Thermoplastic powder adhesive spray molding ceramic manufacturing method and ceramic

By using a composite binder spray molding method combining thermoplastic powder and ceramic powder, combined with infiltration treatment, the problems of density and high temperature resistance of ceramic green bodies have been solved, achieving high-precision, water-resistant, and acid and alkali-resistant ceramic molding, which is suitable for the rapid manufacturing of complex structure ceramics.

CN119039014AActive Publication Date: 2024-11-29SHANGHAI JIAOTONG UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411156232.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

Existing adhesive spray molding ceramic manufacturing processes suffer from problems such as low green body density, cracking and disintegration during sintering, poor high-temperature resistance, and difficulty in achieving high-precision molding.

Method used

Thermoplastic powder is mixed with ceramic powder, and polyvinyl alcohol solution and polyethylene glycol are used as composite binders. After spray molding with the binder, impregnation treatment is performed to increase inorganic adhesive bridges and low-melting-point liquid phase substances, promote sintering and form pores.

Benefits of technology

It has achieved high-precision, water-resistant, solvent-resistant, acid and alkali-resistant ceramic green bodies that can be preserved for a long time and sintered at high temperature. They have high strength and high porosity and are suitable for the rapid manufacturing of complex ceramic structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039014A_ABST
    Figure CN119039014A_ABST
Patent Text Reader

Abstract

The invention provides a thermoplastic powder adhesive spray molding ceramic manufacturing method and ceramic, and the method comprises the following steps: providing thermoplastic adhesive powder and ceramic powder, and mixing to obtain mixed powder; the preparation method comprises the following steps: dissolving polyvinyl alcohol powder into deionized water, and then adding polyethylene glycol 400, glycerol and an FS-8 fluorocarbon surfactant to obtain a mixed solution; the mixed solution serves as an adhesive, the mixed powder serves as a base material, and ceramic adhesive spraying manufacturing is carried out; the forming cylinder containing the ceramic biscuit is taken out and dried; carrying out secondary curing, and then naturally cooling the ceramic biscuit; carrying out infiltration treatment in an infiltration solution; and baking and drying, and carrying out high-temperature sintering treatment to obtain the thermoplastic powder adhesive spray molding ceramic. The preparation method solves the problems of low biscuit strength, poor high temperature resistance, poor acid and alkali resistance, poor sintering performance and the like in ceramic adhesive spray molding, and can be used for preparing ceramic products with complex structures and high requirements on precision, strength and porosity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic manufacturing, and in particular to a method for manufacturing thermoplastic powder adhesive spray-molded ceramics and the ceramics. Background Art

[0002] The development of engineering technology has put forward higher requirements for ceramic products. Some application scenarios require the molding of ceramic products with complex shapes, high porosity, and low sintering shrinkage. As a new type of additive manufacturing method, the adhesive jetting method has the advantages of high manufacturing precision, the ability to form complex parts, fast manufacturing, and short manufacturing cycle. However, adhesive jetting manufacturing is not widely used in ceramic manufacturing. The main reason is that the density of the ceramic blanks sprayed by adhesives is low, and it is difficult to achieve sintering densification; at the same time, during the sintering process of the ceramic blanks formed by adhesive jetting, the internal adhesive volatilizes at high temperature, resulting in cracking and direct collapse of the ceramics formed by adhesive jetting after high-temperature sintering. Therefore, it is of great significance to study a ceramic adhesive molding method with high manufacturing precision, good high temperature resistance, and good sintering performance.

[0003] Thermoplastic powder is commonly used in the injection molding of ceramics and metals to manufacture ceramic or metal blanks. It has a long history in the ceramic production industry. Its advantages are that the manufactured ceramic blanks have good strength, high precision, strong resistance to high-temperature deformation, and good sintering performance, but it cannot be directly applied to adhesive jetting ceramic molding. Polyvinyl alcohol solution is a commonly used adhesive in adhesive jetting. Its advantages are high printing accuracy and low diffusion. However, due to the low bonding strength of polyvinyl alcohol itself and the serious problem of polyvinyl alcohol absorbing water in the air, the blanks have low strength, are difficult to post-process after molding, have low sintering strength, and cannot be stored for a long time in humid air. These problems make it difficult to directly mold adhesive jetting ceramics.

