Fragrance slow-release ceramic material and preparation method thereof

The preparation of high porosity fragrance ceramic materials through hot die casting molding process solves the problems of complex process and low fragrance absorption in the prior art, realizes the long-term emanation of fragrance and the durability of ceramics, and provides color and decoration. Sexual function.

CN119039041AActive Publication Date: 2024-11-29WUHAN CUBIC OPTOELECTRONICS CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411125846.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-29
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The preparation process of existing fragrance ceramic materials is complex, with low porosity and fragrance absorption. The dye decomposition of colored ceramics after the use time increases, affecting the performance of ceramic materials.

Method used

Using hot die-casting process of sheet alumina and calcined kaolin with liquid paraffin and additives, high porosity ceramic materials are prepared by sintering and surface treatment, and metal mineral coloring materials are added to the raw materials to maintain color uniformity and Incense rate.

Benefits of technology

The preparation of ceramic materials with high porosity and high fragrance absorption is achieved, which simplifies the process flow, reduces costs, ensures the long-term emanation of the fragrance and the durability of the ceramics, and provides color and decorative functions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039041A_ABST
    Figure CN119039041A_ABST
Patent Text Reader

Abstract

The invention discloses a fragrance slow-release ceramic material and a preparation method thereof. The invention relates to the technical field of fragrance products. The preparation method comprises the following steps: S1, uniformly mixing flaky aluminum oxide and calcined kaolin powder; s2, heating and stirring the powder, adding liquid paraffin which is molten in a hot state and an additive at the same time, and stirring to obtain ceramic slurry; s3, vacuumizing and stirring the prepared ceramic slurry, and performing hot die-casting forming to prepare a ceramic green body; s4, embedding the ceramic green body into aluminum oxide sintering powder, then putting the ceramic green body into a kiln for primary sintering, taking out a sintered ceramic block after cooling, and then carrying out surface treatment; and S5, the treated ceramic block is soaked with fragrance, and packaging is conducted after the surface of the ceramic block is dried after fragrance soaking is completed. The microcosmic pore structure of the porous ceramic block is optimized, and meanwhile, a hot die-casting forming mode is adopted, so that the contradiction between light weight and high strength of the traditional porous ceramic is overcome, and the porous ceramic block has relatively high porosity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fragrance products, and in particular to a fragrance slow-release ceramic material and a preparation method thereof. Background Art

[0002] There are two main ways of dispersing fragrance products commonly found on the market: liquid and solid. Liquid fragrances evaporate quickly and have a distinct smell, but they are prone to leakage, have harsh storage environments, and may burn and explode at high temperatures, so they are rarely used in car fragrances; solid fragrances mainly include fragrance pastes and fragrance carriers, which make the fragrance into a solid paste or use other carriers to absorb the fragrance liquid so that the fragrance is slowly released. Therefore, compared with liquid fragrances, solid fragrances are more flexible and convenient to use, and the fragrance lasts longer.

[0003] Compared with liquid perfume, solid fragrance has a more delicate fragrance and a longer fragrance dissipation time. Common fragrance pastes are made by mixing fragrance with pastes and then putting them into containers to make pastes, which can be dispersed by natural evaporation; while carrier products often use carrier media such as gypsum, silica gel, paper, and ceramics to absorb a large amount of fragrance liquid and control the evaporation rate, so as to achieve long-term fragrance retention. Among the common carrier materials, the strength of gypsum carriers is relatively low, and the fragrance absorption rate of silica gel carriers is not high. The porous ceramic carrier has become the preferred fragrance carrier material due to its excellent mechanical strength, stable physical and chemical properties, strong fragrance adsorption and excellent decorative effect. By absorbing a sufficient amount of fragrance liquid by ceramic materials, it can have the function of slowly dispersing fragrance for a long time, but general ceramics absorb fragrance substances and penetrate into ceramic products with porous structures, and use pores to store fragrance liquid, but the fragrance substances are released too quickly. In addition, some high-end users require the use of colored ceramic carriers, which use different colors of pigments to match ceramics, have unique decorative effects, and can be used in different occasions.

