Glass forming method, glass and vehicle

By forming spaced-arranged penetration holes on the glass and controlling the difference in cooling speed for cutting, the problem of glass forming difficulty and poor optical quality in the concave area is solved, and glass forming with low tensile stress and high optical quality is achieved, which improves the Productivity and user experience.

CN119038861AActive Publication Date: 2024-11-29FUYAO GLASS IND GROUP CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411138367.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-29
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

When handling glass with concave areas or holes, existing glass forming processes have problems such as difficult cutting, low yield, high edge tension stress and poor optical quality, especially heating of the inner contour during thermal bending forming. and uneven cooling lead to sudden changes in bending trends and poor refractive refractive power.

Method used

The penetration holes arranged spaced along the preset inner contour line on the glass are formed to form a point penetration cutting path, separate the first area from the second area through heating and cooling, and use the cooling air nozzle to control the difference in cooling speed for cutting. , reduce the tensile stress of the inner profile and improve the optical quality.

Benefits of technology

It effectively reduces the difficulty of forming the inner contour of the glass, improves the yield rate, reduces production costs, and ensures that the inner contour of the molded glass has low tension stress and high optical quality, avoids the risk of lobes and discontinuous curvature changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038861A_ABST
    Figure CN119038861A_ABST
Patent Text Reader

Abstract

The invention relates to a glass forming method, glass and a vehicle, and the glass forming method comprises the following steps: forming the outer contour of the glass along an outer contour line preset on the glass; forming a plurality of penetrating holes in the glass, and arranging the plurality of penetrating holes at intervals along an inner contour line preset on the glass to form a point penetrating cutting path; the glass is heated; the heated glass is cooled; wherein the cooling speed of a first area, located on the inner side of the point penetrating cutting path, on the glass is smaller than the second cooling speed of a glass area, located on the outer side of the point penetrating cutting path, on the glass, so that the first area is separated from the second area; the first region is removed, and the second region is retained. The technical problems that the glass with the inner contour is difficult to form, high edge tensile stress is easily generated after forming, and the optical quality is poor are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of glass, and in particular to a glass forming method, glass and a vehicle. Background Art

[0002] At present, the process flow used for physically strengthened glass (such as automotive glass) is mainly as follows: the original glass is first cut, bent, and ground to form the desired contour shape, then the necessary decorative layer is printed on the glass, and then it is processed through processes such as hot bending, heat strengthening, and tempering to bend the glass into the desired shape. Finally, according to functional requirements, the interlayer and accessory integration processes are completed on the product.

[0003] However, for glass with special contour shapes such as a large concave area, inner hole or window in window on the glass (where the outer contour of the glass is the outer contour, and the edge position of the concave area, inner hole or window in window is the inner contour of the glass), it is necessary to adopt a process of cutting and grinding first and then hot bending. However, this forming method has the following problems:

[0004] 1. Due to the difficulty of glass cutting and edge bending technology, the cycle time and yield rate are low. When forming the inner contour of glass, complex cutting and edge bending design is required, which is easy to cause edge bursting and low yield rate. If the offline water jet cutting method is adopted, not only the cutting speed is slow, but also additional processes such as rinsing and inner edge grinding are required after cutting, which is complex and costly.

[0005] 2. During the hot bending or tempering process of the glass, stress and optical defects are easily generated on the inner contour of the glass. Since the heating and cooling speeds of the edges of the concave area and the inner hole are inconsistent with the normal glass areas around them, the thermal expansion and cooling contraction of the inner contour of the glass are restricted in the internal space, resulting in greater edge tensile stress at the inner contour of the glass than at the outer contour of the glass, increasing the risk of glass cracking. In addition, during the hot forming process, the glass is affected by the bending tendency of the inner contour of the glass, which is prone to discontinuous curvature changes, resulting in poor refractive optics of the inner contour of the glass, resulting in unsatisfactory use of the formed glass.

[0006] In the related art, glass with an inner contour is difficult to shape, and is prone to high edge tensile stress and poor optical quality after shaping. Summary of the invention

[0007] The purpose of the present invention is to provide a glass forming method, glass and vehicle, which change the original glass forming process and can form glass with an inner contour and low tensile stress at the edge of the inner contour and high optical quality. At the same time, it can greatly reduce the difficulty of forming the inner contour of the glass, improve the yield rate and reduce production costs.

