Foam concrete based on waste glass wool recovery and preparation method thereof
By mixing chopped waste glass wool with fiber dispersant, and using sulfoaluminate cement and highly active fillers, the corrosion and agglomeration problems of waste glass wool in alkaline environments were solved, achieving uniform distribution and performance improvement in foamed concrete, thus solving the problems of environmental pollution and performance enhancement.
Patent Information
- Application Number
- CN202411168947.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
Waste glass wool is easily corroded in the alkaline environment of cement slurry, causing fiber agglomeration, which weakens its reinforcing ability in foamed concrete and makes it difficult to recycle effectively, resulting in environmental pollution.
A suspension was prepared by high-speed stirring of chopped waste glass wool, fiber dispersant and water. Sulfoaluminate cement was used instead of silicate cement. Highly active fillers such as silica fume and fly ash were added, and the quality of autoclaving steam was reduced. Organic hemp fiber was added to improve the bonding strength between the fiber and the cementitious material.
This method achieves uniform distribution and durability of waste glass wool in foamed concrete, improves the flexural strength and compressive strength of foamed concrete, solves the problem of recycling waste glass wool, and alleviates environmental pollution.
Smart Images

Figure CN119038934A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a foam concrete based on recycling of waste glass wool and a preparation method thereof. Background Art
[0002] Glass wool is a lightweight, low-cost inorganic soft material with excellent thermal insulation effect. It has been widely used in insulation fields such as building exterior walls and medium- and high-temperature steam pipes. Since the main chemical component of glass wool is SiO2, landfilled waste glass wool is difficult to degrade naturally and often causes many environmental problems. Therefore, the effective recycling of waste glass wool is not only conducive to solving its own environmental problems, but also brings potential economic benefits.
[0003] Foamed concrete is an inorganic rigid porous thermal insulation material made of calcium and silicon materials through chemical or physical foaming. With the advantages of low cost, good thermal insulation and flame retardant properties, and durability, it has been widely used in the field of building insulation. Reinforced fibers are often used to improve the flexural strength of foamed concrete, including glass fibers, polypropylene fibers, plant fibers, etc. For example, the Chinese invention patent "A composite fiber reinforced foamed concrete and its preparation method" achieves a 50% to 100% increase in flexural strength by incorporating composite fibers (patent publication number: CN102199044A). Unlike it, waste glass wool is exposed to a hot and humid environment for a long time, resulting in obvious fiber agglomeration. At the same time, the glass wool is not alkali-resistant during the production process, which makes the waste glass wool easily corroded in the alkaline environment of cement slurry, thereby weakening the reinforcement ability, and the later autoclave curing process often accelerates the corrosion of the fibers. Therefore, how to solve the problem of easy agglomeration and weak alkali resistance of waste glass wool is conducive to the recycling of waste glass wool in foamed concrete. Summary of the invention
[0004] The purpose of the present invention is to provide a foam concrete based on the recycling of waste glass wool and a preparation method thereof. The foam concrete recycles the waste glass wool resources, which not only alleviates the environmental pollution caused by the landfill of waste glass wool, but also improves the flexural strength of the foam concrete.
[0005] In order to achieve the above-mentioned purpose, the present invention proposes to stir the chopped waste glass wool with a fiber dispersing agent and water at a high speed to prepare a suspension in which the waste glass wool is evenly distributed. In addition, in order to alleviate the corrosion of the surface of the waste glass wool and enhance the durability of the waste glass wool in an alkaline environment, it is decided to use sulphoaluminate cement instead of the more common silicate cement, use highly active fillers such as silica fume and fly ash with higher activity, and appropriately reduce the steam quality of autoclave curing. The specific technical scheme of the present invention is as follows:
[0006] In a first aspect, the present invention provides a foamed concrete based on the recycling of waste glass wool, wherein the foamed concrete is composed of the following raw material components in percentage by mass: 15% to 25% of cementitious material, 30% to 45% of high-activity filler, 0.1% to 8% of chemical foaming agent, 1% to 3% of additive, 0.1% to 0.5% of fiber dispersion aid, 0.5% to 1% of organic hemp fiber, 0.5% to 3% of waste glass wool, and 30% to 40% of water, and the sum of the percentages of each component is 100%.