[0004] At present, there are various methods for preparing porous ceramics, such as particle stacking method, pore-forming agent method, extrusion molding method, foam impregnation method and foaming method, but most of them are complicated and costly. For example, the Chinese patent, publication number CN111807861A provides a porous ceramic, which uses a dry pressing molding method. Not only is the manufacturing process complicated, but the final porosity of the prepared ceramic and the fragrance release time cannot be taken into account; at the same time, it uses solid fragrance material melt impregnation, which increases the difficulty of absorbing fragrance; another example is a multi-level aperture fragrance slow-release ceramic disclosed in publication number CN115893979A. This technology uses dry pressing to prepare a porous ceramic matrix, and then prepares a slurry of whisker-reinforced microporous ceramics, which is poured onto the surface of the porous ceramic matrix. After drying, the assembly is obtained. Not only is the process complicated, but it also complicates the design of the product. The porosity of the porous ceramic matrix finally obtained is only about 30%.

[0005] In addition, in order to meet the needs of high-end users for colorful ceramic carriers, the existing technology usually dyes the finished scented ceramic products, but the dye will gradually decompose with the increase of usage time, and after the colorant is added to the raw materials, the colorant will affect the porosity and aroma absorption rate of the ceramic material during the sintering process.

[0006] In summary, the present application aims to solve the problems of complex preparation process, low porosity and low fragrance absorption rate existing in the aroma ceramic materials in the prior art. Summary of the invention

[0007] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and to propose a fragrance slow-release ceramic material and a preparation method thereof. The ceramic prepared by the present invention has the characteristics of high porosity, and the pores in the ceramic are used to store fragrance substances and slowly release the fragrance.

[0008] A method for preparing a fragrance slow-release ceramic material of the present invention comprises the following steps:

[0009] S1. Mix the weighed flaky alumina and calcined kaolin powder evenly;

[0010] S2, heating and stirring the above powder, adding hot melted liquid paraffin and additives, and stirring for a period of time to obtain a ceramic slurry;

[0011] S3, vacuuming, stirring, and hot-pressing the prepared ceramic slurry to obtain a ceramic green body;

[0012] S4, burying the ceramic green body in alumina sintered powder, and then putting it into a kiln for firing, taking out the buried and fired ceramic block after cooling, and then performing surface treatment;

[0013] S5, soaking the processed ceramic block in fragrance, and packaging the ceramic block after the surface is dried.

[0014] Furthermore, the step S1 further comprises a colorant, the mass of which is 1% to 10% of the sum of the mass of the colorant, flaky alumina and calcined kaolin.

[0015] Furthermore, the colorant is a metallic mineral phase colorant.

[0016] Furthermore, the median diameter of the flaky aluminum oxide is between 3 and 30 μm, and the width-to-thickness ratio is between 1 and 10; the median diameter of the calcined kaolin is between 1 and 3 μm.

[0017] Furthermore, in the ceramic slurry, the mass ratio of flaky alumina, calcined kaolin, paraffin wax and additives is 40-60:20-40:15-20:1-5.

[0018] Furthermore, in step S2, the heating temperature is 65°C to 90°C, and the stirring time is 4 to 8 hours.

[0019] Furthermore, the additive is beeswax, stearic acid or oleic acid.

[0020] Furthermore, the specific operation of step S3 is: adding the prepared ceramic slurry into a molding machine, setting the temperature at 60°C to 75°C, evacuating and stirring for 10 to 300 minutes, and then hot-die casting at a pressure between 0.4 and 0.8 MPa and a holding time of 5s to 30s.

[0021] Furthermore, in step S4, the primary sintering temperature is controlled between 1200 and 1400°C.

[0022] Furthermore, after the firing is completed, the product is first subjected to vibration screening to remove the buried powder, and then the surface of the product is polished to remove the adhering powder particles.

[0023] Furthermore, the incense soaking method can be a soaking or infusion method according to needs.

[0024] A fragrance slow-release ceramic material prepared by the above-mentioned preparation method.

[0025] The preparation of a fragrance slow-release ceramic material of the present invention includes the following raw materials: flaky alumina, calcined kaolin, solid paraffin and additives. Flaky alumina and calcined kaolin are used as raw materials for ceramic blocks to provide them with porous properties; paraffin has a low melting point and is in liquid state after heating, which is easy for slurry injection molding, and is easy to shape after cooling and solidification; commonly used additives include beeswax, stearic acid, oleic acid, etc., which can reduce the surface energy of the interface between paraffin and powder particles, thereby reducing the amount of paraffin, increasing the solid phase content of ceramic powder in the slurry, and obtaining good slurry fluidity.

