Building concrete based on Portland cement and manufacturing process thereof
By using functional fibers and composite additives in concrete, the problem of insufficient crack resistance and compressive strength is solved, the microstructure and water retention properties of concrete are improved, and its compressive strength and crack resistance are significantly improved, which delays water The chemical process ensures the long-term stability of concrete.
Patent Information
- Application Number
- CN202411206393.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The problems of existing concrete crack resistance, compressive strength and rapid surface loss in the early plastic stages lead to reduced structural durability and frequent deformation and cracking.
Using a building concrete formula based on silicate cement, functional fibers and composite additives were added, and sulfonic acid groups and amide groups were introduced into sepiolite fibers through chemical grafting. The modified fibers and composite additives were used to improve the Crack resistance and hydration prevention rate enhance the microstructure and water retention properties of concrete.
It significantly improves the compressive strength and crack resistance of concrete, delays the hydration process, reduces cracks and deformation caused by shrinkage, and ensures the long-term stability and performance maintenance of concrete.
Smart Images

Figure CN119038928A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a building concrete based on Portland cement and a manufacturing process thereof. Background Art
[0002] Concrete refers to a building material made by mixing cement as a binder with water, sand, gravel, and, when necessary, chemical admixtures and mineral admixtures in appropriate proportions, and then evenly stirring, compacting, and curing and hardening. It is one of the most important building materials in contemporary times and has a wide range of uses. It can be used to build houses, roads, bridges and other building structures. Among them, Portland cement is one of the most widely used binders in concrete and has good mechanical properties and durability.
[0003] With the acceleration of urbanization and the continuous development of infrastructure construction, the demand for concrete has gradually increased. However, due to the diversity of building types and the complexity of construction conditions, the functional requirements for concrete are also getting higher and higher. In a large number of existing cement concrete engineering structures, concrete cracking is very common, and cracks are channels for moisture, chemicals, etc. to enter the interior of the concrete. Once cracks are formed, these substances will accelerate the corrosion and deterioration of the concrete, thereby reducing the durability of the structure. Secondly, as the main material in building structures, concrete needs to withstand various external loads, such as gravity loads, wind loads, earthquake loads, etc., and compressive strength is an important indicator to measure the ability of concrete to resist these loads. In addition, rapid water loss on the surface of concrete in the early plastic stage will lead to the generation of plastic cracks. Therefore, building concrete needs to have good crack resistance, compressive strength and water retention properties to ensure that the performance can be maintained stable during long-term use and avoid deformation, cracking and other problems.
[0004] In the prior art, a common method for improving the functionality of concrete is to add various functional fillers and additives to give concrete a variety of special properties. For example, the invention patent with publication number CN113105193B discloses an anti-cracking concrete and its production process. The invention adds cellulose ether, calcium chloride, calcium acetate, and barium zirconate to the concrete formula and heats it to make the connection between the cement colloid and the aggregate stronger and not easy to be separated from the aggregate, so that the prepared concrete has good anti-cracking performance. Summary of the invention
[0005] The object of the present invention is to provide a building concrete based on silicate cement and a manufacturing process thereof, which solves the following technical problems:
[0006] (1) Solved the problem of poor crack resistance of conventional concrete;
[0007] (2) It solves the problem of poor compressive strength of conventional concrete;
[0008] (3) It solves the problem of rapid surface water loss of conventional concrete in the early plastic stage.
[0009] The purpose of the present invention can be achieved through the following technical solutions:
[0010] A building concrete based on silicate cement comprises the following raw materials in parts by weight: 80-120 parts of sand, 200-260 parts of crushed stone, 20-40 parts of fly ash, 100-140 parts of ordinary silicate cement, 8-12 parts of functionalized fiber, 6-8 parts of composite additives and 100-120 parts of water.
[0011] Through the above technical scheme, sand is used as fine aggregate, which is mixed with slurry and filled in the gaps between coarse aggregates, which helps to improve the overall density and strength of concrete; the addition of crushed stone can improve the compressive strength and tensile strength of concrete, and ensure the durability and stability of the concrete structure; the addition of fly ash can effectively improve the workability of concrete, and its small particle size can fill the gaps between cement particles and improve the density of concrete; the addition of ordinary Portland cement can improve the mechanical properties and durability of concrete.