[0007] Preferably, the cementitious material is sulphoaluminate cement.
[0008] Preferably, the high-activity filler is selected from at least one of silica fume, fly ash and metakaolin.
[0009] Preferably, the chemical foaming agent is at least one of hydrogen peroxide, aluminum powder, ammonium carbonate and ammonium bicarbonate.
[0010] Preferably, the additives consist of a foam stabilizer, a water reducer, a thickener and an early strength agent; the foam stabilizer is selected from at least one of calcium stearate, dodecyl dimethyl amine oxide, and alkyl alcohol amide, the water reducer is selected from at least one of polycarboxylic acid high-efficiency water reducer, naphthalene-based high-efficiency water reducer, and aliphatic high-efficiency water reducer, the thickener is selected from at least one of sodium bentonite, cellulose ether, and polyacrylate, and the early strength agent is selected from at least one of methyl sulfate, sodium nitrate, and calcium formate.
[0011] Preferably, the fiber dispersing aid is selected from at least one of a cationic surfactant, an anionic surfactant, a zwitterionic surfactant, and a nonionic surfactant.
[0012] Preferably, the organic hemp fiber is selected from at least one of sisal, jute and ramie.
[0013] Preferably, the waste glass wool is preliminarily sequentially washed with water, filtered for impurities, soaked in acrylic emulsion, centrifugally crushed and dried, and the final fiber length is less than 2 mm.
[0014] In a second aspect, the present invention provides a method for preparing foamed concrete based on recycling of waste glass wool as described in any one of the schemes of the first aspect above, and the specific method is as follows:
[0015] Step 1: Measure the following components by mass: 15% to 25% of gelling material, 30% to 45% of highly active filler, 0.1% to 8% of chemical foaming agent, 1% to 3% of additive, 0.1% to 0.5% of fiber dispersing aid, 0.5% to 1% of organic hemp fiber, 0.5% to 2% of waste glass wool, and 30% to 40% of water;
[0016] Step 2: All the waste glass wool measured in the first step is washed, impurities are filtered, soaked in acrylic emulsion, centrifuged and crushed, and dried to obtain waste glass wool with a fiber length of less than 2 mm;
[0017] Step 3: Add all the waste glass wool obtained in the second step, all the fiber dispersing aids obtained in the first step, and 5% to 15% of the total water obtained in the first step into the first container, and stir at a high speed of 1000 to 2000 r / min for 25 to 35 minutes to obtain a waste glass wool suspension;
[0018] Step 4: add all the gelling materials measured in the first step and all the high-activity fillers measured in the first step into the second container, and stir at a medium speed of 500-1000 r / min for 3-5 minutes;
[0019] Step 5: Add all the additives measured in the first step, all the organic hemp fibers measured in the first step, and all the remaining water in the total amount of water measured in the first step into the second container, and stir at a high speed of 1500-2000 r / min for 8-12 minutes to obtain a slurry;
[0020] Step 6: Add the waste glass wool suspension in the first container into the second container, stir at a high speed of 1000-2000 r / min for 2-3 minutes, then add all the chemical foaming agent measured in the first step, continue stirring at a high speed of 1000-2000 r / min until uniformly mixed, and then pour into the mold;
[0021] Step 7: The sample cast in the mold is subjected to standard curing, demoulding and cutting, autoclave curing and drying in sequence to obtain the final foam concrete product.
[0022] Preferably, the room temperature for standard curing is 25-35°C, the humidity is greater than 80%, and the curing time is one day; the steam used for autoclave curing is saturated steam at 120-160°C, and the curing time is 4-6 hours.
[0023] Compared with the prior art, the features and innovations of the present invention are:
[0024] 1. The present invention proposes to recycle waste glass wool by means of foam concrete, which not only solves the environmental problem caused by landfilling waste glass wool, but also improves the flexural strength of foam concrete.
[0025] 2. In order to solve the problem of weak alkali resistance of waste glass wool, the present invention uses sulphoaluminate cement instead of silicate cement, uses a large amount of high-activity fillers such as silica fume and fly ash, and reduces the steam quality during autoclave curing, thereby alleviating corrosion on the fiber surface and enhancing its durability in an alkaline environment.