[0026] By combining the above raw materials, using flaky alumina and calcined kaolin of specific particle size and morphology, that is, by using flaky alumina powder with a fixed width-to-thickness ratio, combined with calcined kaolin, adding heated liquid paraffin, stirring and mixing evenly, a slurry with stable characteristics is made, and after hot die casting, the paraffin therein is cooled and solidified to obtain a formed ceramic block; sintering is performed once at a high temperature, the wax therein is removed, and the small particles of kaolin powder are bonded together with the flaky alumina particles to form a large number of fine gaps. At the same time, due to the use of flaky alumina, some slightly larger pores will be formed between its particles, such as the attached Figure 2. Therefore, without adding any pore-forming agent, a ceramic block with high porosity (porosity can reach 45% to 55%) and specific pore size is manufactured, which ensures the long-term release of fragrance and provides performance guarantee for practical applications; at the same time, after use, the pores are used to store fragrance substances and slowly release the fragrance. After the fragrance fades, the same fragrance liquid can be repeatedly added for continued use; even different fragrance liquids can be added after high-temperature treatment to achieve multiple reuse of ceramic blocks, greatly improving utilization and reducing costs. At the same time, it also has different colors, which can be matched with different fragrances according to the color, so it also has a unique decorative effect and can be used in different occasions.

[0027] The fragrance slow-release ceramic material of the present invention optimizes the microscopic pore structure of the porous ceramic block and adopts the hot-pressing casting method to have a high porosity, and has the advantages of simple process and low cost. The raw materials with specific characteristics not only ensure the strength of the product, but also do not reduce the porosity of the product, so that the fragrance durability is guaranteed; at the same time, the mold can be changed according to the needs, so that products of various shapes can be prepared.

[0028] On the other hand, the present invention adopts liquid fragrance material, which has obvious fragrance characteristics, and provides the fragrance ceramic with the ability to emit fragrance for a long time; and then stores and further slows down the emission speed of the fragrance material by absorption through tiny pores inside the product.

[0029] Beneficial effects of the present invention:

[0030] 1. The present invention uses the matching effect of raw materials with specific particle sizes and morphologies, mixes colorants, and prepares high-porosity ceramic materials through a simple hot-pressing molding process without a pore-forming agent, providing an excellent storage carrier for fragrance substances, overcoming the disadvantage of low strength of traditional fragrance ceramic carriers, and achieving more absorption and slow release of fragrance; it can also prepare colored ceramics by adding colorants to the raw materials as needed, which not only ensures uniform color mixing, but also does not affect the porosity and fragrance absorption rate of the ceramic material during the sintering process.

[0031] 2. The present invention uses a hot die casting process, including mixing, stirring slurry, hot die casting, one-time firing, surface treatment and other processes. Compared with dry pressing, the difficulty is greatly reduced; at the same time, one-time firing is used to combine the traditional wax removal and firing processes, which reduces the cost, and the molded products are more uniform and more efficient; the difficulty of production is greatly reduced, and 1 to 2 people can complete the preparation of the product. At the same time, one-time firing greatly shortens the time and improves the efficiency.

[0032] 3. The product prepared by the present invention has a higher degree of freedom in design. Products of various shapes can be prepared according to the adjustment of the mold. The product itself can also have different colors. At the same time, the product surface can be etched or glazed to meet the needs of different scenes. The decorative effect and application range of the product are greatly improved.

[0033] 4. The present invention uses liquid fragrance, so compared with solid fragrance, the fragrance is more obvious and rich, which reduces the difficulty of the sample to absorb the fragrance, and different fragrances can be added, and the fragrance can be matched according to the color of the product, so that the ornamental value of the product is improved; after a long period of use, the fragrance can be repeatedly added and continued to be used, or after high-temperature treatment, different fragrance liquids can be added, and the utilization rate of the ceramic block is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is the electron microscope image of the raw material flake aluminum oxide;

[0035] Figure 2 This is a physical picture of the fragrance ceramic block product prepared in Example 1;