[0008] The purpose of the present invention can be achieved by adopting the following scheme:

[0009] The present invention provides a glass forming method, which comprises the following steps:

[0010] Shape the outer contour of the glass along the outer contour line preset on the glass;

[0011] Forming a plurality of penetration holes on the glass, wherein the plurality of penetration holes are arranged at intervals along an inner contour line preset on the glass to form a point penetration cutting path;

[0012] heating the glass;

[0013] Cooling the heated glass; wherein a cooling rate of a first region on the glass and located inside the point penetration cutting path is lower than a cooling rate of a second region on the glass and located outside the point penetration cutting path, so that the first region is separated from the second region;

[0014] The first area is removed, and the second area is retained.

[0015] In a preferred embodiment of the present invention, a plurality of penetration holes are formed on the glass, and the plurality of penetration holes are arranged at intervals along an inner contour line preset on the glass to form a point penetration cutting path, including:

[0016] Cutting the glass by laser to form the through hole on the glass;

[0017] A plurality of the penetration holes are arranged at intervals to form the point penetration cutting path;

[0018] Locally heating the area on the glass corresponding to the point-through cutting path to enlarge the size of the penetration hole on the point-through cutting path to form a cutting line that can separate the first area.

[0019] In a preferred embodiment of the present invention, after the area corresponding to the point-penetrating cutting path on the glass is locally heated, the first area and the second area are still in a connected state.

[0020] In a preferred embodiment of the present invention, the diameter of the through-hole is 2 μm to 20 μm, and / or the distance between two adjacent through-holes is 1 μm to 10 μm.

[0021] In a preferred embodiment of the present invention, after heating the glass and before cooling the glass, the method further comprises:

[0022] The glass is subjected to a bending process so as to form the glass into a preset curved shape.

[0023] In a preferred embodiment of the present invention, the glass is cooled by blowing with compressed air at room temperature;

[0024] Wherein, cooling air nozzles are arranged in the first area and the second area respectively, and the density and number of the cooling air nozzles arranged in the second area are greater than the density and number of the cooling air nozzles arranged in the first area;

[0025] Alternatively, cooling air nozzles are arranged only in the second area.

[0026] In a preferred embodiment of the present invention, if the glass is tempered glass, the wind pressure in the second area is set to be greater than or equal to 1500 mmWC, and the wind pressure in the first area is set to be less than or equal to 1200 mmWC.

[0027] In a preferred embodiment of the present invention, the glass is heat-strengthened glass, and the wind pressure in the second area is set to be greater than or equal to 800 mmWC, and the wind pressure in the first area is set to be less than or equal to 600 mmWC.

[0028] The present invention provides a glass having a concave area on the outer contour of the glass or a hollow area inside the outer contour of the glass, so that an inner contour line of the glass is formed along the edge of the concave area or the hollow area;

[0029] The concave area or the hollow area is formed by the above-mentioned glass forming method.

[0030] In a preferred embodiment of the present invention, the glass is tempered glass or heat-strengthened glass.

[0031] In a preferred embodiment of the present invention, if the glass is tempered glass, the tensile stress on the inner contour edge of the glass is 8MPa to 28MPa, and the tensile stress on the outer contour edge of the glass is 10MPa to 35MPa;

[0032] Alternatively, if the glass is heat-strengthened glass, the tensile stress on the inner contour edge of the glass is 4 MPa to 16 MPa, and the tensile stress on the outer contour edge of the glass is 5 MPa to 20 MPa.

[0033] In a preferred embodiment of the present invention, a chamfer with a straight or arc-shaped cross section is provided along the edge of the inner contour line of the glass.

[0034] In a preferred embodiment of the present invention, the length L of the chamfer is 0.2 mm to 1 / 4 of the thickness H of the glass.

[0035] In a preferred embodiment of the present invention, the length L of the chamfer is 0.2 mm to 2.0 mm of the thickness H of the glass.

[0036] In a preferred embodiment of the present invention, the depth h of the chamfer is less than or equal to 1 / 3 of the thickness H of the glass.

[0037] In a preferred embodiment of the present invention, if the glass is tempered glass, the thickness H of the glass is 2.5 mm to 6.0 mm;

[0038] Alternatively, if the glass is heat-strengthened glass, the thickness H of the glass is 1.4 mm to 2.5 mm.

[0039] In a preferred embodiment of the present invention, the perimeter of the inner contour line of the glass is greater than or equal to 300 mm.

[0040] The present invention provides a vehicle, wherein the vehicle has the above-mentioned glass.

