obtain a tungsten trioxide semiconductor nanowire material.

[0077] See also Figure 5 The obtained tungsten trioxide semiconductor nanowire material has a uniform linear morphology, a nanowire length of more than 5 μm, and a width of 30 nm.

[0078] Embodiment 6:

[0079] A method for preparing a tungsten trioxide semiconductor nanowire material comprises the following steps:

[0080] Step A, dissolving 75 mg of decanyltrimethylammonium bromide and 75 mg of octadecyltrimethylammonium bromide in 50 ml of anhydrous n-propanol, stirring at room temperature for 15 min until completely dissolved, to obtain an organic solution of a cationic surfactant;

[0081] Step B, adding 150 mg of solid tungsten chloride to a solution containing a cationic surfactant, stirring for 10 minutes to obtain a light yellow transparent solution (i.e., a reaction solution);

[0082] Step C, transferring the obtained light yellow transparent solution into a polytetrafluoroethylene bottle and sealing it with a cover; placing the polytetrafluoroethylene bottle containing the reaction solution into a hydrothermal kettle and tightening it with a cover; placing the hydrothermal kettle containing the reaction solution in an oven, adjusting the oven temperature at 180° C., and reacting for 24 hours;

[0083] Step D, centrifuging the product obtained by the hydrothermal reaction to obtain a powder product, washing the powder product with ethanol, and then vacuum drying it at 40° C. for 24 hours to obtain a tungsten trioxide semiconductor nanowire material.

[0084] See also Figure 6 The obtained tungsten trioxide semiconductor nanowire material has a uniform linear morphology, the nanowire length is more than 5 μm, and the width is 25 nm.

[0085] Application Example 1:

[0086] This application example provides the test results of the tungsten trioxide semiconductor nanowire material of the present invention for detecting ozone concentration at 125°C.

[0087] The specific test method includes the following steps:

[0088] Step A, dispersing the tungsten trioxide semiconductor nanowire material prepared in Example 3, 4 or 6 in anhydrous n-butanol and grinding to a slurry state, wherein the mass ratio of the tungsten trioxide semiconductor nanowire material to the anhydrous n-butanol is 5:1;

[0089] Step B: evenly apply 1 μL of slurry material on the substrate of the MEMS test element (1×1 mm 2 ) and let dry;

[0090] Step C, heating the test element coated with tungsten trioxide semiconductor nanowire material to 250° C. and aging for 48 hours;

[0091] Step D, placing the test element coated with tungsten trioxide semiconductor nanowire material in the NanoRay MA1.0 gas sensing test system, adjusting the temperature to 125°C, injecting 0.1-2.5ppm ozone successively and recording the response value;

[0092] The material of Example 3 has a response value of 7.6 to 2.5 ppm of ozone, and in this concentration range, the response value and the concentration have a good linear correlation (correlation coefficient is 0.98).

[0093] The material of Example 4 has a response value of 9.0 to 2.5 ppm of ozone, and in this concentration range, the response value and the concentration have a good linear correlation (correlation coefficient is 0.99).

[0094] The material of Example 6 has a response value of 10.2 to 2.5 ppm of ozone, and in this concentration range, the response value and the concentration have a good linear correlation (correlation coefficient is 0.99).

[0095] The following table shows the response values ​​and correlation coefficients of different embodiments of the present invention to a specific concentration of ozone.

[0096] serial number Width(nm) Response value (2.5ppm ozone) Correlation coefficient Example 3 30 7.6 0.98 Example 4 20 9.0 0.99 Example 6 25 10.2 0.99

[0097] Example 6 uses a compound of decanyl trimethyl ammonium bromide (DTAB) and octadecyl trimethyl ammonium bromide (OTAB). From the perspective of chemical structure, this compound significantly improves the preparation effect of tungsten trioxide nanowires. The mechanism lies in the synergistic effect caused by the difference in chain length between the two. DTAB molecules are shorter and have lower hydrophobicity, which can disperse faster in the solution and promote the early nucleation of tungsten trioxide grains; while OTAB molecular chains are longer and more hydrophobic, providing a more stable coating effect on the surface of the grains, inhibiting overgrowth, and guiding the grains to extend in a specific direction, ultimately forming a stable nanowire structure. After compounding, the rapid nucleation of DTAB and the stable growth characteristics of OTAB are combined, so that the size uniformity and morphological stability of tungsten trioxide nanowires are significantly improved. In addition, the molecular interaction between DTAB and OTAB enhances the orderliness of molecular adsorption on the surface of the grains, further optimizes the growth direction of the nanowires, thereby ensuring the high specific surface area and oxygen vacancy concentration of the material. This optimized microstructure significantly improves the performance of nanowires in gas sensing, especially in low-concentration ozone detection, showing extremely high sensitivity. The composite can more effectively control the size and growth of nanowires than a single surfactant, making the material have better sensing performance. Therefore, preferably, the cationic surfactant is a combination of octadecyltrimethylammonium bromide and dodecyltrimethylammonium bromide, and more preferably, the mass ratio of octadecyltrimethylammonium bromide to dodecyltrimethylammonium bromide is (1-4): (1-4), and the optimal is 1:1.

