Low-elastic-modulus light-weight high-strength concrete and preparation method thereof
By using modified rubber particles to wrap sulfaluminate cement and homemade high-strength ceramic particles, the brittleness of high-strength light aggregate concrete and the easy floating and peeling during the forming process of rubber concrete is solved, and the impact resistance of concrete is improved and Load capacity has achieved the goal of resource recycling and environmental protection of waste tires.
Patent Information
- Application Number
- CN202410973247.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-19
AI Technical Summary
High-strength light aggregate concrete has safety hazards of brittle damage under high load conditions, and the problems of existing rubber concrete being easily floated during the molding process and being easily peeled under load have not been effectively solved.
Modified rubber particles are used to wrap sulfaluminate cement. Through modification treatment and the use of water glass, the bonding strength between the rubber and cement-based materials is enhanced, the possibility of rubber peeling under load is reduced, and high titanium slag is passed , ferrochrome slag and other industrial solid wastes make high-strength ceramic particles to replace natural materials, improving the mechanical properties of concrete.
It significantly reduces the brittleness of concrete, improves impact resistance and frost resistance, enhances load capacity, ensures the stability and performance of rubber particles in lightweight high-strength concrete, and provides a new way to reuse waste tires. At the same time, it reduces pollution to the natural environment.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a low elastic modulus lightweight high-strength concrete and a preparation method thereof. Background Art
[0002] With the development of urbanization, buildings are gradually developing towards high-rise, large-span, and diversified structures. At the same time, the environmental conditions of buildings are also complex and changeable. In order to meet the structural requirements, most buildings currently use high-strength concrete with high strength and good durability. However, its large self-weight defect is gradually magnified with the increase of floors and bridge spans, which to a certain extent provides a huge space for the development of high-strength lightweight aggregate concrete. In addition to its small self-weight, high-strength lightweight aggregate concrete has significantly better thermal insulation, heat insulation, moisture retention, heat insulation, fire resistance and seismic resistance than ordinary concrete. Therefore, the use of lightweight aggregate concrete can not only save cement, steel bars and other materials, and achieve direct economic benefits, but also reduce the cost of foundation treatment, increase the use area, extend the service life of the project, and obtain significant indirect economic benefits. In addition, artificial lightweight aggregate can be fired from industrial waste such as fly ash and coal gangue, sludge, and calcined ash of domestic garbage. This is a green aggregate, which can greatly reduce the mining and utilization of natural aggregates. However, studies have found that under high load conditions, the failure of high-strength lightweight aggregate concrete presents explosive brittle failure, which poses certain safety hazards in its engineering applications.
[0003] With the vigorous development of the automobile industry, the number of waste automobile tires has increased dramatically, and the rational recycling of waste tires has become urgent. In recent years, crushing waste rubber tires and using them as coarse and fine aggregates in concrete has gradually become an important way to recycle waste tires. The volume of rubber powder is used to replace part of the sand, and the effect of the amount of rubber powder and the type of rubber powder on the compressive strength and flexural tensile strength of cement concrete is analyzed. The test results show that the amount and type of rubber powder have a significant effect on the strength of concrete, and the overall strength decreases with the increase of the amount of rubber powder. The Chinese patent "High-performance road rubber concrete and its preparation method" with publication number CN112341104A uses rubber powder obtained by tire crushing, and then uses it for high-performance concrete after modification, so that it has the characteristics of strong pressure bearing capacity, high toughness, high deformation resistance and high durability, and is used for highway pavement engineering under heavy traffic. The Chinese patent "A high-performance rubber concrete and its preparation method" with publication number CN117361977A uses sodium hydroxide to treat rubber powder. The prepared high-performance rubber concrete has the characteristics of high workability, high compressive strength and high durability, which solves the problems of low working performance and serious deterioration of compressive strength of existing rubber concrete. Although the above patents all use the rubber particles obtained by crushing waste tires in ordinary concrete to obtain high-performance rubber concrete with excellent performance. However, there is no relevant research on the application of rubber particles to lightweight aggregate concrete. In addition, the rubber concrete in the prior art still has defects such as the rubber is easy to float during the molding process and the rubber is easy to peel off under load. Summary of the invention