[0026] 3. The present invention proposes that the organic hemp fibers are chopped and soaked in warm water, thereby improving the cohesion of the hemp fibers and the cementitious material of the foamed concrete, and improving the flexural and compressive properties of the foamed concrete.
[0027] 4. The present invention proposes that after the waste glass wool is soaked in acrylic emulsion, the cohesion of the fiber and the cementitious material of the foam concrete is improved, and the weather resistance, durability, impermeability and other properties of the foam concrete are improved.
[0028] 5. In order to solve the problem that waste glass wool is easy to agglomerate, the present invention adopts the measure of stirring the chopped waste glass wool with a fiber dispersing agent and water at a high speed to prepare a waste glass wool suspension, which is conducive to achieving a more uniform distribution of the waste glass wool in the slurry. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The present invention is a flow chart for preparing foamed concrete based on the recycling of waste glass wool.
[0030] Figure 2 This is a stereomicroscope image of the product prepared in Example 1 of the present invention.
[0031] Figure 3 This is an electron microscope scanning image of the discarded glass wool in the product prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] The present invention will be further described and illustrated below in conjunction with the accompanying drawings and specific implementation methods.
[0033] like Figure 1 As shown, the method for preparing foamed concrete based on waste glass wool recycling in the present invention is as follows:
[0034] Step 1: Measure the following components by mass: 15% to 25% of gelling material, 30% to 45% of highly active filler, 0.1% to 8% of chemical foaming agent, 1% to 3% of additive, 0.1% to 0.5% of fiber dispersing aid, 0.5% to 1% of organic hemp fiber, 0.5% to 2% of waste glass wool, and 30% to 40% of water;
[0035] Step 2: All the waste glass wool measured in the first step is washed, impurities are filtered, soaked in acrylic emulsion, centrifuged and crushed, and dried to obtain waste glass wool with a fiber length of less than 2 mm;
[0036] Step 3: Add all the waste glass wool obtained in the second step, all the fiber dispersing aids obtained in the first step, and 5% to 15% of the total water obtained in the first step into the first container, and stir at a high speed of 1000 to 2000 r / min for 25 to 35 minutes to obtain a waste glass wool suspension;
[0037] Step 4: add all the gelling materials measured in the first step and all the high-activity fillers measured in the first step into the second container, and stir at a medium speed of 500-1000 r / min for 3-5 minutes;
[0038] Step 5: Add all the additives measured in the first step, all the organic hemp fibers measured in the first step, and all the remaining water in the total amount of water measured in the first step into the second container, and stir at a high speed of 1500-2000 r / min for 8-12 minutes to obtain a slurry;
[0039] Step 6: Add the waste glass wool suspension in the first container into the second container, stir at a high speed of 1000-2000 r / min for 2-3 minutes, then add all the chemical foaming agent measured in the first step, continue stirring at a high speed of 1000-2000 r / min until uniformly mixed, and then pour into the mold;
[0040] Step 7: The sample cast in the mold is subjected to standard curing, demoulding and cutting, autoclave curing and drying in sequence to obtain the final foam concrete product.
[0041] The room temperature of the curing room for the above standard curing is 25-35°C, the humidity is greater than 80%, and the curing time is one day; the steam used for the autoclave curing is saturated steam at 120-160°C, and the curing time is 4-6 hours.
[0042] In the embodiment of the present invention, the cementitious material can be sulphoaluminate cement, the high-activity filler is selected from at least one of silica fume, fly ash and metakaolin, the chemical foaming agent is selected from at least one of hydrogen peroxide, aluminum powder, ammonium carbonate and ammonium bicarbonate, and the additives are composed of a foam stabilizer, a water reducer, a thickener and an early strength agent; the foam stabilizer is selected from at least one of calcium stearate, dodecyl dimethyl amine oxide, and alkyl alcohol amide, the water reducer is selected from at least one of polycarboxylic acid high-efficiency water reducer, naphthalene-based high-efficiency water reducer, and aliphatic high-efficiency water reducer, the thickener is selected from at least one of sodium bentonite, cellulose ether, and polyacrylate, and the early strength agent is selected from at least one of methyl sulfate, sodium nitrate, and calcium formate; the fiber dispersing aid is selected from at least one of a cationic surfactant, an anionic surfactant, a zwitterionic surfactant, and a non-ionic surfactant; the organic hemp fiber is selected from at least one of sisal, jute, and brown hemp. In addition, waste glass wool is a waste resource utilization raw material. It is best to pre-treat it before using it to prepare foam concrete. The specific method is to wash the waste raw materials with water, filter out impurities, soak them in acrylic emulsion, centrifuge them, and dry them in sequence. The final fiber length is preferably less than 2mm.