[0098] Figure 7 The concentration gradient response curve and concentration-response value curve of tungsten trioxide nanowires to ozone gas provided by Example 4 of the present invention. Figure 7 Since the tungsten oxide nanowires prepared in Example 4 have uniform width and good dispersibility, high specific surface area and oxygen vacancy concentration, the material has high sensitivity to low concentrations of ozone and can detect 0.1 ppm of ozone at a relatively low temperature (125°C).

[0099] Application Comparative Example 1:

[0100] This comparative example provides the test results of using tungsten trioxide semiconductor nanowire material synthesized by precipitation-hydrothermal method in the literature (Cryst. Growth Des. 2017, 17, 9, 4949-4957) to detect ozone concentration at 125°C.

[0101] The specific preparation method of the above-mentioned tungsten trioxide semiconductor nanowire material is as follows: 400 mg of WCl6 is dissolved in 40 ml of ethanol to form a transparent solution, which is placed in a 50 ml stainless steel autoclave lined with polytetrafluoroethylene, kept warm in air for 1 hour, then placed in a muffle furnace and heated to 200°C at a heating rate of 5°C / min, kept warm for 12 hours, and finally cooled naturally to room temperature. After centrifugation, the precipitate is washed with ethanol and distilled water, and finally dried at 60°C for 4 hours.

[0102] The specific test method includes the following steps:

[0103] Step A, dispersing the tungsten trioxide semiconductor nanowire material synthesized by the precipitation-hydrothermal method in the literature in anhydrous n-butanol and grinding it into a slurry, the mass ratio of the tungsten trioxide semiconductor nanowire material to the anhydrous n-butanol being 5:1;

[0104] Step B: evenly apply 1 μL of slurry material on the substrate of the MEMS test element (1×1 mm 2 ) and let dry;

[0105] Step C, heating the test element coated with the tungsten trioxide semiconductor nanowire material to 250° C. and aging for 48 hours;

[0106] Step D, placing the test element coated with the tungsten trioxide semiconductor nanowire material in the NanoRay MA1.0 gas sensing test system, adjusting the temperature to 125° C., injecting 0.1-2.5 ppm ozone successively and recording the response value;

[0107] See also Figure 8 The material has a low sensitivity to low concentrations of ozone. At relatively low temperatures (125°C), it is unable to detect 0.1-1ppm of ozone. The response value of the material to 2.5ppm of ozone is only 1.1, and the linear correlation between the response value and the concentration in this concentration range is poor (the correlation coefficient is 0.96).

[0108] Application Comparative Example 2:

[0109] This comparative application example provides the test results of using the tungsten trioxide semiconductor nanowire material synthesized in the method without adding a surfactant to detect ozone concentration at 125°C.

[0110] The specific preparation method is as follows: dissolve 150 mg of tungsten chloride solid in 50 ml of anhydrous n-propanol, stir at room temperature for 10 minutes to obtain a light yellow transparent solution (i.e., reaction solution); transfer the obtained light yellow transparent solution to a polytetrafluoroethylene bottle and seal it with a cover; put the polytetrafluoroethylene bottle containing the reaction solution into a hydrothermal kettle, cover it and tighten it; place the hydrothermal kettle containing the reaction solution in an oven, adjust the oven temperature at 180°C, and react for 24 hours; centrifuge the product obtained by the hydrothermal reaction to obtain a powder product, wash the powder product with ethanol, and then vacuum dry it at 40°C for 24 hours to obtain a tungsten trioxide semiconductor nanowire material.