[0041] As described above, the characteristics and advantages of the glass forming method, glass and vehicle of the present invention are:

[0042] The original forming method of the inner contour on the glass is changed. First, a plurality of penetration holes arranged at intervals are formed on the glass along a preset inner contour line. The arrangement path of the plurality of penetration holes is the formed point penetration cutting path. Then the glass is heated and quickly cooled. Since the cooling rate of the first area located on the inner side of the point penetration cutting path is lower than the cooling rate of the second area located on the outer side of the point penetration cutting path, the first area and the second area on the glass have different rates of thermal expansion and contraction due to heat, resulting in different degrees of deformation of the first area and the second area. Therefore, the glass can be cut along the point penetration cutting path to separate the first area and the second area on the glass. The inner contour position of the glass formed by the above method is subjected to small tensile stress, which reduces the risk of glass cracking after forming. Moreover, the inner contour position of the formed glass will not have a sudden change in bending trend and will not form a discontinuous curvature change, thereby ensuring that the formed glass has good optical quality and improves the user experience. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The following drawings are only intended to illustrate and explain the present invention, and are not intended to limit the scope of the present invention.

[0044] in:

[0045] Figure 1 : is one of the flow charts of the glass forming method of the present invention;

[0046] Figure 2 : is the second flow chart of the glass forming method of the present invention;

[0047] Figure 3 : is one of the structural schematic diagrams of the glass of the present invention;

[0048] Figure 4 : is the second structural schematic diagram of the glass of the present invention;

[0049] Figure 5 : is a schematic diagram of the position of the penetration hole in the glass of the present invention during the molding process;

[0050] Figure 6 : A schematic diagram showing the separation of the first area and the second area of ​​the glass during the forming process of the present invention;

[0051] Figure 7 : is a partial schematic diagram of the chamfer position in the glass of the present invention;

[0052] Figure 8 : is a schematic diagram of the structure of the glass refractive optical testing device in the present invention;

[0053] Fig. 9 : One of the grid images formed by using the glass of the present invention to perform refractive optical quality testing;

[0054] Fig.10 : A second grid image formed by using the glass of the present invention to perform a refractive optical quality test;

[0055] Fig.11 : One of the grid images formed by the refractive optical quality test using traditional glass;

[0056] Fig.12 : The second grid image formed by using traditional glass for refractive optical quality testing.

[0057] The accompanying drawings in the present invention are:

[0058] 1. Glass; 101. Outer contour line;

[0059] 102, inner contour line; 103, penetration hole;

[0060] 104. First area; 105. Second area;

[0061] 106. chamfer; 10. grid part;

[0062] 20. Lighting device; 30. Placement support device;

[0063] 40. back panel; 50. image acquisition device;

[0064] 60. Ceiling. DETAILED DESCRIPTION

[0065] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described with reference to the accompanying drawings.

[0066] Implementation Method 1

[0067] like Figures 1 to 5 As shown, the present invention provides a glass forming method, which includes the following steps:

[0068] Step S1: shaping the outer contour of the glass 1 along the outer contour line 101 preset on the glass 1;

[0069] Step S2: forming a plurality of penetration holes 103 on the glass 1, wherein the plurality of penetration holes 103 are arranged at intervals along an inner contour line 102 preset on the glass 1 to form a point penetration cutting path;

[0070] Step S3: heating the glass 1;

[0071] Step S4: Cooling the heated glass 1; wherein the cooling rate of the first region 104 on the glass 1 and located inside the point penetration cutting path is lower than the cooling rate of the second region 105 on the glass 1 and located outside the point penetration cutting path, so that the first region 104 is separated from the second region 105;

[0072] Step S5: remove the first area 104 and keep the second area 105.

[0073] In the present invention, by changing the original forming method of the inner contour on the glass, a plurality of through holes 103 arranged at intervals are first formed on the glass 1 along the preset inner contour line 102, and the arrangement path of the plurality of through holes 103 is the formed point penetration cutting path, and then the glass 1 is heated and quickly cooled. Since the cooling rate of the first area 104 on the glass 1 and located on the inner side of the point penetration cutting path is lower than the cooling rate of the second area 105 on the glass 1 and located on the outer side of the point penetration cutting path, the first area 104 and the second area 105 on the glass 1 will have different shrinkage degrees due to the inconsistent speed of thermal expansion and contraction, so that the first area 104 and the second area 105 on the glass 1 can be separated along the point penetration cutting path. The inner contour position of the glass 1 formed by the above method is subjected to small tensile stress, which reduces the risk of glass cracking after forming, and the inner contour position of the formed glass 1 will not have a sudden change in bending trend, and will not form a discontinuous curvature change, thereby ensuring that the formed glass 1 has good optical quality and improves the user experience. In addition, the glass forming method of the present invention can significantly reduce the difficulty of forming the inner contour of the glass 1, improve the yield of the glass, and reduce production costs.