[0004] After searching, it was found that the Chinese invention patent with application publication number CN116986910A discloses a method for preparing aluminum nitride ceramics by adhesive injection molding technology. The prior art uses submicron aluminum nitride powder for preparation, and the powder is modified with polyvinyl butyral and hydrophobic agent successively; after the green body is degreased, the green body is infiltrated with metal ions by an infiltration process, and the aluminum nitride ceramic green body is successfully printed out by adhesive injection technology, which can prepare aluminum nitride ceramics with higher performance. The above patent uses polyvinyl butyral as an adhesive for molding, and uses the method of infiltrating metal ions to catalyze the reaction sintering process of aluminum nitride ceramics. In essence, it is still a conventional application of adhesive injection molding ceramics. Summary of the invention

[0005] In view of the defects in the prior art, the purpose of the present invention is to provide a method for manufacturing thermoplastic powder adhesive injection-molded ceramics and ceramics.

[0006] According to one aspect of the present invention, a method for manufacturing ceramics by spraying thermoplastic powder binder is provided, the method comprising:

[0007] Providing thermoplastic adhesive powder and ceramic powder, and mixing the two evenly to obtain mixed powder;

[0008] Dissolve polyvinyl alcohol powder in deionized water at a preset temperature, add polyethylene glycol 400, glycerol and FS-8 fluorocarbon surfactant after the solution is cooled, mix well, and obtain a mixed solution;

[0009] Using the mixed solution as an adhesive and the mixed powder as a base material, performing ceramic adhesive spraying manufacturing;

[0010] Take out the forming cylinder containing the printed ceramic blank and dry it;

[0011] The ceramic green body is subjected to secondary solidification, and then the ceramic green body is allowed to cool naturally;

[0012] The cooled ceramic blank is infiltrated in an infiltration liquid;

[0013] The ceramic green body after the infiltration treatment is baked and dried, and then subjected to high-temperature sintering treatment to obtain thermoplastic powder binder injection-molded ceramics.

[0014] Optionally, thermoplastic adhesive powder and ceramic powder are provided, wherein: the particle size of the thermoplastic adhesive powder and the ceramic powder is 20-100 μm, and the thermoplastic adhesive powder accounts for 3-15wt% of the mixed powder.

[0015] Optionally, in the mixed solution, the mass ratio of polypropylene alcohol is 3-10wt%.

[0016] Optionally, the mixed solution has a solution viscosity of 6-12 mPa·s and a surface tension of 26-42 N / m.

[0017] Optionally, the mixed solution is used as an adhesive and the mixed powder is used as a base material to perform ceramic adhesive jetting manufacturing, wherein: the printing layer thickness is 0.03-0.30 mm, and the adhesive jetting saturation is 30-70%.

[0018] Optionally, the forming cylinder containing the printed ceramic blank is taken out and dried, wherein the drying temperature is 120-145° C. and the drying time is 4-8 hours.

[0019] Optionally, the ceramic green body is subjected to secondary curing, wherein the curing temperature is 5-8° C. above the melting point of the thermoplastic adhesive powder and the curing temperature is maintained for 1-1.5 hours.

[0020] Optionally, the cooled ceramic green body is infiltrated in an infiltration liquid, wherein the infiltration liquid is any one of titanium dioxide sol, aluminum sol and ethyl silicate.

[0021] Optionally, the cooled ceramic green body is subjected to an infiltration treatment in an infiltration liquid, wherein the infiltration treatment time is 1-3 hours and the infiltration treatment is carried out in a vacuum environment.

[0022] According to another aspect of the present invention, there is provided a ceramic, which is prepared by the above-mentioned method for manufacturing ceramic by spraying thermoplastic powder binder.