[0043] The specific preparation method and technical effect of the above-mentioned foamed concrete based on the recycling of waste glass wool are demonstrated through multiple embodiments below.
[0044] Example 1
[0045] In this embodiment, the preparation method of foamed concrete based on the recycling of waste glass wool is as follows:
[0046] The first step is to take the raw material components according to the following mass parts: 180 catties of sulphoaluminate cement, 50 catties of silica fume, 400 catties of first-grade fly ash, 35 catties of 27.5% hydrogen peroxide, 5.8 catties of foam stabilizer (calcium stearate), 7.7 catties of water reducer (high-efficiency polycarboxylic acid), 0.01 catties of thickener (hydroxypropyl methylcellulose ether), 6.6 catties of early strength agent (calcium formate), 6 catties of organic hemp fiber (jute), 1 catties of fiber dispersing aid (polyacrylamide), 5 catties of waste glass wool and 309 catties of water;
[0047] In the second step, all 5 catties of waste glass wool measured in the first step are washed with clean water for 5 minutes, the washed waste glass wool is filtered through a 40-mesh screen for impurities, and the waste glass wool after impurities are filtered out is immersed in an acrylic emulsion for 4 hours, and the waste glass wool is taken out after 4 hours, and is crushed by a centrifuge at a high speed of 1000-1500r / min for 15 minutes, and finally put into a blast hot air furnace at 80°C for drying for 1 hour, and finally waste glass wool with a fiber length of less than 2mm is obtained;
[0048] In the third step, all the waste glass wool obtained in the second step, all the 1 catties fiber dispersing aid obtained in the first step and part of the water (18 catties) are added into the container ①, and the waste glass wool suspension is obtained after high-speed stirring at 1000-2000 r / min for 30 minutes, and then allowed to stand for use;
[0049] Step 4: add all 180 catties of sulphoaluminate cement, 50 catties of silica fume and 400 catties of first-grade fly ash obtained in the first step into container ② and stir at a medium speed of 500-1000 r / min for 3-5 minutes;
[0050] Step 5: Add all the additives obtained in the first step (5.8 catties of calcium stearate foam stabilizer, 7.7 catties of high-efficiency polycarboxylate water reducer, 0.01 catties of hydroxypropyl methylcellulose ether thickener and 6.6 catties of calcium formate early strength agent), 6 catties of organic hemp fiber and the remaining water (291 catties) into the container ② of the third step and mix with the original materials, and stir at a high speed of 1500-2000 r / min for 10 minutes;
[0051] Step 6: Add all the waste glass wool suspension in container ① into container ② in step 4, stir at 1000-2000 r / min for 2-3 minutes, then add all 35 catties of 27.5% concentration of hydrogen peroxide obtained in step 1, continue stirring at 1000-2000 r / min for 5-10 seconds, and then pour into the mold;
[0052] In the seventh step, the sample cast in the mold in the sixth step is cured in a standard curing room with a temperature of 25-35°C and a humidity greater than 80% and an autoclave (saturated steam at 120-160°C) for a specified time, and then dried to obtain the final foam concrete product.