[0074] In step S1 of the present invention, an outer contour line 101 may be preset on the glass 1 according to the shape of the glass 1 to be formed, and the outer contour of the glass 1 may be formed along the outer contour line 101 preset on the glass 1 using an existing forming method, thereby forming the outer contour shape of the glass 1. The method of forming the outer contour of the glass 1 may include, but is not limited to, cutting, edge grinding, and other treatments on the glass 1, and may also be configured to apply a decorative layer such as an ink layer and a silver paste layer according to actual needs to meet the decorative requirements of the glass 1. Of course, other methods may also be used, and the specific method of forming the outer contour shape of the glass 1 is not limited here.

[0075] In an optional embodiment of the present invention, Figure 2 As shown, step S2 includes:

[0076] Step S201: cutting the glass 1 by laser to form a through hole 103 on the glass 1;

[0077] The laser for cutting the glass 1 may be, but is not limited to, nanosecond short pulse laser, picosecond ultrashort pulse laser or femtosecond ultrashort pulse laser.

[0078] Step S202 : a plurality of penetration holes 103 are arranged at intervals to form a point penetration cutting path; wherein, the overall arrangement trend of the plurality of penetration holes 103 on the inner contour line 102 of the glass 1 is to be continuously distributed along the inner contour line 102 of the glass 1 .

[0079] Step S203: locally heating the area corresponding to the point-penetrating cutting path on the glass 1 to enlarge the size of the penetration hole 103 on the point-penetrating cutting path to form a cutting line that can separate the first area 104.

[0080] The glass 1 is locally heated, and heating methods such as CO2 laser or local heating tube may be used but are not limited to it. By locally heating and expanding the glass 1, a plurality of discontinuous penetration holes 103 are enlarged, the distance between two adjacent penetration holes 103 is reduced, and microcracks are generated between two adjacent penetration holes 103, so as to ensure that the first area 104 and the second area 105 can be separated smoothly after subsequent operations.

[0081] In step S203, by locally heating the area corresponding to the point penetration cutting path on the glass 1, the size of the penetration hole 103 can be enlarged and the distance between two adjacent penetration holes 103 can be shortened, so that the first area 104 and the second area 105 can be more easily separated, and it is easier to achieve cutting along the point penetration cutting path. Among them, the size of the penetration hole 103 and the specific range of the distance between two adjacent penetration holes 103 can be adjusted according to the difficulty of separation between the first area 104 and the second area 105. The distance between two adjacent penetration holes 103 can be equal or different, and the size of the penetration hole 103 can be the same or different, which can ensure that after the steps S3 and S4 are completed in sequence, the first area 104 and the second area 105 on the glass 1 can be separated smoothly.

[0082] In step S203 , after the area corresponding to the point-through cutting path on the glass 1 is locally heated, the first area 104 and the second area 105 are still not separated.

[0083] In this embodiment, the through hole 103 may be a circular hole or close to a circular hole, and the diameter of the through hole 103 may be, but is not limited to, 2 μm to 20 μm.

[0084] Furthermore, the distance between two adjacent through holes 103 (ie, the distance between the centers of two adjacent through holes 103 ) may be, but is not limited to, 1 μm to 10 μm.

[0085] In an optional embodiment of the present invention, before step S3 and step S4, the glass 1 may be bent to form a preset curved shape. The bending process of the glass 1 may be performed by, but not limited to, hot bending or hot pressing. The positions of the outer contour and inner contour of the glass 1 on the mold used in the bending process need to be designed according to the preset outer contour line 101 and inner contour line 102 of the glass 1. After the bending process is completed, subsequent annealing, heat strengthening or tempering treatment may be performed as needed.

[0086] In an optional embodiment of the present invention, in step S4, the glass may be blown to cool / anneal the glass using compressed air at room temperature;

[0087] Among them, cooling air nozzles can be arranged in the first area 104 and the second area 105 respectively, and it is necessary to ensure that the density and number of cooling air nozzles arranged in the second area 105 are greater than the density and number of cooling air nozzles arranged in the first area 104, so as to achieve the purpose of controlling the cooling speed of the first area 104 to be lower than the cooling speed of the second area 105. Alternatively, cooling air nozzles can be arranged only in the second area 105, while cooling air nozzles are not arranged in the first area 104. Figure 6As shown, the overall size of the glass 1 (the first region 104 and the second region 105) expands when heated at a high temperature, and the first region 104 and the second region 105 expand to the same extent. At this time, the cooling rate of the second region 105 can be controlled to be greater than the cooling rate of the first region 104, so that the shrinkage of the second region 105 after the cooling treatment is less than the shrinkage of the first region 104 after the cooling treatment, thereby achieving complete separation of the first region 104 and the second region 105 at the point penetration cutting path.