[0036] Figure 3 This is a pore size measurement diagram of the fragrance sustained-release ceramic material prepared in Example 1. DETAILED DESCRIPTION

[0037] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0038] The preparation method of a fragrance slow-release ceramic material of the present invention comprises the following specific steps:

[0039] 1. Add the weighed special flake alumina and calcined kaolin powder into the mixer and mix evenly;

[0040] 2. Place the mixed powder in a mixer, set the temperature at 65°C to 90°C, add hot melted liquid paraffin and additives, and obtain ceramic slurry after stirring for 4 to 8 hours;

[0041] Specifically, the median particle size of the flaky alumina powder is between 1 and 30 μm, preferably 3-15 μm to obtain better slurry properties and the porosity of the final ceramic block; the width-to-thickness ratio of the flaky particles is between 1 and 20, preferably between 4 and 10, as shown in the attached Figure 1 At the same time, in order to have a better match with the flaky aluminum oxide, the median particle size of the calcined kaolin powder is selected to be between 1 and 10 μm; the additive can be beeswax, stearic acid or oleic acid, etc.

[0042] 3. Add the prepared ceramic slurry into the molding machine, set the temperature at 60°C to 75°C, evacuate and stir for 10 to 300 minutes, and then hot-die cast the slurry at a pressure between 0.4 and 0.8 MPa and a holding time of 5s to 30s.

[0043] 4. In order to ensure the shape of the ceramic block during high-temperature sintering, we need to bury the obtained ceramic green body in a specific alumina sintering powder, then put it into the kiln for firing once, take out the buried ceramic block after cooling, and then perform surface treatment.

[0044] Specifically, the primary firing temperature is controlled between 1200 and 1400° C. After firing, the product is first subjected to vibration screening to remove the buried burnt powder, and then the surface of the product is polished to remove the adhered powder particles.

[0045] 5. Soak the processed products in fragrance, and then package them after the surface of the products are dry.

[0046] Specifically, the incense soaking method can be a soaking or incense injection method according to needs.

[0047] Embodiment 1:

[0048] (1) 3300 g of flaky aluminum oxide and 2700 g of calcined kaolin were weighed in a mixer, and the mixture was ball-milled for 24 h. The powder was then transferred to a blender, and 1470 g of hot melted paraffin, 200 g of beeswax, and 32 g of oleic acid were added. The mixture was mixed and stirred for 4 h to obtain a ceramic slurry.

[0049] (2) The ceramic slurry obtained in step (1) was transferred into a hot molding machine, and vacuum was started and stirred for 30 minutes. After completion, the hot pressing pressure was adjusted to 0.6 MPa and the holding time was 15 seconds to obtain a sample green body.

[0050] (3) The ceramic green body obtained in step (2) is buried and then sent into a kiln for firing at a temperature of 1300° C. After firing, the sample is vibrated and sorted to obtain a fired sample, such as Figure 2 .

[0051] (4) The ceramic block obtained in step (3) is surface-polished to remove the powder adhering to the surface to obtain a finished product.

[0052] Finally, a porous ceramic block with a porosity of 49% was obtained according to the above steps. The ceramic block was immersed in the fragrance liquid for 24 hours, and its weight fragrance absorption rate could reach about 25%.

[0053] Figure 3 This is the pore size distribution spectrum of the fragrance sustained-release ceramic material prepared in Example 1, and the corresponding average pore size is 643.73 nm.

[0054] Embodiment 2:

[0055] (1) Weigh 4200 g of flaky aluminum oxide and 1800 g of calcined kaolin in a mixer, mix by ball milling for 24 h, then transfer the powder to a blender, add 1470 g of hot melted paraffin, 200 g of beeswax and 32 g of oleic acid, mix and stir for 4 hours to obtain a ceramic slurry;

[0056] (2) The ceramic slurry obtained in step (1) was transferred into a hot molding machine, and vacuum was started and stirred for 30 minutes. After completion, the hot pressing pressure was adjusted to 0.6 MPa and the holding time was 15 seconds to obtain a sample green body.

[0057] (3) The ceramic green body obtained in step (2) is buried and then sent into a kiln for firing at a temperature of 1300° C. After firing, the sample is vibrated and sorted to obtain a fired sample.

[0058] (4) The ceramic block obtained in step (3) is surface-polished to remove the powder adhering to the surface to obtain a finished product.