[0004] In order to reduce the brittleness of lightweight aggregate concrete and expand the application scenarios of rubber particles, the present invention proposes a low elastic modulus lightweight high-strength concrete and a preparation method thereof. Furthermore, the method of wrapping the rubber particles with fast-hardening sulphoaluminate cement solves the problem of weak bonding in the interface transition zone formed by rubber and cement-based materials, solves the problem of easy peeling of rubber under load, and guarantees the mechanical properties of rubber lightweight aggregate concrete to a certain extent.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A low elastic modulus, lightweight, high-strength concrete comprising the following raw materials in the following mass proportions:
[0007] Cement: 480~600kg / m 3 ;
[0008] Fly ash: 240~300kg / m 3 ;
[0009] Silica fume: 80~100kg / m 3 ;
[0010] Hollow glass microspheres: 64-80 kg / m 3 ;
[0011] Ceramic sand: 150~220kg / m 3 ;
[0012] Modified rubber particles: 120~180kg / m 3 ;
[0013] Ceramic aggregate: 225~330kg / m 3 ;
[0014] Water reducing agent: 2.4~3.0kg / m 3 ;
[0015] Defoaming agent: 1.6~2.0kg / m 3 ;
[0016] The water-to-binder ratio is 0.22-0.24, the cement, fly ash and silica fume are cementitious materials, and the water-to-binder ratio is the mass ratio of water to cementitious materials.
[0017] Furthermore, the cement is low-heat silicate cement, wherein the mineral content is: C2S: 42-46wt%, C3S: 30-40wt%, C3A: 1-3wt%, C4AF: 15-19wt%.
[0018] Furthermore, the fly ash is Class I fly ash with a specific surface area of 350m 2 / kg, median diameter 16.4um.
[0019] Furthermore, the silica fume is ultrafine silica fume with a specific surface area of 400m 2 / kg, water requirement ratio <125%, 7d activity index of silica fume ≥105%.
[0020] Furthermore, the hollow glass microspheres are in the form of white powder, with a particle size ranging from 70 to 80 μm, a moisture content of ≤0.25%, and a floating rate of ≥96%.
[0021] Furthermore, the ceramsite is self-made high-strength ceramsite with a particle size range of 4.75 to 10 mm.
[0022] Furthermore, the ceramic sand is obtained by crushing homemade ceramsite, wherein the cumulative sieve residue percentage of sand particles with a diameter of >4.75 mm is 0%, the cumulative sieve residue percentage of sand particles with a diameter of >2.36 mm is 36%, the cumulative sieve residue percentage of sand particles with a diameter of >1.18 mm is 61%, the cumulative sieve residue percentage of sand particles with a diameter of >0.60 mm is 78%, the cumulative sieve residue percentage of sand particles with a diameter of >0.30 mm is 91%, the cumulative sieve residue percentage of sand particles with a diameter of >0.15 mm is 100%, and the fineness modulus is 3.34.
[0023] Furthermore, the self-made high-strength ceramsite is made of high-titanium slag, ferrochrome slag, and microsilica powder as main raw materials, and industrial magnesium oxide and industrial aluminum oxide as auxiliary raw materials, and is fired by a high-temperature solid phase method, specifically comprising: 25wt% of high-titanium slag, 45wt% of ferrochrome slag, 10wt% of microsilica powder, 12wt% of industrial magnesium oxide, and 8.0wt% of industrial aluminum oxide;
[0024] The apparent density of the self-made high-strength ceramsite is 1450kg / m 3 , 24h water absorption ≤5.0wt%, cylinder pressure strength ≥10MPa.
[0025] Among them, the utilization rate of high-titanium slag and ferrochrome slag heavy metal industrial solid waste can reach up to 80wt%.
[0026] The mechanism of high-temperature solid-phase sintering is as follows: based on the MgO-Al2O3-SiO2-CaO system, the quaternary system phase diagram is drawn using FactSage6.0 thermodynamic simulation software, and the heavy metals of high-titanium slag and ferrochrome slag are further dissolved into the ceramsite mineral phase lattice with the help of the phase diagram; Cr 2+ and Cr 3+ The ionic radii of Mg and 2+ and Al 3+ The ionic radius is 0.072nm and 0.054nm respectively, and the ionic radius of chromium and magnesium is very close, so chromium can easily replace magnesium or aluminum and dissolve into the crystal lattice of cordierite and spinel minerals. After testing, the heavy metal element dissolution amount of the self-made high-strength ceramsite is 0.237mg / L, which is far less than the national standard.