[0088] In an optional embodiment of the present invention, if the glass 1 is tempered glass, the wind pressure of the second area 105 is set to be greater than or equal to 1500 mmWC, and the wind pressure of the first area 104 is set to be less than or equal to 1200 mmWC. The surface stress of the tempered glass is greater than or equal to 90 MPa.

[0089] In another optional embodiment of the present invention, if the glass 1 is heat-strengthened glass, the wind pressure of the second area 105 is set to be greater than or equal to 800 mmWC, and the wind pressure of the first area 104 is set to be less than or equal to 600 mmWC. The surface stress of the heat-strengthened glass is 15-60 MPa.

[0090] Since the surface stress of tempered glass is relatively large, a fast cooling speed and a large cooling wind pressure are required; while the surface stress of laminated glass and heat-strengthened glass is relatively small, and a laminated sheet is required to be laminated glass and heat-strengthened glass to ensure safety in use. Therefore, the required cooling speed and wind pressure are relatively small, and the above-mentioned wind pressure ranges are respectively applicable to the cooling treatment of tempered glass and laminated glass and heat-strengthened glass in the present invention.

[0091] In an optional embodiment of the present invention, in step S5, the first region 104 separated from the second region 105 on the glass 1 may be removed by, but not limited to, sucking, lifting and / or blowing. Of course, it is also possible that the first region 104 and the second region 105 are automatically separated under the weight of the first region 104 without other auxiliary means.

[0092] In an optional embodiment of the present invention, after step S5, the glass can be chamfered along the inner contour line 102 in the glass area outside the point penetration cutting path to obtain a finished glass, thereby avoiding the edge of the inner contour line 102 of the finished glass being too sharp, avoiding possible safety accidents, and helping to optimize the appearance and touch of the molded glass, and avoiding the possibility of the molded glass being broken as a whole due to easy collision at the sharp corners. The above-mentioned chamfer is described from the perspective of the cross section of the glass 1, and if it is along the extension direction of the inner contour line 102, it can also be understood as a chamfer.

[0093] Further, such as Figure 7As shown, the length L of the chamfer 106 (i.e., the dimension at the location of the chamfer 106 and perpendicular to the thickness direction of the glass 1) is 0.2 mm to 1 / 4 of the thickness H of the glass 1, i.e., 0.2≤L≤(1 / 4)H. Thus, the problem of sharp glass edges can be solved.

[0094] Further, such as Figure 7 As shown, the depth h of the chamfer 106 (i.e., the dimension at the location of the chamfer 106 and along the thickness direction of the glass 1) is less than or equal to 1 / 3 of the thickness H of the glass 1, i.e., h≤(1 / 3)H. The depth of the stress layer on the glass 1 needs to be considered when setting the depth of the chamfer 106. Usually, the stress depth of the tempered or heat-strengthened glass 1 is about 1 / 3 of the thickness of the glass 1. Therefore, the depth of the chamfer 106 can be set to not exceed 1 / 3 of the thickness of the glass 1, so that the setting of the chamfer 106 will not damage the stress layer on the glass 1, thereby ensuring the strength of the glass 1.

[0095] In an optional embodiment of the present invention, after step S5, the finished glass may be subjected to subsequent processing, wherein the subsequent processing includes but is not limited to accessory integration processing, lamination and edge wrapping processing. The specific subsequent processing required for the glass 1 may be determined according to the actual vehicle usage.

[0096] The characteristics and advantages of the glass forming method of the present invention are:

[0097] 1. The inner contour of the glass 1 formed by the above-mentioned glass forming method is subjected to little tensile stress, thereby reducing the risk of glass cracking after forming. In addition, the inner contour of the formed glass 1 will not have a sudden change in bending trend and will not form a discontinuous curvature change, thereby ensuring that the glass 1 has good optical quality after forming and improving the user experience.

[0098] Second, the above-mentioned glass forming method can greatly reduce the difficulty of forming the inner contour of the glass 1, improve the yield of the glass, and reduce the production cost.

[0099] Implementation Method 2

[0100] like Figures 3 to 7 As shown, the present invention provides a glass 1, which is formed by the above-mentioned glass forming method, and has a concave area (such as Figure 4 As shown) or having a hollow area on the inner side of the outer contour of the glass 1 (as shown Figure 5 As shown), to form an inner contour line 102 of the glass 1 along the edge of the concave area or the hollow area; wherein the concave area or the hollow area is formed by the above-mentioned glass forming method.

[0101] In an optional embodiment of the present invention, for the glass 1 formed in the present invention, the tensile stress at the inner contour line 102 of the glass 1 is less than the tensile stress at the outer contour line 101 of the glass 1, and the circumference of the inner contour line 102 of the glass 1 is greater than or equal to 300 mm.