[0012] Furthermore, the method for preparing the functionalized fiber comprises the following steps:
[0013] S1: adding sepiolite fiber into hydrochloric acid solution, treating at 75-85° C. for 10-15 h, filtering, washing and drying to obtain pretreated sepiolite fiber;
[0014] S2: adding the pretreated sepiolite fiber and N,N-dimethylformamide to a nitrogen-protected reactor, ultrasonically dispersing for 20 to 40 minutes, and continuing to add maleic anhydride and p-toluenesulfonic acid to the reactor. After the addition is completed, the temperature is raised to 60 to 80°C, and after stirring for 2 to 4 hours, the heating is stopped and the nitrogen is removed. The material is cooled naturally, filtered, washed, and vacuum dried to obtain the modified sepiolite fiber;
[0015] S3: Add modified sepiolite fiber and 2-aminoethanesulfonic acid to the dimethyl sulfoxide solution, and perform ultrasonic treatment to form a uniform dispersion. Under nitrogen protection, add the accelerator and dehydrating agent to the dispersion. After the addition, stir at room temperature for 4 to 8 hours, filter and separate the solid material, and obtain the functionalized fiber after washing and drying.
[0016] Furthermore, in step S1, the average diameter of the sepiolite fibers is 2 μm, and the average length is 4 mm.
[0017] Furthermore, in step S1, the mass fraction of the hydrochloric acid solution is 2% to 4%.
[0018] Furthermore, in step S3, the accelerator is any one of 4-dimethylaminopyridine, 1-hydroxybenzotriazole or N-hydroxysuccinimide; the dehydrating agent is any one of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, N,N'-diisopropylcarbodiimide or dicyclohexylcarbodiimide.
[0019] Furthermore, the preparation method of the composite additive comprises the following steps:
[0020] SS1: Mix polymalic acid and N-methylpyrrolidone, stir evenly, add epoxidized soybean oil and catalyst, turn on heating, wait until the system temperature reaches 60-80°C, stir at constant temperature for 4-6 hours, cool down and discharge, and you can get the intermediate material;
[0021] SS2: Add the intermediate material and dimethyl sulfoxide into the reactor, stir mechanically to make it uniform, add 2,3-epoxypropyltrimethylammonium chloride and boron trifluoride etherate, raise the temperature to 75-85°C, keep stirring at this temperature for 4-8 hours, remove the solvent by vacuum distillation to obtain the composite additive.
[0022] Furthermore, in step SS1, the number average molecular weight of the polymalic acid is 1000-2000.
[0023] Furthermore, in step SS1, the catalyst is any one of tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate or tetramethylammonium bromide.
[0024] Furthermore, in step SS2, the mass ratio of the intermediate material to 2,3-epoxypropyltrimethylammonium chloride is 1:0.1-0.4.
[0025] A process for manufacturing building concrete based on Portland cement comprises the following steps:
[0026] (1) adding sand, crushed stone, fly ash, ordinary Portland cement and functionalized fiber into a mixer, setting the speed of the mixer to 500-700 r / min, stirring for 20-40 min to obtain a blend;
[0027] (2) adding the composite additive and water to the blend prepared in step (1), and continuing stirring for 10 to 30 minutes to obtain a concrete slurry;
[0028] (3) The concrete slurry prepared in step (2) is sequentially subjected to pouring treatment, vibrating treatment, leveling treatment and curing treatment to obtain architectural concrete.
[0029] Beneficial effects of the present invention:
[0030] (1) The present invention utilizes a chemical grafting method to introduce sulfonic acid groups and amide groups into sepiolite fibers to obtain functionalized fibers, wherein the sulfonic acid groups and amide groups can react with calcium hydroxide in the slurry to promote the hydration of tricalcium aluminate, a mineral component in the slurry, so that calcium aluminate is generated faster, thereby improving the early strength of the concrete. At the same time, cement particles can be loaded on the surface of the sepiolite fibers to promote the uniform distribution of the sepiolite fibers in the slurry. By utilizing the excellent properties of the sepiolite fibers, the microstructure of the concrete can be improved and the compressive strength of the concrete can be improved. When tiny cracks appear inside the concrete, the sepiolite fibers can play a "bridging role" in the concrete, filling the cracks and forming bridges, which can effectively prevent the generation and development of cracks, thereby improving the crack resistance of the concrete. In addition, the hydrophilic sulfonic acid groups can absorb a large amount of water, thereby enhancing the water retention performance of the concrete and avoiding the problem of too fast hydration rate of the slurry causing cracks in the concrete.