[0027] The calculation of the FactSage 6.0 thermodynamic simulation software is based on the main mineral phases of ceramsite, magnesium aluminum spinel (MgAl2O4) and cordierite (Mg2Al4Si5O 18 ) as the benchmark, the content range of Al2O3, SiO2 and CaO was calculated by fixing the MgO content. After calculation, the content range of each oxide is: MgO (7.96-19.32wt%), Al2O3 (20.08-43.50wt%), SiO2 (44.54-71.96wt%), CaO (0-7.5wt%).
[0028] The ratio of main raw materials to auxiliary raw materials is determined by calculating the content variation range of each oxide in the MgO-Al2O3-SiO2-CaO system according to the thermodynamic software, including: 25wt% high-titanium slag, 45wt% ferrochrome slag, 10wt% silicon powder, 12wt% industrial magnesium oxide, and 8.0wt% industrial aluminum oxide.
[0029] Furthermore, the high-titanium slag is water-quenched slag, in which the content of magnesium-aluminum-silicon oxide is more than 40wt%, the content of calcium-titanium oxide is 50wt%, and the content of Fe2O3 is 6wt%; preferably, the high-titanium slag is water-quenched slag from Sichuan Wei Iron and Steel Group.
[0030] Furthermore, the ferrochrome slag contains magnesium, aluminum and silicon oxides at a content of more than 85 wt%, Fe2O3 at a content of 6 wt% and Cr2O3 at a content of 8 wt%.
[0031] Furthermore, the silicon oxide content in the silicon micropowder is ≥95wt%, the Al2O3 content in the industrial alumina is ≥98wt%, and the MgO content in the industrial magnesium oxide is ≥99wt%.
[0032] Furthermore, the particle size of the modified rubber particles is 2.36-4.76 mm, and the apparent density is 1316 kg / m 3 , bulk density is 636kg / m 3 .
[0033] Furthermore, the modification method of the modified rubber particles is as follows: SA, sodium hypochlorite, concentrated hydrochloric acid and deionized water are prepared into a mixed solution at a volume ratio of V(NaClO):V(HCl):V(H2O)=4:1:100, and then rubber particles are added to the mixed solution, the volume ratio of the mixed solution to the rubber particles is 2:1, and then placed in a 25°C constant temperature water tank for a water bath for 10 minutes, and then filtered, washed with deionized water for multiple times until the pH of the washing water is neutral, and then filtered, and dried in an oven at 80°C for 12 hours to complete the surface oxidation of the rubber particles; SB, the surface-oxidized rubber particles are added with water glass and mixed, and after mixing evenly, sulphoaluminate cement is added, and stirring is continued until each rubber particle is coated with a layer of sulphoaluminate cement, and finally dried in an oven at 40°C to obtain the modified rubber particles.
[0034] The purpose of the SA is to oxidize the surface of the rubber particles so as to increase the number of surface polar functional groups, increase the roughness, and improve the wettability.
[0035] Furthermore, the mass ratio of the surface-oxidized rubber particles to water glass and sulphoaluminate cement is 1:0.1:0.2.
[0036] Furthermore, the water glass is a Na2SiO3 aqueous solution with a modulus of 3.1.
[0037] Since the main component of water glass is sodium silicate, it has two main functions: on the one hand, as a binder, water glass can effectively bond rubber particles with sulphoaluminate cement, making it difficult for rubber and cement to fall off; on the other hand, sodium silicate is a soluble inorganic silicate, which can react with calcium hydroxide produced during cement hydration to form calcium silicate gel, which can fill the capillary pores between rubber particles and cement matrix, increase the interfacial bonding strength between rubber and cement matrix, and reduce the impact of rubber particles on concrete strength. In addition, sodium silicate can also improve the impermeability and corrosion resistance of concrete and enhance the durability of concrete.