[0102] Furthermore, the tensile stress at the inner contour line 102 of the glass 1 is less than 80% of the tensile stress at the outer contour line 101 of the glass 1. Compared with the glass with a concave area or a hollow area formed by a traditional method, the tensile stress at the inner contour line 102 of the glass 1 of the present invention is greatly reduced, thereby effectively avoiding the risk of glass cracking.

[0103] In the present invention, the glass 1 may be, but is not limited to, tempered glass or heat-strengthened glass.

[0104] If the glass 1 is a tempered glass, the tensile stress on the inner contour line 102 of the glass 1 is 8 MPa to 28 MPa, and the tensile stress on the outer contour line 101 of the glass 1 is 10 MPa to 35 MPa.

[0105] If the glass 1 is heat-strengthened glass, the tensile stress at the inner contour line 102 of the glass 1 is 4 MPa to 16 MPa, and the tensile stress at the outer contour line 101 of the glass 1 is 5 MPa to 20 MPa.

[0106] In an optional embodiment of the present invention, if the glass 1 is tempered glass, the thickness H of the glass 1 may be, but is not limited to, 2.5 mm to 6.0 mm. The color of the glass 1 may be, but is not limited to, white glass C, green glass G, dark green glass SG, and gray glass Y.

[0107] In another optional embodiment of the present invention, if the glass 1 is heat-strengthened glass, the thickness H of the glass 1 may be, but is not limited to, 1.4 mm to 2.5 mm. The color of the glass 1 may be, but is not limited to, white glass C, green glass G, dark green glass SG, and gray glass Y.

[0108] In an optional embodiment of the present invention, Figure 7 As shown, a chamfer 106 having a straight or arc-shaped cross section is provided along the edge of the inner contour line 102 of the glass 1 .

[0109] The length L of the chamfer 106 (i.e., the dimension at the position of the chamfer 106 and perpendicular to the thickness direction of the glass 1) is 0.2 mm to 1 / 4 of the thickness H of the glass 1, i.e., 0.2≤L≤(1 / 4)H. Preferably, the length L of the chamfer 106 is 0.2 mm to 2.0 mm of the thickness H of the glass, i.e., 0.2≤L≤(1 / 4)×2.0.

[0110] The depth h of the chamfer 106 (ie, the dimension at the location of the chamfer 106 and along the thickness direction of the glass 1 ) is less than or equal to 1 / 3 of the thickness H of the glass 1 , ie, h≤(1 / 3)H.

[0111] In addition, the present invention also provides a glass refraction optical testing device for testing the refraction quality of the inner contour line 102 or the position close to the inner contour line 102 of the formed glass in the present invention. Specifically,

[0112] like Figure 8 As shown, the glass refractive optical testing device includes a grid portion 10 with crossed grid lines, a placement support device 30, a back plate 40 and an image acquisition device 50. The back plate 40 is arranged on the top of the placement support device 30, and the glass 1 is fixedly arranged on the top of the back plate 40. The grid portion 10 is arranged above the placement support device 30 so that the grid lines on the grid portion 10 can be displayed on the glass 1 below. The image acquisition device 50 is located on one side of the placement support device 30 and is located at the same height as the glass 1 so that the image acquisition device 50 can accurately capture the image of the grid lines reflected from the surface of the glass 1. The refractive optical quality of the glass 1 can be determined based on whether the captured grid lines reflected from the surface of the glass 1 are distorted.

[0113] The back plate 40 is a black background plate, which ensures that the glass 1 can display the image of the grid lines more clearly and also ensures that the collected image is clearer and more accurate.

[0114] The image acquisition device 50 may be, but is not limited to, a camera.

[0115] In the present invention, the image acquisition device 50 can be used to automatically acquire the image of the grid lines reflected from the surface of the glass 1, which has the advantage of high accuracy. Of course, the human eye can also be used to directly observe the surface of the glass 1 at the location of the image acquisition device 50 to determine whether the grid lines reflected from the surface of the glass 1 are distorted.

[0116] In an optional embodiment of the present invention, Figure 8 As shown, the grid portion 10 may be, but is not limited to, a plurality of horizontal lines and a plurality of vertical lines (which may be formed by tensioning white nylon lines, but must be distinguished from the plane background in color) arranged crosswise on a plane, the plurality of horizontal lines are parallel to each other, the plurality of vertical lines are parallel to each other, and the plurality of horizontal lines and the plurality of vertical lines are perpendicularly crossed to form a plane grid of 30×30 mm. The grid portion 10 may be disposed on the ceiling 60 or near the ceiling 60.