[0053] Example 2
[0054] In this embodiment, the preparation method of foamed concrete based on the recycling of waste glass wool is as follows:
[0055] The first step is to take the raw material components according to the following mass parts: 180 catties of sulphoaluminate cement, 50 catties of silica fume, 370 catties of first-grade fly ash, 35 catties of 27.5% hydrogen peroxide, 5.8 catties of foam stabilizer (calcium stearate), 7.7 catties of water reducer (high-efficiency polycarboxylic acid), 0.01 catties of thickener (hydroxypropyl methylcellulose ether), 6.6 catties of early strength agent (calcium formate), 2 catties of fiber dispersing aid (polyacrylamide), 6 catties of organic hemp fiber (jute), 10 catties of waste glass wool and 333 catties of water;
[0056] In the second step, all 10 jin of waste glass wool measured in the first step are washed with clean water for 5 minutes, the washed waste glass wool is filtered through a 40-mesh screen for impurities, and the waste glass wool after impurities are filtered out is immersed in an acrylic emulsion for 4 hours, and the waste glass wool is taken out after 4 hours, and is crushed by a centrifuge at a high speed of 1000-1500r / min for 15 minutes, and finally put into a blast hot air furnace at 80°C for drying for 1 hour, and finally waste glass wool with a fiber length of less than 2mm is obtained;
[0057] In the third step, all the waste glass wool obtained in the second step, all the 2 catties fiber dispersing aid obtained in the first step and part of the water (30 catties) are added into the container ①, and the waste glass wool suspension is obtained after high-speed stirring at 1000-2000 r / min for 30 minutes, and then allowed to stand for use;
[0058] Step 4: add all 180 catties of sulphoaluminate cement, 50 catties of silica fume and 370 catties of first-grade fly ash obtained in the first step into container ② and stir at a medium speed of 500-1000 r / min for 3-5 minutes;
[0059] Step 5: Add all the additives obtained in the first step (5.8 catties of calcium stearate foam stabilizer, 7.7 catties of high-efficiency polycarboxylate water reducer, 0.01 catties of hydroxypropyl methylcellulose ether thickener, 6.6 catties of calcium formate early strength agent), 6 catties of organic hemp fiber and the remaining water (303 catties) into the container ② of the third step and mix with the original materials, and stir at a high speed of 1500-2000 r / min for 10 minutes;
[0060] Step 6: Add all the waste glass wool suspension in container ① into container ② in step 4, stir at 1000-2000 r / min for 2-3 minutes, then add all 35 catties of 27.5% concentration of hydrogen peroxide obtained in step 1, continue stirring at 1000-2000 r / min for 5-10 seconds, and then pour into the mold;
[0061] In the seventh step, the sample cast in the mold in the sixth step is cured in a standard curing room with a temperature of 25-35°C and a humidity greater than 80% and an autoclave (saturated steam at 120-160°C) for a specified time, and then dried to obtain the final foam concrete product.
[0062] Example 3
[0063] In this embodiment, the preparation method of foamed concrete based on the recycling of waste glass wool is as follows:
[0064] The first step is to take the raw material components according to the following mass parts: 180 catties of sulphoaluminate cement, 50 catties of silica fume, 340 catties of first-grade fly ash, 35 catties of 27.5% hydrogen peroxide, 5.8 catties of foam stabilizer (calcium stearate), 7.7 catties of water reducer (high-efficiency polycarboxylic acid), 0.01 catties of thickener (hydroxypropyl methylcellulose ether), 6.6 catties of early strength agent (calcium formate), 3 catties of fiber dispersing aid (polyacrylamide), 6 catties of organic hemp fiber (jute), 20 catties of waste glass wool and 352 catties of water;
[0065] In the second step, all 20 catties of waste glass wool measured in the first step are washed with clean water for 5 minutes, the washed waste glass wool is filtered through a 40-mesh screen for impurities, and the waste glass wool after impurities are filtered out is immersed in an acrylic emulsion for 4 hours, and the waste glass wool is taken out after 4 hours, and is crushed by a centrifuge at a high speed of 1000-1500r / min for 15 minutes, and finally put into a blast hot air furnace at 80°C for drying for 1 hour, and finally waste glass wool with a fiber length of less than 2mm is obtained;
[0066] In the third step, all the waste glass wool obtained in the second step, all the 3 catties fiber dispersing aid obtained in the first step and part of the water (40 catties) are added into the container ①, and the waste glass wool suspension is obtained after high-speed stirring at 1000-2000 r / min for 30 minutes, and then allowed to stand for use;
[0067] Step 4: Add all 180 catties of sulphoaluminate cement, 50 catties of silica fume and 340 catties of first-grade fly ash obtained in the first step into container ② and stir at a medium speed of 500-1000 r / min for 3-5 minutes;
[0068] Step 5: Add all the additives obtained in the first step (5.8 catties of calcium stearate foam stabilizer, 7.7 catties of high-efficiency polycarboxylate water reducer, 0.01 catties of hydroxypropyl methylcellulose ether thickener, 6.6 catties of calcium formate early strength agent), 6 catties of organic hemp fiber and the remaining water (312 catties) into the container ② of the third step and mix with the original materials, and stir at a high speed of 1500-2000 r / min for 10 minutes;
[0069] Step 6: Add all the waste glass wool suspension in container ① into container ② in step 4, stir at 1000-2000 r / min for 2-3 minutes, then add all 35 catties of 27.5% concentration of hydrogen peroxide obtained in step 1, continue stirring at 1000-2000 r / min for 5-10 seconds, and then pour into the mold;
[0070] In the seventh step, the sample cast in the mold in the sixth step is cured in a standard curing room with a temperature of 25-35°C and a humidity greater than 80% and an autoclave (saturated steam at 120-160°C) for a specified time, and then dried to obtain the final foam concrete product.