[0038] Furthermore, the water reducer is polycarboxylate water reducer 540P; preferably, the water reducer is Sika 540P polycarboxylate high-performance water reducer, which is a white powder with high water reduction rate and high plasticity.
[0039] Furthermore, the defoamer is a polyether powder defoamer, and preferably, the defoamer is Degussa polyether powder defoamer.
[0040] The present invention also provides a method for preparing low elastic modulus lightweight high-strength concrete, comprising the following steps:
[0041] S1. Weigh the raw materials of each mass, stir cement, fly ash, silica fume, hollow glass microspheres and ceramic sand for 60 seconds, preferably in a forced concrete mixer, and then add water, water reducer and defoamer in sequence and continue stirring for 2 minutes, finally add modified rubber particles and ceramsite, continue stirring, and perform molding and curing to obtain the low elastic modulus lightweight high-strength concrete.
[0042] Furthermore, the low elastic modulus lightweight high strength concrete has the following indicators: concrete bulk density ≤ 1750kg / m 3 , slump ≥ 200mm, expansion ≥ 380mm, 28d compressive strength ≥ 45MPa, elastic modulus ≤ 25GPa, the elastic modulus value is the secant modulus value under 30% axial compressive strength stress.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] (1) In the present invention, the rubber particles have the characteristics of low density and low elastic modulus. Applying them to lightweight high-strength concrete will not only not increase the bulk density of the concrete, but also reduce the stress concentration of the concrete under load because the rubber has a good energy absorption effect, thereby improving the impact resistance of the lightweight high-strength concrete and reducing the brittleness of the concrete.
[0045] (2) The present invention applies the rubber particles obtained from the crushing of waste tires to lightweight high-strength concrete, which provides a new idea for the resource recycling of waste tires. In addition, the rubber particles in concrete can be regarded as "elastomers" due to their good elasticity, which can absorb strain energy and limit the occurrence and expansion of cracks, thereby improving the frost resistance of lightweight high-strength concrete.
[0046] (3) The present invention uses sodium hypochlorite to oxidize the surface of rubber particles to increase the hydrophilicity and surface roughness of the rubber particles. Water glass is further used as a binder to wrap the rubber particles with a layer of sulphoaluminate cement with rapid hydration. The continuous hydration of the sulphoaluminate cement further strengthens the interfacial bonding strength between the rubber particles and the cement matrix, improves the interfacial properties of the two, alleviates the possibility of damage caused by inconsistent deformation of the rubber particles and the cement matrix under load to a certain extent, and improves the bearing capacity of the concrete.
[0047] (4) The present invention uses industrial solid wastes containing heavy metals such as high-titanium slag and ferrochrome slag to replace natural silicon-aluminum raw materials such as clay to produce high-strength expanded clay and ceramic sand, which not only reduces the pollution of heavy metal industrial solid waste to the natural ecological environment, but also alleviates the excessive consumption of natural silicon-aluminum raw materials such as clay, which is in line with the current low-carbon and environmentally friendly production concept. DETAILED DESCRIPTION
[0048] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0049] Example 1
[0050] As a preferred embodiment of the present invention, a low elastic modulus lightweight high strength concrete of this embodiment has a composition as shown in Table 1.
[0051] Table 1
[0052] raw material <![CDATA[Mass / kg / m 3 > Low heat silicate cement 480 Fly ash 240 Silica Fume 80 Hollow glass microspheres 64 Pottery Sand 220 Modified rubber particles 120 Clay 330 Water reducing agent 2.4 Defoaming agent 1.6
[0053] In this embodiment, the water-to-binder ratio is 0.22.
[0054] Example 2
[0055] As a preferred embodiment of the present invention, a low elastic modulus lightweight high strength concrete of this embodiment has a composition as shown in Table 2.
[0056] Table 2
[0057] raw material <![CDATA[Mass / kg / m 3 > Low heat silicate cement 540 Fly ash 270 Silica Fume 90 Hollow glass microspheres 72 Pottery Sand 185 Modified rubber particles 150 Clay 277.5 Water reducing agent 2.7 Defoaming agent 1.8
[0058] In this embodiment, the water-to-binder ratio is 0.23.
[0059] Example 3
[0060] As a preferred embodiment of the present invention, a low elastic modulus lightweight high strength concrete of this embodiment has a composition as shown in Table 3.