[0059] Finally, a porous ceramic block with a porosity of 51% was obtained according to the above steps. The ceramic block was immersed in the fragrance liquid for 24 hours, and its weight fragrance absorption rate could reach about 25%.

[0060] Embodiment 3:

[0061] (1) 3750 g of flaky aluminum oxide and 2250 g of calcined kaolin were weighed in a mixer, and the mixture was ball-milled for 24 h. The powder was then transferred to a blender, and 1470 g of hot melted paraffin, 200 g of beeswax, and 32 g of oleic acid were added. The mixture was mixed and stirred for 4 h to obtain a ceramic slurry.

[0062] (2) The ceramic slurry obtained in step (1) was transferred into a hot molding machine, and vacuum was started and stirred for 30 minutes. After completion, the hot pressing pressure was adjusted to 0.6 MPa and the holding time was 15 seconds to obtain a sample green body.

[0063] (3) The ceramic green body obtained in step (2) is buried and then sent into a kiln for firing at a temperature of 1250° C. After firing, the sample is vibrated and sorted to obtain a fired sample.

[0064] (4) The ceramic block obtained in step (3) is surface-polished to remove the powder adhering to the surface to obtain a finished product.

[0065] Finally, a porous ceramic block with a porosity of 51% was obtained according to the above steps. The ceramic block was immersed in the fragrance liquid for 24 hours, and its weight fragrance absorption rate could reach about 25%.

[0066] In order to meet the needs of high-end users for colored ceramic carriers. The prior art usually dyes the finished scented ceramics to maintain the porosity and aroma absorption capacity of the original color ceramics, but the dye will gradually decompose with the increase of use time. The present invention adds colorants to the raw materials, which not only ensures uniform color mixing, but also does not affect the porosity and aroma absorption rate of the ceramic material during the sintering process.

[0067] Specifically, the mass ratio of the colorant to the sum of the mass of flaky alumina and calcined kaolin is 1% to 10%, which can be adjusted according to the actual color requirements; the mixing method can be selected: directly adding the colorant and other raw materials to the wax slurry and stirring and mixing, using a mixer to mix by ball milling, wet ball milling, drying after ball milling, and pulverizing to make pulp. Among them, the wet ball milling method is the most uniform colorant mixing, but the most complicated; direct mixing of the slurry is the most convenient, but the colorant is prone to uneven mixing. The time for mixing each colorant with the powder should be guaranteed to be 12h to 24h, and the specific implementation is shown in Examples 4 and 5.

[0068] Embodiment 4:

[0069] (1) 300 g of colorant, 3135 g of flaky alumina, and 2565 g of calcined kaolin were weighed in a mixer and ball-milled for 24 h. The colorant accounted for 10% of the powder. The powder was then transferred to a mixer, and 1500 g of hot melted paraffin, 200 g of beeswax, and 32 g of oleic acid were added. The mixture was mixed and stirred for 4 hours to obtain a ceramic slurry.

[0070] (2) The ceramic slurry obtained in step (1) was transferred into a hot molding machine, and vacuum was started and stirred for 30 minutes. After completion, the hot pressing pressure was adjusted to 0.6 MPa and the holding time was 15 seconds to obtain a sample green body.

[0071] (3) The ceramic green body obtained in step (2) is buried and then sent into a kiln for firing at a temperature of 1250° C. After firing, the sample is vibrated and sorted to obtain a fired sample.

[0072] (4) The ceramic block obtained in step (3) is surface-polished to remove the powder adhering to the surface to obtain a finished product.

[0073] Finally, a colorful porous ceramic block with a porosity of 46% was obtained according to the above steps. The ceramic block was immersed in the fragrance liquid for 24 hours, and its weight fragrance absorption rate could reach about 25%.

[0074] Embodiment 5:

[0075] (1) Weigh 600 g of colorant, 2970 g of flaky alumina, and 2430 g of calcined kaolin in a mixer, and mix them by ball milling for 24 hours. The colorant accounts for 10% of the powder. Then, the powder is transferred to a mixer, and 1500 g of hot melted paraffin, 200 g of beeswax, and 32 g of oleic acid are added. The mixture is mixed and stirred for 4 hours to obtain a ceramic slurry.