[0031] (2) The present invention prepares a composite additive as a filling modifier for concrete. Since the composite additive has a hyperbranched structure, it can extend into the gaps in cement, provide more contact points for the attachment of cement particles, and is not prone to shrinkage, which helps to evenly distribute cement particles in the solution and balance internal stress, thereby enhancing the anti-cracking performance of concrete. The polymalic acid in the composite additive can improve the water retention performance of concrete. In the mortar hydration stage, the polymalic acid can absorb and store a large amount of water. In the mortar hardening stage, the water absorbed by the polymalic acid is gradually released and produces a continuous hydration effect, reducing the volume shrinkage caused by cement hardening and preventing cracks and deformation caused by shrinkage. At the same time, the epoxy soybean oil in the composite additive has good fluidity, can better fill the gaps, and reduce the formation of voids and defects. In addition, the quaternary ammonium salt cations in the composite additive can react with components such as silicates in concrete, thereby improving the thixotropy of concrete, further increasing fluidity, and enhancing the mud resistance of concrete.
[0032] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0034] Figure 1 This is an infrared spectrum test chart of the functionalized fiber prepared in Example 1 of the present invention.
[0035] Figure 2 This is an infrared spectrum test chart of the intermediate material and composite additive prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] 1. Preparation of functionalized fibers
[0039] S1: adding 10 g of sepiolite fibers with an average diameter of 2 μm and an average length of 4 mm into a 3% hydrochloric acid solution, treating at 80° C. for 12 h, filtering, washing, and drying to obtain pretreated sepiolite fibers;
[0040] S2: 5 g of pretreated sepiolite fiber and N,N-dimethylformamide were added to a nitrogen-protected reactor, and ultrasonic dispersion was performed for 30 min. 1.2 g of maleic anhydride and 0.05 g of p-toluenesulfonic acid were added to the reactor. After the addition was completed, the temperature was raised to 70°C, and after stirring for 3 h, the heating was stopped and the nitrogen was removed. The material was cooled naturally, filtered, washed, and vacuum dried to obtain modified sepiolite fiber.
[0041] S3: Add 5 g of modified sepiolite fiber and 1.5 g of 2-aminoethanesulfonic acid to the dimethyl sulfoxide solution, and perform ultrasonic treatment to form a uniform dispersion. Under nitrogen protection, add 0.08 g of 4-dimethylaminopyridine and 0.1 g of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide to the dispersion. After the addition, stir at room temperature for 6 h, filter and separate the solid material, and obtain the functionalized fiber after washing and drying.
[0042] Through the above technical scheme, the anhydride groups in the maleic anhydride structure are highly active. Under the action of p-toluenesulfonic acid, they can undergo a ring-opening esterification reaction with the hydroxyl groups on the surface of the sepiolite fiber, thereby introducing carboxyl groups on the surface of the sepiolite fiber to obtain modified sepiolite fibers. The carboxyl groups on the surface of the fibers are used as active sites. Under the action of a dehydrating agent, 2-aminoethanesulfonic acid is introduced into the surface of the sepiolite fiber by utilizing the mechanism that the carboxyl groups can react with the amino groups in the 2-aminoethanesulfonic acid structure, thereby obtaining functionalized fibers.
[0043] The functionalized fibers were analyzed by infrared spectroscopy using a Nicolet 380 FT-IR Fourier transform infrared spectrometer. Figure 1 As shown by Figure 1 It can be seen that in the infrared spectrum of functionalized fibers, 1731 cm -1 The absorption peak of the ester group C=O appears at 3440 cm -1 The absorption peak of NH in amide appears at 1665 cm -1 The absorption peak of C=O in amide appears at 1238 cm -1 and 1092cm -1 The absorption peak of sulfonic acid group appears at
[0044] 2. Preparation of composite additives
[0045] SS1: Mix 6 g of polymalic acid with a number average molecular weight of 2000 with N-methylpyrrolidone, stir evenly, then add 2.6 g of epoxidized soybean oil and 0.1 g of tetrabutylammonium bromide. After the addition is complete, turn on the heating. After the system temperature reaches 70°C, stir at a constant temperature for 5 hours, cool down and discharge the material to obtain the intermediate material.