[0111] The specific test method includes the following steps:

[0112] Step A, dispersing the above-mentioned tungsten trioxide semiconductor nanowire material in anhydrous n-butanol and grinding it into a slurry state, wherein the mass ratio of the tungsten trioxide semiconductor nanowire material to the anhydrous n-butanol is 5:1;

[0113] Step B: evenly apply 1 μL of slurry material on the substrate of the MEMS test element (1×1 mm 2 ) and let dry;

[0114] Step C, heating the test element coated with the tungsten trioxide semiconductor nanowire material to 250° C. and aging for 48 hours;

[0115] Step D, placing the test element coated with the tungsten trioxide semiconductor nanowire material in the NanoRay MA 1.0 gas sensing test system, adjusting the temperature to 125° C., injecting 0.1-2.5 ppm ozone successively and recording the response value;

[0116] See also Fig. 9 When no surfactant is added, the length of the tungsten oxide nanowire obtained is 2μm, the width is 60nm, and the uniformity and dispersion of the material are poor. The material is very insensitive to low concentrations of ozone. At relatively low temperatures (125°C), 0.1-1ppm ozone cannot be detected. The material's response value to 2.5ppm ozone is only 3.7, and the linear correlation between the response value and the concentration in this concentration range is poor (the correlation coefficient is 0.95).

[0117] The above is a preferred embodiment of the present invention. It should be noted that the present invention is not limited to the exemplary embodiments disclosed above. The essence of the description is only to help those skilled in the relevant field to comprehensively understand the specific details of the present invention. For those skilled in the art, without departing from the principles of the present invention, several improvements and modifications made within the technical scope disclosed by the present invention, and changes or replacements that can be easily thought of, should be covered within the protection scope of the present invention.

Claims

1. A method for preparing tungsten trioxide semiconductor nanowire material, It is characterized in that The steps include: Step A: adding a cationic surfactant into an organic solvent to prepare an organic solution containing the cationic surfactant; Step B: adding tungsten chloride to the organic solution containing the cationic surfactant to prepare a reaction solution; Step C: heating the reaction solution to perform a hydrothermal reaction; Step D: Centrifuge, wash and vacuum dry.

2. The method for preparing the tungsten trioxide semiconductor nanowire material according to claim 1, It is characterized in that The cationic surfactant is one or more of cetyltrimethylammonium bromide, cetyltrimethylammonium chloride, dodecyltrimethylammonium bromide, octadecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide and dodecyltrimethylammonium bromide.

3. The method for preparing the tungsten trioxide semiconductor nanowire material according to claim 1, It is characterized in that The organic solvent is one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol and isobutanol.

4. The method for preparing the tungsten trioxide semiconductor nanowire material according to claim 1, It is characterized in that The mass ratio of the cationic surfactant to the organic solvent is 1:(0.2-1).

5. The method for preparing the tungsten trioxide semiconductor nanowire material according to claim 1, It is characterized in that The mass ratio of the tungsten chloride to the organic solvent is 1:(1-6).

6. The method for preparing the tungsten trioxide semiconductor nanowire material according to claim 1, It is characterized in that The hydrothermal reaction conditions are 160-220° C. for 12-24 hours.

7. The method for preparing the tungsten trioxide semiconductor nanowire material according to any one of claims 1 to 6, It is characterized in that The steps include: Step A, adding a cationic surfactant to an organic solvent and mixing them evenly, stirring at room temperature for 10-20 minutes to obtain an organic solution containing a cationic surfactant; Step B, adding tungsten chloride to the organic solution containing the cationic surfactant, stirring for 10-20 minutes until it is completely dissolved, to obtain a reaction solution; Step C, transferring the reaction solution into a polytetrafluoroethylene bottle and sealing it with a cover; then placing the polytetrafluoroethylene bottle containing the reaction solution into a hydrothermal kettle and tightening it with a cover; placing it in an oven, adjusting the oven temperature between 160-220° C., and performing a hydrothermal reaction for 12-24 hours; Step D, centrifuging the product obtained by the hydrothermal reaction in step C, washing it with ethanol, and then vacuum drying it at 35-55° C. to obtain a tungsten trioxide semiconductor nanowire material.

8. A tungsten trioxide semiconductor nanowire material, It is characterized in that The method is prepared by any one of claims 1 to 7.

9. The tungsten trioxide semiconductor nanowire material according to claim 8, It is characterized in that The width of the tungsten trioxide semiconductor nanowire material is 20-50 nm; and the length is greater than 0.5 μm.

Citation Information

Cited By

  • Large-scale simple preparation method of ultra-long single crystal tungsten oxide nanowire

    CN121651435A