[0076] (2) The ceramic slurry obtained in step (1) was transferred into a hot molding machine, and vacuum was started and stirred for 30 minutes. After completion, the hot pressing pressure was adjusted to 0.6 MPa and the holding time was 15 seconds to obtain a sample green body.

[0077] (3) The ceramic green body obtained in step (2) is buried and then sent into a kiln for firing at a temperature of 1300° C. After firing, the sample is vibrated and sorted to obtain a fired sample.

[0078] (4) The ceramic block obtained in step (3) is surface-polished to remove the powder adhering to the surface to obtain a finished product.

[0079] Finally, a colorful porous ceramic block with a porosity of 45% was obtained according to the above steps. The ceramic block was immersed in the fragrance liquid for 24 hours, and its weight fragrance absorption rate could reach about 25%.

[0080] Comparative Example 1:

[0081] (1) Weighing 3300 g of another type of alumina (in granular form with a median diameter of 2.1 μm) and 2700 g of calcined kaolin, placing them in a blender, adding 1470 g of hot melted paraffin, 200 g of beeswax and 32 g of oleic acid, mixing and stirring for 4 hours to obtain a ceramic slurry;

[0082] (2) The ceramic slurry obtained in step (1) was transferred into a hot molding machine, and vacuum was started and stirred for 30 minutes. After completion, the hot pressing pressure was adjusted to 0.6 MPa and the holding time was 15 seconds to obtain a sample green body.

[0083] (3) The ceramic green body obtained in step (2) is buried and then sent into a kiln for firing at a temperature of 1300° C. After firing, the sample is vibrated and sorted to obtain a fired sample.

[0084] (4) The ceramic block obtained in step (3) is surface-polished to remove the powder adhering to the surface to obtain a finished product.

[0085] Finally, a porous ceramic block with a porosity of 42% was obtained. When the ceramic block was soaked in fragrance liquid for 24 hours, its weight fragrance absorption rate could reach about 20%.

[0086] Comparative Example 2:

[0087] (1) 300 g of each colorant, 3300 g of another type of alumina (granular in shape, with a median diameter of 2.1 μm), and 2700 g of calcined kaolin were weighed and placed in a blender, and 1470 g of hot melted paraffin, 200 g of beeswax, and 32 g of oleic acid were added, and the mixture was mixed and stirred for 4 hours to obtain a ceramic slurry;

[0088] (2) The ceramic slurry obtained in step (1) was transferred into a hot molding machine, and vacuum was started and stirred for 30 minutes. After completion, the hot pressing pressure was adjusted to 0.6 MPa and the holding time was 15 seconds to obtain a sample green body.

[0089] (3) The ceramic green body obtained in step (2) is buried and then sent into a kiln for firing at a temperature of 1300° C. After firing, the sample is vibrated and sorted to obtain a fired sample.

[0090] (4) The ceramic block obtained in step (3) is surface-polished to remove the powder adhering to the surface to obtain a finished product.

[0091] Finally, a porous ceramic block with a porosity of 41% was obtained. When the ceramic block was soaked in fragrance liquid for 24 hours, its weight fragrance absorption rate could reach about 19%.

[0092] Test: The porosity, density, fragrance absorption rate, and fragrance release rate of the finished products obtained in the embodiment and the comparative example were measured and compared, and the test data are shown in the table. Among them: the porosity, density, etc. are measured in accordance with the national standard GB / T 25995-2010 "Test Method for Density and Apparent Porosity of Fine Ceramics", and the pore size is measured using the mercury intrusion method; the fragrance absorption rate is calculated by the fragrance absorption after the ceramic block is completely immersed in the fragrance liquid for 24 hours, and the fragrance weight loss rate is calculated by the weight loss of the fragrance liquid after simulating the installed fan test for 180 hours.

[0093] Table 1

[0094] sample Porosity Bulk density g / cm3 Colorant addition% Weight aroma absorption rate % Installation test fragrance weightlessness Example 1 48.65% 1.667 0% 26.29% 23.42% Example 2 50.80% 1.697 0% 26.97% 23.63% Example 3 50.63% 1.653 0% 26.53% 23.89% Example 4 48.43% 1.760 5% 25.53% 24.75% Example 5 42.86% 1.988 10% 22.29% 27.93% Comparative Example 1 46.02% 1.815 0% 20.17% 32.40% Comparative Example 2 34.22% 2.102 5% 15.31% 35.79%

[0095] It can be seen from Table 1 that after the raw materials with different particle sizes and morphologies were replaced in the comparative example, the porosity of the ceramic blocks prepared at the same organic content was still reduced. It can be seen that the particle size and morphology of the material will directly affect the porosity of the colored ceramic.