[0046] SS2: Add 6 g of the intermediate material and dimethyl sulfoxide into the reactor, stir mechanically to make it uniform, add 1.8 g of 2,3-epoxypropyltrimethylammonium chloride and 0.08 g of boron trifluoride etherate, raise the temperature to 80°C, keep stirring at this temperature for 6 hours, and then remove the solvent by vacuum distillation to obtain a composite additive.
[0047] Through the above technical scheme, the carboxyl groups in the polymalic acid structure can undergo a ring-opening reaction with the epoxy groups in the epoxy soybean oil structure under the action of a catalyst to obtain an intermediate material. At the same time, the hydroxyl groups in its structure produced by the ring-opening reaction can react with the epoxy groups in the 2,3-epoxypropyltrimethylammonium chloride structure under the action of tetrabutylammonium bromide to obtain a composite additive.
[0048] The intermediate material and compound additives were analyzed by infrared spectroscopy using Nicolet 380FT-IR Fourier transform infrared spectrometer. Figure 2 As shown by Figure 2 It can be seen that in the infrared spectrum of the intermediate material, 1759cm -1 The absorption peak of the ester group C=O appears at 3270 cm -1 The absorption peak of the hydroxyl group OH appears at 3279cm -1 The absorption peak of hydroxyl group OH appears at 1020cm -1 The absorption peak of ether bond COC appears at 1410 cm -1 The absorption peak of CN in the quaternary ammonium salt appears at
[0049] 3. Preparation of architectural concrete
[0050] (1) 80 g of sand, 200 g of crushed stone, 20 g of fly ash, 100 g of ordinary Portland cement and 8 g of functionalized fiber were added into a mixer, the speed of the mixer was set to 500 r / min, and stirred for 20 min to obtain a blend;
[0051] (2) adding 6 g of the composite additive and 100 g of water to the blend prepared in step (1), and continuing stirring for 10 min to obtain a concrete slurry;
[0052] (3) The concrete slurry prepared in step (2) is sequentially subjected to pouring treatment, vibrating treatment, leveling treatment and curing treatment to obtain architectural concrete.
[0053] Example 2
[0054] Preparation of architectural concrete
[0055] (1) 100 g of sand, 230 g of crushed stone, 30 g of fly ash, 120 g of ordinary Portland cement and 10 g of functionalized fiber were added to a mixer, the speed of the mixer was set to 600 r / min, and stirred for 30 min to obtain a blend;
[0056] (2) adding 7 g of the composite additive and 110 g of water to the blend prepared in step (1), and continuing stirring for 20 min to obtain a concrete slurry;
[0057] (3) The concrete slurry prepared in step (2) is sequentially subjected to pouring treatment, vibrating treatment, leveling treatment and curing treatment to obtain architectural concrete.
[0058] The preparation method of the functionalized fiber and the composite additive is the same as that in Example 1.
[0059] Example 3
[0060] Preparation of architectural concrete
[0061] (1) 120 g of sand, 260 g of crushed stone, 40 g of fly ash, 140 g of ordinary Portland cement and 12 g of functionalized fiber were added to a mixer, the mixer speed was set to 700 r / min, and stirred for 40 min to obtain a blend;
[0062] (2) adding 8 g of the composite additive and 120 g of water to the blend prepared in step (1), and continuing stirring for 30 min to obtain a concrete slurry;
[0063] (3) The concrete slurry prepared in step (2) is sequentially subjected to pouring treatment, vibrating treatment, leveling treatment and curing treatment to obtain architectural concrete.
[0064] The preparation method of the functionalized fiber and the composite additive is the same as that in Example 1.
[0065] Comparative Example 1
[0066] Preparation of architectural concrete
[0067] (1) 100 g of sand, 230 g of crushed stone, 30 g of fly ash, 120 g of ordinary Portland cement and 10 g of functionalized fiber were added to a mixer, the speed of the mixer was set to 600 r / min, and stirred for 30 min to obtain a blend;
[0068] (2) adding 110 g of water to the blend prepared in step (1), and continuing stirring for 20 min to obtain concrete slurry;
[0069] (3) The concrete slurry prepared in step (2) is sequentially subjected to pouring treatment, vibrating treatment, leveling treatment and curing treatment to obtain architectural concrete.