[0071] Example 4
[0072] In this embodiment, the preparation method of foamed concrete based on the recycling of waste glass wool is as follows:
[0073] The first step is to take the raw material components according to the following mass parts: 180 catties of sulphoaluminate cement, 25 catties of silica fume, 325 catties of first-grade fly ash, 35 catties of 27.5% hydrogen peroxide, 5.8 catties of foam stabilizer (calcium stearate), 7.7 catties of water reducer (high-efficiency polycarboxylic acid), 0.01 catties of thickener (hydroxypropyl methylcellulose ether), 6.6 catties of early strength agent (calcium formate), 5 catties of fiber dispersing aid (polyacrylamide), 6 catties of organic hemp fiber (jute), 30 catties of waste glass wool and 380 catties of water;
[0074] In the second step, all 30 catties of waste glass wool measured in the first step are washed with clean water for 5 minutes, and the washed waste glass wool is filtered through a 40-mesh screen for impurities, and the waste glass wool after impurities are filtered out is immersed in an acrylic emulsion for 4 hours, and the waste glass wool is taken out after 4 hours, and is crushed by a centrifuge at a high speed of 1000-1500r / min for 15 minutes, and finally put into a blast hot air furnace at 80°C for drying for 1 hour, and finally waste glass wool with a fiber length of less than 2mm is obtained;
[0075] In the third step, all the waste glass wool obtained in the second step, all the 5 catties fiber dispersing aid obtained in the first step and part of the water (55 catties) are added into the container ①, and the waste glass wool suspension is obtained after high-speed stirring at 1000-2000 r / min for 30 minutes, and then allowed to stand for use;
[0076] Step 4: add all 180 catties of sulphoaluminate cement, 25 catties of silica fume and 325 catties of first-grade fly ash obtained in the first step into container ② and stir at a medium speed of 500-1000 r / min for 3-5 minutes;
[0077] Step 5: add all the additives obtained in the first step (5.8 catties of calcium stearate foam stabilizer, 7.7 catties of high-efficiency polycarboxylate water reducer, 0.01 catties of hydroxypropyl methylcellulose ether thickener, 6.6 catties of calcium formate early strength agent), 6 catties of organic hemp fiber and the remaining water (325) into the container ② of the third step, mix with the original materials, and stir at a high speed of 1500-2000 r / min for 10 minutes;
[0078] Step 6: Add all the waste glass wool suspension in container ① into container ② in step 4, stir at 1000-2000 r / min for 2-3 minutes, then add all 35 catties of 27.5% concentration of hydrogen peroxide obtained in step 1, continue stirring at 1000-2000 r / min for 5-10 seconds, and then pour into the mold;
[0079] In the seventh step, the sample cast in the mold in the sixth step is cured in a standard curing room with a temperature of 25-35°C and a humidity greater than 80% and an autoclave (saturated steam at 120-160°C) for a specified time, and then dried to obtain the final foam concrete product.