[0096] The colored porous ceramics in Examples 1 to 5 are adjusted in terms of the colorant ratio and powder ratio, and the final porosity can reach 45% or above. Under the installed simulation test, the final fragrance meets customer needs, and the weight loss is low, and the fragrance retention ability is stronger. The color depth can also be adjusted according to needs. The color of the sample can be adjusted by adjusting the amount of colorant. Although the porosity is slightly affected, the final test results show that the performance difference is not large. In Comparative Examples 1 and 2, after replacing other materials, the porosity of the ceramic block is significantly reduced, resulting in a decrease in the fragrance absorption rate in the same time. At the same time, the final fragrance loses more weight and the fragrance retention ability becomes worse.

[0097] For matters not mentioned above, the prior art applies.

[0098] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a fragrance sustained-release ceramic material, characterized in that: The steps include: S1. Mix the weighed flaky alumina and calcined kaolin powder evenly; S2, heating and stirring the above powder, adding hot melted liquid paraffin and additives, and stirring for a period of time to obtain a ceramic slurry; S3, vacuuming, stirring, and hot-pressing the prepared ceramic slurry to obtain a ceramic green body; S4, burying the ceramic green body in alumina sintered powder, and then putting it into a kiln for firing, taking out the buried and fired ceramic block after cooling, and then performing surface treatment; S5, soaking the processed ceramic block in fragrance, and packaging the ceramic block after the surface is dried.

2. The method for preparing a fragrance sustained-release ceramic material according to claim 1, characterized in that: The step S1 further includes a colorant, wherein the mass of the colorant is 1% to 10% of the sum of the mass of the colorant, flaky alumina and calcined kaolin; and\or, The pigment is a metallic mineral phase pigment.

3. The method for preparing a fragrance slow-release ceramic material according to claim 1, characterized in that: The median diameter of the flaky aluminum oxide is between 3 and 30 μm, and the width-to-thickness ratio is between 1 and 10; the median diameter of the calcined kaolin is between 1 and 3 μm.

4. The method for preparing a fragrance slow-release ceramic material according to claim 1, characterized in that: In the ceramic slurry, the mass ratio of flaky alumina, calcined kaolin, paraffin wax and additives is 40-60:20-40:15-20:1-5.

5. The method for preparing a fragrance slow-release ceramic material according to claim 1, characterized in that: In step S2, the heating temperature is 65°C to 90°C, and the stirring time is 4 to 8 hours.

6. The method for preparing a fragrance slow-release ceramic material according to claim 1, characterized in that: The additive is beeswax, stearic acid or oleic acid.

7. The method for preparing a fragrance slow-release ceramic material according to claim 1, characterized in that: The specific operation of step S3 is: adding the prepared ceramic slurry to the molding machine, setting the temperature at 60°C to 75°C, evacuating and stirring for 10 to 300 minutes, and then hot-pressing and molding, with a pressure between 0.4 and 0.8 MPa and a holding time of 5s to 30s.

8. The method for preparing a fragrance slow-release ceramic material according to claim 1, characterized in that: In step S4, the primary firing temperature is controlled between 1200 and 1400°C.

9. The method for preparing a fragrance slow-release ceramic material according to claim 1, characterized in that: After the firing is completed, the product is first subjected to vibration screening to remove the buried burning powder, and then the surface of the product is polished to remove the adhering powder particles; and\or, the incense soaking method adopts the method of soaking or\and incense injection.

10. A fragrance slow-release ceramic material, wherein the fragrance slow-release ceramic material is prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of porous Al2O3 ceramic

    CN101844934A

  • Porous ceramic material and preparation method thereof

    CN111574203A

  • Durable fragrant ceramic decorative plate and preparation method thereof

    CN111807861A

  • Preparation of ceramic sintered product

    JP1990267175A

  • Porous ceramic body and production thereof

    JP1992092873A