[0070] The preparation method of the functionalized fiber is the same as that in Example 1.
[0071] Comparative Example 2
[0072] Preparation of architectural concrete
[0073] (1) Add 100 g of sand, 230 g of crushed stone, 30 g of fly ash, and 120 g of ordinary Portland cement into a mixer, set the mixer speed to 600 r / min, and stir for 30 min to obtain a blend;
[0074] (2) adding 7 g of the composite additive and 110 g of water to the blend prepared in step (1), and continuing stirring for 20 min to obtain a concrete slurry;
[0075] (3) The concrete slurry prepared in step (2) is sequentially subjected to pouring treatment, vibrating treatment, leveling treatment and curing treatment to obtain architectural concrete.
[0076] The preparation method of the composite additive is the same as that in Example 1.
[0077] Comparative Example 3
[0078] Preparation of architectural concrete
[0079] (1) Add 100 g of sand, 230 g of crushed stone, 30 g of fly ash, and 120 g of ordinary Portland cement into a mixer, set the mixer speed to 600 r / min, and stir for 30 min to obtain a blend;
[0080] (2) adding 110 g of water to the blend prepared in step (1), and continuing stirring for 20 min to obtain concrete slurry;
[0081] (3) The concrete slurry prepared in step (2) is sequentially subjected to pouring treatment, vibrating treatment, leveling treatment and curing treatment to obtain architectural concrete.
[0082] Performance Testing
[0083] ① According to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the compressive strength of the building concrete prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 3 was tested at 7d, 28d and 56d of curing. The specific test results are shown in the following table:
[0084]
[0085] From the test results in the above table, it can be seen that the construction concrete prepared in Examples 1 to 3 all have good early strength performance and later compressive strength; the construction concrete prepared in Comparative Example 1 added functionalized fibers, and the compressive strength of the concrete reached 13.7 MPa on the first day, and the compressive strength of the concrete reached 76.6 MPa on the 28th day, and the prepared construction concrete had good early strength performance and later compressive strength; the construction concrete prepared in Comparative Example 2 added composite additives but no functionalized fibers, and compared with the examples, the early strength performance and later compressive strength of the concrete were poor; in the construction concrete prepared in Comparative Example 3, neither functionalized fibers nor composite additives were added, so the early strength performance and later compressive strength performance of the concrete were the worst.
[0086] ② According to JGJ / T 70-2009 "Standard for Test Methods for Basic Properties of Building Mortar", the water retention rate of the building concrete prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 3 was tested; according to JC / T 951-2005 "Test Method for Cement Mortar Cracking Resistance", the cracking index of the building concrete prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 3 was tested; according to GB / T 8077-2012 "Test Method for Homogeneity of Concrete Admixtures", the fluidity of the building concrete prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 3 was tested, using a cement-clay slurry system with a mass ratio of 1:1, and the initial fluidity and fluidity after 1 hour of the slurry were tested. The specific test results are shown in the following table:
[0087]
[0088] From the test results in the above table, it can be seen that the construction concrete prepared in Examples 1 to 3 all have excellent anti-cracking performance, water retention performance, fluidity and mud resistance; the construction concrete prepared in Comparative Example 1 only added functionalized fibers. Compared with the examples, the cracking index of the concrete is smaller, the water retention rate decreases more, the initial fluidity and the fluidity after 1 hour change greatly, the anti-cracking performance of the concrete is good, the water retention performance is average, and the fluidity and mud resistance performance are poor; the construction concrete prepared in Comparative Example 2 did not add functionalized fibers, but only used composite additives for filling and modification. The initial fluidity and fluidity after 1 hour of the concrete changed little, therefore, the fluidity and mud resistance performance were good, but the water retention and anti-cracking performance were average; the construction concrete prepared in Comparative Example 3 was not modified by adding a modifier, so the performance of various indicators was extremely poor.
[0089] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A building concrete based on Portland cement, characterized in that: The invention comprises the following raw materials in parts by weight: 80-120 parts of sand, 200-260 parts of crushed stone, 20-40 parts of fly ash, 100-140 parts of ordinary Portland cement, 8-12 parts of functionalized fiber, 6-8 parts of composite additives and 100-120 parts of water.