[0117] In an optional embodiment of the present invention, Figure 8As shown, the glass refractive optical testing device further includes a plurality of lighting devices 20, which are evenly and spacedly arranged below the grid portion 10 along the circumference of the grid portion 10, and the light emitted by the lighting devices 20 is directed toward the grid portion 10 at a preset tilt angle to ensure that the grid can be clearly displayed. The lighting devices 20 may be, but are not limited to, fluorescent lamps.

[0118] In an optional embodiment of the present invention, Figure 8 As shown, the placement support device 30 includes a lifting bracket, and a roller is provided at the bottom of the lifting bracket, which can drive the glass 1 to move, so as to adjust the position of the glass 1; in addition, one end of the back plate 40 is hinged to the top of the lifting bracket, and the lifting bracket itself can adjust the height to ensure that the glass 1 can be at the same height as the image acquisition device 50, and by adjusting the angle between the back plate 40 and the lifting bracket, the inclination angle of the glass 1 relative to the horizontal plane can also be adjusted to ensure that the image acquisition device 50 can accurately and clearly capture the image of the grid lines reflected on the surface of the glass 1.

[0119] In an optional embodiment of the present invention, Figure 8 As shown, the vertical distance N between the grid portion 10 and the center of the glass 1 is 1 m to 2 m, preferably 1.4 m.

[0120] The following is a specific embodiment in which the glass refractive optical testing device of the present invention is used to test the refractive optical quality of the glass 1 having the concave area and the glass 1 having the hollow area.

[0121] During the test, a white nylon line is stretched into a 30×30mm plane grid and hovered above the detection area at an appropriate height. A plurality of fluorescent lamps are arranged below the grid portion 10 along its circumference, and the angle of incident light is adjusted so that the light emitted by the fluorescent lamp is directed to the upper grid portion 10 at a certain inclination angle. During the test, the glass 1 is placed on the placement support device 30 below the grid portion 10 at a preset angle, and a black back plate 40 is placed below the glass 1. The human eye or image acquisition device 50 is placed at the same horizontal height as the glass 1, and the grid stripes reflected on the surface of the glass 1 are observed at a certain distance. The grid area should be large enough to allow the white grid to be completely reflected on the surface of the glass 1.

[0122] The test results and comparison examples are shown in Table 1 below.

[0123]

[0124]

[0125] Table 1

[0126] It can be seen from the above test comparison experiments that the glass 1 formed by the glass forming method of the present invention, when the glass 1 is heat-strengthened glass and the thickness is in the range of 1.4mm-2.5mm, the tensile stress at the inner contour line 102 of the glass 1 is 4MPa to 16MPa, the tensile stress at the outer contour line 101 of the glass 1 is 5MPa to 20Mpa, and the formed heat-strengthened glass has harmonious and uniform refractive optical quality; when the glass 1 is tempered glass and the thickness is in the range of 2.5mm-6.0mm, the tensile stress at the inner contour line 102 of the glass 1 is 8MPa to 28MPa, the tensile stress at the outer contour line 101 of the glass 1 is 10MPa to 35Mpa, and the formed tempered glass has harmonious and uniform refractive optical quality.

[0127] In addition, by comparing Examples 1-10 with Comparative Examples 1 and 2, it can be found that the tensile stress on the inner contour of the glass 1 formed by the glass forming method of the present application is smaller than that on the glass formed by the traditional method, which can reduce the risk of glass cracking after forming. Figures 9 to 12 By comparison, it can be intuitively found that the inner contour position of the glass 1 made by the glass forming method of the present invention will not have a sudden change in bending trend, and will not form a discontinuous curvature change, thereby ensuring that the glass 1 has good optical quality after forming and improving the user experience.

[0128] Implementation Method 3

[0129] The present invention provides a vehicle, wherein the vehicle has the glass 1 mentioned above.

[0130] Among them, the glass 1 is used as the front windshield, door glass, window glass and rear windshield of the vehicle. Of course, it can also be used in other locations of the vehicle where the glass 1 can be installed, so that the glass 1 with a concave area or a hollow area can be adapted and installed with the vehicle.

[0131] In the present invention, after the glass 1 is formed, the formed glass 1 may be subjected to, but not limited to, accessory integration processing, lamination and edge wrapping processing to form the required automotive glass. The specific subsequent processing required for the glass 1 may be determined according to the actual vehicle usage.

[0132] The vehicle of the present invention has the advantages and features of the above-mentioned glass 1, which will not be described in detail here.

[0133] The above description is only an illustrative embodiment of the present invention and is not intended to limit the scope of the present invention. Any equivalent changes and modifications made by any person skilled in the art without departing from the concept and principle of the present invention shall fall within the scope of protection of the present invention.