[0023] Compared with the prior art, the present invention has at least one of the following beneficial effects:

[0024] 1. The ceramic manufacturing method provided by the present invention uses polyvinyl alcohol solution and thermoplastic binder powder as a secondary composite binder system to perform adhesive spraying ceramic manufacturing, which can ensure that the adhesive spraying ceramic blank has high precision and good water resistance, solvent resistance, acid and alkali resistance and high temperature resistance, so that the ceramic blank has the ability to be stored for a long time, sintered at high temperature and impregnated with solution. Then, the adhesive spraying ceramic blank is subjected to infiltration treatment. First, the infiltration treatment increases the inorganic bonding bridge inside the ceramic blank, which increases the high temperature resistance of the ceramic blank during the sintering process; secondly, the bonding bridge is added between the ceramic blank particles, which helps the atomic diffusion on the surface of the ceramic particles and increases the sintering performance; thirdly, the inorganic bonding bridge added between the ceramic powder itself is a low melting point liquid phase substance, which can promote the sintering of ceramics. At the same time, the thermoplastic component oxidizes and disappears during the high temperature sintering process to form pores, which also ensures that the final product has a higher porosity.

[0025] 2. The adhesive sprayed ceramic product prepared by the present invention has the advantages of high green body strength and high dimensional accuracy, and the green body has good water resistance, solvent resistance, acid and alkali resistance, and can be stored for a long time in a humid environment. The dimensional accuracy and product strength of the product obtained after sintering are both high, and the porosity is high to meet the relevant requirements.

[0026] 3. The present invention can manufacture ceramic products with any complex shape and structure, and is suitable for the production of structural ceramics and functional ceramics with complex shapes, which can greatly reduce the production cycle and save manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0028] Figure 1 It is a schematic diagram of the process of manufacturing a ceramic by spraying thermoplastic powder adhesive in one embodiment of the present invention;

[0029] Figure 2 Schematic diagram of a printed model manufactured by jetting ceramic adhesive according to an embodiment of the present invention. DETAILED DESCRIPTION

[0030] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0031] An embodiment of the present invention provides a method for manufacturing ceramics by spraying thermoplastic powder adhesive, referring to Figure 1 The process diagram shown in FIG. 1 includes:

[0032] S1. Providing thermoplastic adhesive powder and ceramic powder, and mixing the two evenly to obtain mixed powder;

[0033] S2, dissolving polyvinyl alcohol powder in 60-80° C. deionized water, adding polyethylene glycol 400, glycerol and FS-8 fluorocarbon surfactant after the solution is cooled, and mixing well to obtain a mixed solution;

[0034] S3, using the mixed solution as an adhesive and the mixed powder as a base material to perform ceramic adhesive spraying manufacturing;

[0035] S4, taking out the forming cylinder containing the printed ceramic blank and drying it;

[0036] S5, performing secondary solidification on the ceramic blank, and then allowing the ceramic blank to cool naturally to room temperature;

[0037] S6, infiltrating the cooled ceramic blank into an infiltration liquid;

[0038] S7, baking and drying the ceramic green body after the infiltration treatment, and sintering it at high temperature to obtain thermoplastic powder binder injection-molded ceramics.

[0039] The method provided in the embodiment of the present invention adopts polyvinyl alcohol solution and thermoplastic powder as a composite adhesive system to achieve high-strength, high-precision, acid-alkali salt water-resistant and long-term storable adhesive spraying ceramic green billets, and finally achieves high-strength and variable high-porosity ceramic molding, which solves the problems of low green billet strength, inability to perform infiltration treatment, poor high temperature resistance, poor acid and alkali resistance, poor sintering performance, etc. in ceramic adhesive spraying molding, and can be used for adhesive spraying preparation of ceramic products with complex structures and high requirements for precision, strength and porosity.

[0040] In some embodiments, in step S1, the thermoplastic adhesive powder can be any one of polypropylene (PP), polylactic acid (PLA), acrylonitrile-butadiene-styrene copolymer (ABS), industrial paraffin, etc.; the ceramic powder can be any one of aluminum oxide, zirconium oxide, aluminum nitride, silicon carbide, boron nitride, etc. The particle size of the thermoplastic adhesive powder and the ceramic powder is 20-100μm, and the particle size of the thermoplastic adhesive powder is selected to be the same as or similar to the particle size of the ceramic powder. The specific particle size value is determined by the application scenario. In order to achieve uniform mixing of the thermoplastic adhesive powder and the ceramic powder, the two are placed in a mixer and stirred thoroughly. The thermoplastic adhesive powder accounts for 3-15wt% of the mixed powder, and the green blank strength and porosity increase with the increase of the mass ratio of the thermoplastic adhesive.