[0080] Comparative Example 1
[0081] In this embodiment, the preparation method of foamed concrete based on the recycling of waste glass wool is as follows:
[0082] The first step is to take the raw material components according to the following mass parts: 180 catties of silicate cement, 350 catties of first-grade fly ash, 35 catties of 27.5% hydrogen peroxide, 5.8 catties of foam stabilizer (calcium stearate), 7.7 catties of water reducer (high-efficiency polycarboxylic acid), 0.01 catties of thickener (hydroxypropyl methylcellulose ether), 6.6 catties of early strength agent (calcium formate), 5 catties of fiber dispersing aid (polyacrylamide), 6 catties of organic hemp fiber (jute), 30 catties of waste glass wool and 380 catties of water;
[0083] In the second step, the waste glass wool measured in the first step is washed with clean water for 5 minutes, the washed waste glass wool is filtered through a 40-mesh screen for impurities, and the waste glass wool after impurities are filtered out is immersed in an acrylic emulsion for 4 hours, and the waste glass wool is taken out after 4 hours, and is crushed by a centrifuge at a high speed of 1000-1500r / min for 15 minutes, and finally put into a blast hot air furnace at 80°C for drying for 1 hour, and finally the waste glass wool with a fiber length less than 2mm is obtained;
[0084] In the third step, all the waste glass wool obtained in the second step, all the 5 catties fiber dispersing aid obtained in the first step and part of the water (55 catties) are added into the container ①, and the waste glass wool suspension is obtained after high-speed stirring at 1000-2000 r / min for 30 minutes, and then allowed to stand for use;
[0085] Step 4: add all 180 catties of Portland cement and 350 catties of first-grade fly ash obtained in the first step into container ②, and stir at a high speed of 500-1000 r / min for 3-5 minutes;
[0086] Step 5: Add all the additives obtained in the first step (5.8 catties of calcium stearate foam stabilizer, 7.7 catties of high-efficiency polycarboxylate water reducer, 0.01 catties of hydroxypropyl methylcellulose ether thickener, 6.6 catties of calcium formate early strength agent), 6 catties of organic hemp fiber and the remaining water (325 catties) into the container ② of the third step and mix with the original materials, and stir at a high speed of 1500-2000 r / min for 10 minutes;
[0087] Step 6: Add all the waste glass wool suspension in container ① into container ② in step 4, stir at 1000-2000 r / min for 2-3 minutes, then add all 35 catties of 27.5% concentration of hydrogen peroxide obtained in step 1, continue stirring at 1000-2000 r / min for 5-10 seconds, and then pour into the mold;
[0088] In the seventh step, the sample cast in the mold in the sixth step is cured in a standard curing room with a temperature of 25-35°C and a humidity greater than 80% and an autoclave (saturated steam at 120-160°C) for a specified time, and then dried to obtain the final foam concrete product.
[0089] In this comparative example, except that sulphoaluminate cement is replaced by silicate cement, and the silica fume in the high-activity filler is completely replaced by primary fly ash with lower activity, the rest of the raw materials and preparation method are the same as those of Example 4.
[0090] The products of Examples 1 to 4 of the present invention and Comparative Example 1 were prepared into test pieces. The performance test results of the above-mentioned Examples and Comparative Examples are as follows:
[0091] Taking the foamed concrete specimen in Example 1 as an example, the stereomicroscope image and the electron microscope scanning image of the waste glass wool are as follows: Figure 2 and Figure 3As shown in the figure, it can be found that the pore structure of foamed concrete is mainly composed of circular holes with a pore size of 0.2 to 0.7 mm, and the pore walls are smooth and dense, which is conducive to improving the compressive strength of foamed concrete. In addition, organic hemp fiber and waste glass wool are evenly dispersed in the foamed concrete, and no obvious agglomeration phenomenon is observed. These two types of fibers are tightly combined with the matrix and have no obvious corrosion phenomenon, which further enhances the compressive strength performance of foamed concrete. These results show that the preparation method proposed in the present invention effectively solves the problem of easy agglomeration and corrosion of waste glass wool, and realizes the effective recycling of waste glass wool.
[0092] In addition, the apparent density, compressive strength and flexural strength of the test pieces in Examples 1 to 4 of the present invention and Comparative Example 1 were tested with reference to GB / T 5486-2008 “Test methods for inorganic rigid thermal insulation products”, and the test results are summarized in Table 1.
[0093] Table 1 Summary of test values of apparent density, compressive strength and flexural strength of products
[0094]
[0095] The above-described embodiment is only a preferred solution of the present invention, but it is not intended to limit the present invention. A person skilled in the relevant technical field may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.