Claims

1. A glass forming method, characterized in that: The method comprises the following steps: Shape the outer contour of the glass along the outer contour line preset on the glass; Forming a plurality of penetration holes on the glass, wherein the plurality of penetration holes are arranged at intervals along an inner contour line preset on the glass to form a point penetration cutting path; heating the glass; Cooling the heated glass; wherein a cooling rate of a first region on the glass and located inside the point penetration cutting path is lower than a cooling rate of a second region on the glass and located outside the point penetration cutting path, so that the first region is separated from the second region; The first area is removed, and the second area is retained.

2. The glass forming method according to claim 1, characterized in that: The step of forming a plurality of penetration holes on the glass, wherein the plurality of penetration holes are arranged at intervals along an inner contour line preset on the glass to form a point penetration cutting path, comprises: Cutting the glass by laser to form the through hole on the glass; A plurality of the penetration holes are arranged at intervals to form the point penetration cutting path; Locally heating the area on the glass corresponding to the point-through cutting path to enlarge the size of the penetration hole on the point-through cutting path to form a cutting line that can separate the first area.

3. The glass forming method according to claim 2, characterized in that: After locally heating the area on the glass corresponding to the point-penetrating cutting path, the first area and the second area are still in a connected state.

4. The glass forming method according to claim 2 or 3, characterized in that: The diameter of the through holes is 2 μm to 20 μm, and / or the distance between two adjacent through holes is 1 μm to 10 μm.

5. The glass forming method according to claim 1, wherein: After heating the glass and before cooling the glass, the method further comprises: The glass is subjected to a bending process so as to form the glass into a preset curved shape.

6. The glass forming method according to claim 1, wherein: Using compressed air at room temperature to blow and cool the glass; Wherein, cooling air nozzles are arranged in the first area and the second area respectively, and the density and number of the cooling air nozzles arranged in the second area are greater than the density and number of the cooling air nozzles arranged in the first area; Alternatively, cooling air nozzles are arranged only in the second area.

7. The glass forming method according to claim 6, characterized in that: If the glass is tempered glass, the wind pressure in the second area is set to be greater than or equal to 1500 mmWC, and the wind pressure in the first area is set to be less than or equal to 1200 mmWC.

8. The glass forming method according to claim 6, wherein: If the glass is heat-strengthened glass, the wind pressure in the second area is set to be greater than or equal to 800 mmWC, and the wind pressure in the first area is set to be less than or equal to 600 mmWC.

9. A glass, characterized in that: A concave area is provided on the outer contour of the glass or a hollow area is provided inside the outer contour of the glass, so that an inner contour line of the glass is formed along the edge of the concave area or the hollow area; The tensile stress on the inner contour edge of the glass is smaller than the tensile stress on the outer contour edge of the glass.

10. The glass according to claim 9, characterized in that The glass is tempered glass or heat-strengthened glass.

11. The glass according to claim 9, characterized in that If the glass is tempered glass, the tensile stress on the inner contour edge of the glass is 8MPa to 28MPa, and the tensile stress on the outer contour edge of the glass is 10MPa to 35MPa; Alternatively, if the glass is heat-strengthened glass, the tensile stress on the inner contour edge of the glass is 4 MPa to 16 MPa, and the tensile stress on the outer contour edge of the glass is 5 MPa to 20 MPa.

12. The glass according to claim 9, characterized in that A chamfer with a straight or arc-shaped cross section is arranged along the edge of the inner contour line of the glass.

13. The glass according to claim 12, characterized in that The length L of the chamfer is 0.2 mm to 1 / 4 of the thickness H of the glass.

14. The glass according to claim 13, characterized in that The length L of the chamfer is 0.2 mm to 2.0 mm of the thickness H of the glass.

15. The glass according to claim 12, characterized in that The depth h of the chamfer is less than or equal to 1 / 3 of the thickness H of the glass.

16. The glass according to claim 13, wherein: If the glass is tempered glass, the thickness H of the glass is 2.5 mm to 6.0 mm; Alternatively, if the glass is heat-strengthened glass, the thickness H of the glass is 1.4 mm to 2.5 mm.

17. The glass according to claim 9, characterized in that The perimeter of the inner contour line of the glass is greater than or equal to 300 mm.

18. A vehicle, characterized in that: The vehicle comprises the glass according to any one of claims 9 to 17.

Citation Information

Patent Citations

  • 3D laser perforation thermal sagging process

    CN110678422A

  • Splitting method and splitting device for laser cutting glass

    CN113333967A

  • Method for mfg.notch on plane glass / glass ceramic body

    CN1600715A

  • Systems and methods for fabricating ring structures

    TW202430305A

  • 3-d forming of glass

    US20160311717A1