[0041] In step S2, after adding each component, stir thoroughly until the solution is mixed evenly. In some embodiments, in the mixed solution, the mass ratio of polypropylene alcohol is 3-10wt%. According to the performance properties of the solution, polyethylene glycol 400, propylene glycol, FS-8 fluorocarbon surfactant, etc. are added accordingly, polyethylene glycol 400 mainly adjusts the surface tension of the solution, propylene glycol adjusts the viscosity of the solution, and FS-8 is used as an auxiliary to adjust the surface tension of the solution, ensuring that the solution viscosity of the mixed solution is 6-12mPa·s and the surface tension is 26-42N / m, thereby ensuring that the mixed solution has appropriate viscosity and surface tension to meet the requirements of the piezoelectric nozzle printing of the adhesive injection device, and at the same time, the above-mentioned liquid viscosity and surface tension can ensure that the solution produces less blooming and diffusion after being sprayed onto the powder bed, so that it can be used as a liquid adhesive in the adhesive injection.

[0042] In step S3, the mixed powder is used as a printing substrate, and the mixed solution is used as a printing adhesive for printing. In some embodiments, the printing layer thickness is 0.03-0.30 mm, and the adhesive injection saturation is 30-70%. The printing layer thickness mainly determines the interlayer dimensional accuracy of the adhesive injection molding blank, and matches the powder particle size, while the adhesive injection saturation mainly determines the strength of the blank after drying, ensuring that the blank will not be damaged during powder cleaning.

[0043] In step S4, the forming cylinder containing the printed ceramic blank is placed in a blast drying oven for drying. In some embodiments, the drying temperature is 120-145° C. and the drying time is 4-8 hours to ensure that the blank is dried and solidified without melting the thermoplastic adhesive powder.

[0044] In some embodiments, before step S5, the method further comprises: taking out the dried and solidified ceramic blank, and performing a thorough powder cleaning to ensure that no floating powder remains inside the ceramic blank.

[0045] In some embodiments, in step S5, the ceramic blank needs to be placed in glass bead powder for secondary curing, and the curing temperature is 5-8°C above the melting point of the thermoplastic adhesive powder in the mixed powder, and the temperature is kept for 1-1.5 hours. Taking polypropylene (PP) as an example, its melting point is 155°C, and the secondary curing temperature is 160°C to ensure that the polypropylene powder is re-melted and a bonding bridge is formed between the powders, so that the ceramic blank has high strength, solvent resistance, water resistance, acid and alkali resistance, and long-term storage ability.

[0046] In some embodiments, in step S6, the substance infiltrated into the interior of the green blank is an inorganic bonding bridge formed after the impregnation liquid dries, and the bonding bridge itself is a low-melting-point substance. The impregnation liquid used for the infiltration treatment is any one of titanium dioxide sol, aluminum sol and ethyl silicate. Titanium dioxide sol, aluminum sol, ethyl silicate, etc. can provide an inorganic bonding bridge for the ceramic green blank, and the inorganic bonding bridge acts as a low-melting-point phase for fluxing during the sintering process to promote sintering. Furthermore, the impregnation liquid also includes phenolic resin, which, as a reinforcing phase of the green blank, can enhance the strength performance of the ceramic green blank at room temperature. The infiltration time is 1-3 hours, and the infiltration treatment is carried out in a vacuum environment to ensure that the infiltration liquid is fully immersed in the ceramic green blank.

[0047] In some embodiments, in step S7, the baking and drying temperature is 120-150°C, and the high temperature sintering temperature is 900-1550°C. The high temperature sintering temperature is determined by the ceramic powder and the ceramic application occasion, so as to obtain the desired ceramic product.

[0048] Another embodiment of the present invention provides a ceramic, which is prepared by using the above-mentioned method for manufacturing ceramics by spraying thermoplastic powder adhesive.