Claims
1. A foamed concrete based on the recycling of waste glass wool, It is characterized in that The foamed concrete is composed of the following raw material components in percentage by mass: 15% to 25% of cementitious material, 30% to 45% of high-activity filler, 0.1% to 8% of chemical foaming agent, 1% to 3% of additive, 0.1% to 0.5% of fiber dispersing aid, 0.5% to 1% of organic hemp fiber, 0.5% to 3% of waste glass wool, and 30% to 40% of water, and the sum of the percentages of the various components is 100%.
2. The foamed concrete based on recycled waste glass wool according to claim 1, Features The cementitious material is sulphoaluminate cement.
3. The foamed concrete based on recycling of waste glass wool according to claim 1, Features The high-activity filler is selected from at least one of silica fume, fly ash and metakaolin.
4. The foamed concrete based on recycling of waste glass wool according to claim 1, Features The chemical foaming agent is selected from at least one of hydrogen peroxide, aluminum powder, ammonium carbonate and ammonium bicarbonate.
5. The foamed concrete based on recycling of waste glass wool according to claim 1, Features The additives are composed of a foam stabilizer, a water reducer, a thickener and an early strength agent; the foam stabilizer is selected from at least one of calcium stearate, dodecyl dimethyl amine oxide, and alkyl alcohol amide; the water reducer is selected from at least one of polycarboxylic acid high-efficiency water reducer, naphthalene-based high-efficiency water reducer, and aliphatic high-efficiency water reducer; the thickener is selected from at least one of sodium bentonite, cellulose ether, and polyacrylate; and the early strength agent is selected from at least one of methyl sulfate, sodium nitrate, and calcium formate.
6. The foamed concrete based on recycling of waste glass wool according to claim 1, Features The fiber dispersing aid is selected from at least one of a cationic surfactant, an anionic surfactant, a zwitterionic surfactant, and a nonionic surfactant.
7. The foamed concrete based on recycling of waste glass wool according to claim 1, Features The organic hemp fiber is selected from at least one of sisal, jute and flax.
8. The foamed concrete based on recycling of waste glass wool according to claim 1, Features The waste glass wool is preliminarily processed by washing, filtering impurities, soaking in acrylic emulsion, centrifugal crushing and drying, and the final fiber length is less than 2 mm.
9. A method for preparing foamed concrete based on recycling of waste glass wool as claimed in any one of claims 1 to 8, Features: Step 1: Measure the following components by mass: 15% to 25% of gelling material, 30% to 45% of highly active filler, 0.1% to 8% of chemical foaming agent, 1% to 3% of additive, 0.1% to 0.5% of fiber dispersing aid, 0.5% to 1% of organic hemp fiber, 0.5% to 2% of waste glass wool, and 30% to 40% of water; Step 2: All the waste glass wool measured in the first step is washed, impurities are filtered, soaked in acrylic emulsion, centrifuged and crushed, and dried to obtain waste glass wool with a fiber length of less than 2 mm; Step 3: Add all the waste glass wool obtained in the second step, all the fiber dispersing aids obtained in the first step, and 5% to 15% of the total water obtained in the first step into the first container, and stir at a high speed of 1000 to 2000 r / min for 25 to 35 minutes to obtain a waste glass wool suspension; Step 4: add all the gelling materials measured in the first step and all the high-activity fillers measured in the first step into the second container, and stir at a medium speed of 500-1000 r / min for 3-5 minutes; Step 5: Add all the additives measured in the first step, all the organic hemp fibers measured in the first step, and all the remaining water in the total amount of water measured in the first step into the second container, and stir at a high speed of 1500-2000 r / min for 8-12 minutes to obtain a slurry; Step 6: Add the waste glass wool suspension in the first container into the second container, stir at a high speed of 1000-2000 r / min for 2-3 minutes, then add all the chemical foaming agent measured in the first step, continue stirring at a high speed of 1000-2000 r / min until uniformly mixed, and then pour into the mold; Step 7: The sample cast in the mold is subjected to standard curing, demoulding and cutting, autoclave curing and drying in sequence to obtain the final foam concrete product.
10. The preparation method according to claim 9, Features The room temperature of the standard curing is 25-35° C., the humidity is greater than 80%, and the curing time is one day; the steam used in the autoclave curing is saturated steam at 120-160° C., and the curing time is 4-6 hours.