[0061] Table 3
[0062] raw material <![CDATA[Mass / kg / m 3 > Low heat silicate cement 600 Fly ash 300 Silica Fume 100 Hollow glass microspheres 80 Pottery Sand 150 Modified rubber particles 180 Clay 225 Water reducing agent 3.0 Defoaming agent 2.0
[0063] In this embodiment, the water-to-binder ratio is 0.24.
[0064] Comparative Example 1
[0065] The lightweight high-strength concrete of this comparative example is the same as that of Example 1 except that no modified rubber particles are added.
[0066] Comparative Example 2
[0067] The lightweight high-strength concrete of this comparative example is the same as that of Example 1 except that the modified rubber particles are replaced with ordinary rubber particles.
[0068] The concrete of each embodiment and comparative example was tested, and the test results are shown in Table 4.
[0069] Table 4
[0070]
[0071] As shown in Table 1, compared with Example 1 to Example 3, as the amount of rubber particles in the composition increases, the elastic modulus of concrete gradually decreases and the toughness increases, but correspondingly, the compressive strength of concrete also tends to decrease, but the overall concrete strength performance is good and the working performance is also good; compared with Example 1 and Comparative Example 1, it can be seen that rubber particles can significantly reduce the elastic modulus of concrete and improve the toughness of concrete. Compared with the concrete without rubber particles, the elastic modulus of low elastic modulus, lightweight and high strength concrete decreases by about 29.6%; compared with Example 1, Comparative Example 1 and Comparative Example 2, it can be seen that after the rubber particles are oxidized with sodium hypochlorite, water glass is used as a binder to wrap the sulphoaluminate cement on the surface of the rubber particles, which can alleviate the disadvantage of the rubber particles causing the concrete strength to decrease, and the rubber particle concrete wrapped with sulphoaluminate cement has higher strength, lower elastic modulus and better working performance, so the concrete prepared by the invention has the characteristics of low elastic modulus, light weight and high strength.
[0072] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.
Claims
1. A low elastic modulus lightweight high strength concrete, characterized in that: Including the following raw materials in mass ratio: Cement: 480~600kg / m 3 ; Fly ash: 240~300kg / m 3 ; Silica fume: 80~100kg / m 3 ; Hollow glass microspheres: 64-80 kg / m 3 ; Ceramic sand: 150~220kg / m 3 ; Modified rubber particles: 120~180kg / m 3 ; Ceramic aggregate: 225~330kg / m 3 ; Water reducing agent: 2.4~3.0kg / m 3 ; Defoaming agent: 1.6~2.0kg / m 3 ; The water-to-binder ratio is 0.22-0.24, the cement, fly ash and silica fume are cementitious materials, and the water-to-binder ratio is the mass ratio of water to cementitious materials.
2. The low elastic modulus lightweight high strength concrete according to claim 1, characterized in that: The cement is low-heat silicate cement, wherein the mineral contents are: C2S: 42-46 wt%, C3S: 30-40 wt%, C3A: 1-3 wt%, C4AF: 15-19 wt%.
3. The low elastic modulus lightweight high strength concrete according to claim 1, characterized in that: The fly ash is Grade I fly ash with a specific surface area of 350m 2 / kg, median diameter 16.4um; the silica fume is ultrafine silica fume, with a specific surface area of 400m 2 / kg, water requirement ratio <125%, 7d activity index of silica fume ≥105%; the hollow glass microspheres are white powder, with a particle size range of 70-80μm, a moisture content ≤0.25%, and a floating rate ≥96%.
4. The low elastic modulus lightweight high strength concrete according to claim 1, characterized in that: The ceramsite is homemade high-strength ceramsite with a particle size range of 4.75 to 10 mm; the ceramic sand is obtained by crushing homemade ceramsite, wherein the cumulative sieve residue percentage of sand particles with a diameter of >4.75 mm is 0%, the cumulative sieve residue percentage of sand particles with a diameter of >2.36 mm is 36%, the cumulative sieve residue percentage of sand particles with a diameter of >1.18 mm is 61%, the cumulative sieve residue percentage of sand particles with a diameter of >0.60 mm is 78%, the cumulative sieve residue percentage of sand particles with a diameter of >0.30 mm is 91%, the cumulative sieve residue percentage of sand particles with a diameter of >0.15 mm is 100%, and the fineness modulus is 3.