[0049] In the above embodiment of the present invention, polyvinyl alcohol solution and thermoplastic powder are used as the secondary composite adhesive system to manufacture adhesive sprayed ceramics, which ensures that the adhesive sprayed ceramic blank has high precision and good water resistance, solvent resistance, acid and alkali resistance and high temperature resistance, so that the ceramic blank has the ability to be stored for a long time, sintered at high temperature and impregnated with solution. The use of impregnation liquid to infiltrate the adhesive sprayed ceramic blank has the following advantages: (1) inorganic bonding bridges are added inside the ceramic blank to increase the high temperature resistance of the ceramic blank during sintering; (2) bonding bridges are added between the ceramic blank particles, which helps the atomic diffusion on the surface of the ceramic particles and increases the sintering performance; (3) low melting point liquid phase substances are added between the ceramic powders to promote ceramic sintering. At the same time, the thermoplastic components are oxidized and disappear during the high temperature sintering process to form pores, which also ensures that the final product has a higher porosity.

[0050] The above embodiment of the present invention selects thermoplastic powder and polyvinyl alcohol solution as the secondary composite adhesive, and strengthens it through a post-treatment method of infiltration, which is beneficial to reducing the ceramic manufacturing cost, improving the ceramic manufacturing working environment, reducing the ceramic sintering temperature, and reducing the ceramic manufacturing cost.

[0051] By using the above-mentioned embodiment method of the present invention, through the mutual coordination of each step and each process parameter, the obtained adhesive spraying ceramic product has the advantages of high green body strength and high dimensional accuracy. The green body is resistant to water, solvents and acid and alkali, and can be stored for a long time in a humid environment. The product obtained after sintering has high dimensional accuracy and strength, and has high porosity, so as to meet relevant needs.

[0052] The ceramic products manufactured by the adhesive injection molding method in the above-mentioned embodiment of the present invention can be manufactured into any complex shape and structure, and are suitable for the production of structural ceramics and functional ceramics with complex shapes, which can greatly reduce the production cycle and save manufacturing costs.

[0053] The scheme of the present application will be explained below in conjunction with specific embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the documents in this area or the product specifications are carried out. The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained through commercial channels.

[0054] Example 1

[0055] This embodiment provides a method for manufacturing ceramics by spraying thermoplastic powder adhesive, which is used to manufacture alumina ceramic mold shells for turbine blades, comprising the following steps:

[0056] Step 1, placing polypropylene powder with a particle size of 30 μm and alumina ceramic powder with a particle size of 20-50 μm in a blender, and stirring the mixture thoroughly to mix it evenly;

[0057] Step 2, dissolving 5wt% polyvinyl alcohol powder in hot deionized water, adding 10wt% polyethylene glycol 400, 5wt% propylene glycol, and 0.2wt% FS-8 fluorocarbon surfactant after the solution is cooled, and stirring thoroughly until the solution is mixed evenly;

[0058] Step 3: Use the mixed solution as adhesive and the mixed powder as substrate to perform ceramic adhesive jetting in an adhesive jetting device. Select a printing layer thickness of 0.10 mm and an adhesive jetting saturation of 70%. The printed model is as follows: Figure 2 As shown;

[0059] Step 4: Take out the forming cylinder containing the printed ceramic blank and place it in a blast drying oven for drying at a temperature of 120°C for 4 hours;

[0060] Step 5: Take out the dried and solidified ceramic blank and clean the powder carefully to make sure there is no floating powder residue inside the blank;

[0061] Step 6: The ceramic green blank after powder cleaning is subjected to secondary curing at a curing temperature of 160° C. and kept at this temperature for 1 hour, and then the green blank is allowed to cool naturally. At this time, the green blank obtained has high strength, high dimensional accuracy, and acid, alkali, salt and water resistance, and can be stored in various environments for a long time;

[0062] Step 7, placing the above green blank after cooling in ethyl silicate for infiltration treatment, the infiltration time is 1 hour, and vacuum is applied during the infiltration;

[0063] Step 8, bake and dry the green blank sample after infiltration, the drying temperature is 150°C, the drying time is 2 hours, the sample is heated to 1180°C at a rate of 2°C / min, and kept warm for 4 hours, and then sintered at high temperature to finally obtain the required adhesive injection-molded ceramic product, whose room temperature flexural strength reaches 30-50MPa, and high temperature flexural strength reaches 10MPa and above, and at the same time has an apparent porosity higher than 55%. Conventional adhesive injection-molded ceramic products have difficulty in coexisting flexural strength and high porosity. While ensuring that the flexural strength is similar to that of the ceramic product in the embodiment of the present invention, its porosity is generally 35% or less, and it is difficult to achieve both high strength and high porosity.