2. A Portland cement-based building concrete according to claim 1, characterized in that: The method for preparing the functionalized fiber comprises the following steps: S1: adding sepiolite fiber into hydrochloric acid solution, treating at 75-85° C. for 10-15 h, filtering, washing and drying to obtain pretreated sepiolite fiber; S2: adding the pretreated sepiolite fiber and N,N-dimethylformamide to a nitrogen-protected reactor, ultrasonically dispersing for 20 to 40 minutes, and continuing to add maleic anhydride and p-toluenesulfonic acid to the reactor. After the addition is completed, the temperature is raised to 60 to 80°C, and after stirring for 2 to 4 hours, the heating is stopped and the nitrogen is removed. The material is cooled naturally, filtered, washed, and vacuum dried to obtain the modified sepiolite fiber; S3: Add modified sepiolite fiber and 2-aminoethanesulfonic acid to the dimethyl sulfoxide solution, and perform ultrasonic treatment to form a uniform dispersion. Under nitrogen protection, add the accelerator and dehydrating agent to the dispersion. After the addition, stir at room temperature for 4 to 8 hours, filter and separate the solid material, and obtain the functionalized fiber after washing and drying.
3. A Portland cement-based building concrete according to claim 2, characterized in that: In step S1, the average diameter of the sepiolite fibers is 2 μm, and the average length is 4 mm.
4. A Portland cement-based building concrete according to claim 2, characterized in that: In step S1, the mass fraction of the hydrochloric acid solution is 2% to 4%.
5. A Portland cement-based building concrete according to claim 2, characterized in that: In step S3, the accelerator is any one of 4-dimethylaminopyridine, 1-hydroxybenzotriazole or N-hydroxysuccinimide; the dehydrating agent is any one of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, N,N'-diisopropylcarbodiimide or dicyclohexylcarbodiimide.
6. A Portland cement-based building concrete according to claim 1, characterized in that: The preparation method of the composite additive comprises the following steps: SS1: Mix polymalic acid and N-methylpyrrolidone, stir evenly, add epoxidized soybean oil and catalyst, turn on heating, wait until the system temperature reaches 60-80°C, stir at constant temperature for 4-6 hours, cool down and discharge, and you can get the intermediate material; SS2: Add the intermediate material and dimethyl sulfoxide into the reactor, stir mechanically to make it uniform, add 2,3-epoxypropyltrimethylammonium chloride and boron trifluoride etherate, raise the temperature to 75-85°C, keep stirring at this temperature for 4-8 hours, remove the solvent by vacuum distillation to obtain the composite additive.
7. A Portland cement-based building concrete according to claim 6, characterized in that: In step SS1, the number average molecular weight of the polymalic acid is 1000-2000.
8. A Portland cement-based building concrete according to claim 6, characterized in that: In step SS1, the catalyst is any one of tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate or tetramethylammonium bromide.
9. A Portland cement-based building concrete according to claim 6, characterized in that: In step SS2, the mass ratio of the intermediate material to 2,3-epoxypropyltrimethylammonium chloride is 1:0.1-0.
4.
10. A process for manufacturing building concrete based on Portland cement as claimed in claim 1, characterized in that: The following steps are involved: (1) adding sand, crushed stone, fly ash, ordinary Portland cement and functionalized fiber into a mixer, setting the speed of the mixer to 500-700 r / min, stirring for 20-40 min to obtain a blend; (2) adding the composite additive and water to the blend prepared in step (1), and continuing stirring for 10 to 30 minutes to obtain a concrete slurry; (3) The concrete slurry prepared in step (2) is sequentially subjected to pouring treatment, vibrating treatment, leveling treatment and curing treatment to obtain architectural concrete.
Citation Information
Patent Citations
CF50 concrete and preparation process thereof
CN112521065A
Early-strength anti-cracking composite functional additive
CN115286276A
High-crack-resistance concrete and construction method thereof
CN115893940A
Dry-mixed thin-layer anti-crack plastering mortar and preparation method thereof
CN116375399A
Environment-friendly anti-falling ceramic tile adhesive and production process thereof
CN118145937A
Cited By
Modified solid waste recycled aggregate and preparation method thereof
CN120887669A