34.
5. The low elastic modulus lightweight high strength concrete according to claim 4, characterized in that: The self-made high-strength ceramsite is made of high-titanium slag, ferrochrome slag, and microsilica powder as main raw materials, and industrial magnesium oxide and industrial aluminum oxide as auxiliary raw materials, and is fired by a high-temperature solid phase method, specifically comprising: 25wt% of high-titanium slag, 45wt% of ferrochrome slag, 10wt% of microsilica powder, 12wt% of industrial magnesium oxide, and 8.0wt% of industrial aluminum oxide; The apparent density of the self-made high-strength ceramsite is 1450kg / m 3 , 24h water absorption ≤5.0wt%, cylinder pressure strength ≥10MPa.
6. The low elastic modulus lightweight high strength concrete according to claim 5, characterized in that: The high-titanium slag is water-quenched slag, in which the content of magnesium, aluminum and silicon oxides is more than 40wt%, the content of calcium titanium oxide is 50wt%, and the content of Fe2O3 is 6wt%; the content of magnesium, aluminum and silicon oxides in the ferrochrome slag is more than 85wt%, the content of Fe2O3 is 6wt%, and the content of Cr2O3 is 8wt%; the silicon oxide content in the silicon micropowder is ≥95wt%, the content of Al2O3 in the industrial alumina is ≥98wt%, and the content of MgO in the industrial magnesium oxide is ≥99wt%.
7. The low elastic modulus lightweight high strength concrete according to claim 1, characterized in that: The particle size of the modified rubber particles is 2.36-4.76 mm, and the apparent density is 1316 kg / m 3 , bulk density is 636kg / m 3 .
8. The low elastic modulus lightweight high strength concrete according to claim 1, characterized in that: The modification method of the modified rubber particles is as follows: SA, sodium hypochlorite, concentrated hydrochloric acid and deionized water are prepared into a mixed solution at a volume ratio of V(NaClO):V(HCl):V(H2O)=4:1:100, and then rubber particles are added to the mixed solution, the volume ratio of the mixed solution to the rubber particles is 2:1, and then the mixed solution is placed in a 25°C constant temperature water tank for a water bath for 10 minutes, and then filtered, washed with deionized water for multiple times until the pH of the washing water is neutral, and then filtered, and dried in an oven at 80°C for 12 hours to complete the surface oxidation of the rubber particles; SB, the surface-oxidized rubber particles are added with water glass and mixed, and after mixing evenly, sulphoaluminate cement is added, and stirring is continued until each rubber particle is coated with a layer of sulphoaluminate cement, and finally dried in an oven at 40°C to obtain the modified rubber particles; Preferably, the mass ratio of the surface-oxidized rubber particles to water glass and sulphoaluminate cement is 1:0.1:0.2; the water glass is a Na2SiO3 aqueous solution with a modulus of 3.
1.
9. The low elastic modulus lightweight high strength concrete according to claim 1, characterized in that: The water reducer is polycarboxylate water reducer 540P; the defoamer is a polyether powder defoamer.
10. A method for preparing low elastic modulus lightweight high strength concrete according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Weigh the raw materials of each mass, stir cement, fly ash, silica fume, hollow glass microspheres and pottery sand for 60 seconds, then add water, water reducer and defoamer in sequence and continue stirring for 2 minutes, finally add modified rubber particles and ceramsite, continue stirring, and perform molding and curing to obtain the low elastic modulus lightweight high-strength concrete; The low elastic modulus lightweight high strength concrete has the following indicators: concrete bulk density ≤ 1750kg / m 3 , slump ≥ 200mm, expansion ≥ 380mm, 28d compressive strength ≥ 45MPa, elastic modulus ≤ 25GPa, the elastic modulus value is the secant modulus value under 30% axial compressive strength stress.
Citation Information
Patent Citations
High-strength thermal-insulation concrete and preparation method thereof
CN110194624A
Modified rubber particle lightweight ultra-high performance concrete and preparation method thereof
CN111170697A
Modified waste and old rubber, preparation method thereof and sound insulation mortar