[0064] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various modifications or variations within the scope of the claims, which does not affect the essence of the present invention. The above preferred features can be used in any combination without conflicting with each other.

Claims

1. A method for manufacturing ceramics by spraying thermoplastic powder adhesive, It is characterized in that include: Providing thermoplastic adhesive powder and ceramic powder, and mixing the two evenly to obtain mixed powder; Dissolve polyvinyl alcohol powder in deionized water at a preset temperature, add polyethylene glycol 400, glycerol and FS-8 fluorocarbon surfactant after the solution is cooled, mix well, and obtain a mixed solution; Using the mixed solution as an adhesive and the mixed powder as a base material, performing ceramic adhesive spraying manufacturing; Take out the forming cylinder containing the printed ceramic blank and dry it; The ceramic green body is subjected to secondary solidification, and then the ceramic green body is allowed to cool naturally; The cooled ceramic blank is infiltrated in an infiltration liquid; The ceramic green body after the infiltration treatment is baked and dried, and then subjected to high-temperature sintering treatment to obtain thermoplastic powder binder injection-molded ceramics.

2. The method for manufacturing ceramics by spraying thermoplastic powder adhesive according to claim 1, It is characterized in that Thermoplastic adhesive powder and ceramic powder are provided, wherein: the particle size of the thermoplastic adhesive powder and the ceramic powder is 20-100 μm, and the thermoplastic adhesive powder accounts for 3-15wt% of the mixed powder.

3. The method for manufacturing ceramics by spraying thermoplastic powder adhesive according to claim 1, It is characterized in that In the mixed solution, the mass ratio of polypropylene alcohol is 3-10wt%.

4. The method for manufacturing ceramics by spraying thermoplastic powder binder according to claim 1, It is characterized in that The mixed solution has a solution viscosity of 6-12 mPa·s and a surface tension of 26-42 N / m.

5. The method for manufacturing ceramics by spraying thermoplastic powder adhesive according to claim 1, It is characterized in that The mixed solution is used as an adhesive and the mixed powder is used as a base material to perform ceramic adhesive jetting manufacturing, wherein: the printing layer thickness is 0.03-0.30 mm, and the adhesive jetting saturation is 30-70%.

6. The method for manufacturing ceramics by spraying thermoplastic powder adhesive according to claim 1, It is characterized in that The forming cylinder containing the printed ceramic blank is taken out and dried, wherein the drying temperature is 120-145° C. and the drying time is 4-8 hours.

7. The method for manufacturing ceramics by spraying thermoplastic powder adhesive according to claim 1, It is characterized in that The ceramic blank is subjected to secondary curing, wherein the curing temperature is 5-8° C. above the melting point of the thermoplastic adhesive powder and the curing temperature is maintained for 1-1.5 hours.

8. The method for manufacturing ceramics by spraying thermoplastic powder adhesive according to claim 1, It is characterized in that The cooled ceramic blank is infiltrated in an infiltration liquid, wherein the infiltration liquid is any one of titanium dioxide sol, aluminum sol and ethyl silicate.

9. The method for manufacturing ceramics by spraying thermoplastic powder adhesive according to claim 1, It is characterized in that The cooled ceramic blank is infiltrated in an infiltration liquid, wherein the infiltration time is 1-3 hours and the infiltration is carried out in a vacuum environment.

10. A ceramic, It is characterized in that The ceramic is prepared by the method for manufacturing thermoplastic powder adhesive spray-molded ceramics as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Multi-nozzle cooperative control ceramic powder 3D forming method

    CN106903775A

  • Photocuring 3D printing modified ceramic core and preparation method thereof

    CN114105621A

  • Ceramic-metal composite material based on binder jet printing and preparation method thereof

    CN116516209A

  • Method for preparing aluminum nitride ceramic by adhesive spray molding technology

    CN116986910A

  • Built in sterilizing Drying rack

    KR102218159B1