Super-soft ionic liquid conductive self-repairing polyurethane elastomer and preparation method thereof

By forming irreversible covalent crosslinking points in polyurethane materials and adding ionic liquids, the limitations of traditional stretchable materials in terms of electrical conductivity, elasticity and self-repairability are solved, and efficient self-repair and improvement of electrical conductivity at room temperature is achieved. , suitable for flexible electrical sensor parts.

CN119039561AActive Publication Date: 2024-11-29BEIJING INST OF TECH
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411173781.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Existing stretchable electronic materials have limitations in terms of tensileability and self-healing properties. Traditional conductors cannot be restored after breaking, and the addition of conductive fillers will lead to the deterioration of the material's mechanical properties, making it difficult to have both conductivity, good elasticity and flexibility. and self-healing ability.

Method used

Ultra-flexible ionic liquid conducting self-healing polyurethane elastomer is used to form irreversible covalent chemical crosslinking points through polyurethane and polyether 330N, and ionic liquid is added through surface modification to ensure the stability of the conductive and mechanical properties of the material.

Benefits of technology

It realizes efficient self-repair of the material at room temperature, restores tensile strength by 60%, and can detect electrical signals under both large and small strains. It is suitable for flexible electrical sensor parts, improving the mechanical properties and application range of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039561A_ABST
    Figure CN119039561A_ABST
Patent Text Reader

Abstract

The invention relates to a super-soft ionic liquid conductive self-repairing polyurethane elastomer and a preparation method thereof, and belongs to the field of medical care, and the super-soft ionic liquid conductive self-repairing polyurethane elastomer is conductive, good in flexibility and capable of self-repairing materials at normal temperature. The material is low in Young modulus and has good elasticity and flexibility. The material can realize high-efficiency self-repairing under a room-temperature mild condition, and the tensile strength of the material can be recovered to 60% of the initial tensile strength. Besides, the elastomer material has excellent conductivity, can detect electric signals under large strain and small strain, and can be applied to flexible electric sensing devices. Wherein the prepolymer and the polyether 330N form an irreversible covalent chemical crosslinking point, so that the mechanical property of the polyurethane elastomer is improved; and the cross-linked structure can improve the structural stability, so that the mechanical property stability of the ionic liquid surface modified conductive self-repairing polyurethane is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an ultra-soft ionic liquid conductive self-repairing polyurethane elastomer and a preparation method thereof, belonging to the technical field of medical care. The ultra-soft ionic liquid conductive self-repairing polyurethane elastomer is conductive, has a low Young's modulus, has good elasticity and flexibility, and can self-repair the material at room temperature. Background Art

[0002] Stretchable electronic materials and devices have attracted widespread attention due to their important applications in many fields, especially in healthcare. For example, stretchable strain sensors can be used to monitor body movements, and stretchable conductors can be used as epidermal electrodes for biopotential detection. Stretchable strain sensors are usually made of elastomeric composites and nano-conductive fillers, such as carbon nanotubes, graphene, or metal nanomaterials, which are often used as conductive fillers in stretchable composites. The stretchability of traditional conductors is very limited, and they are much harder than soft human skin.

[0003] However, traditional materials use irreversible covalent bonds inside, which cannot be restored once broken, and self-repair is difficult. Self-healing materials can spontaneously repair physical damage and restore mechanical properties to extend their service life. Most healing materials cannot conduct electricity. If conductive fillers are added, the mechanical properties of the materials will deteriorate. Therefore, developing a polyurethane that is conductive, has good elasticity and flexibility, and can self-repair at room temperature is of great significance to improving the mechanical properties and application range of materials. Summary of the invention

[0004] The technical solution of the present invention is to overcome the defects in the prior art, propose a super-soft ionic liquid conductive self-healing polyurethane elastomer and a preparation method thereof, wherein polyurethane and polyether 330N form irreversible covalent chemical crosslinking points, improve the overall performance of the polyurethane elastomer, and add ionic liquids through surface modification to ensure the stability of the structure and mechanical properties of the super-soft ionic liquid conductive self-healing polyurethane elastomer. The material has excellent conductivity, and electrical signals can be detected under large and small strains, and can be applied to flexible electrical sensor devices.

[0005] The objectives of the present invention are achieved through the following technical solutions.

[0006] A super-soft ionic liquid conductive self-healing polyurethane elastomer, the raw materials of which include component A, component B and component C, and also include isopropanol, a toluene solution of di-n-butylamine, a bromocresol blue indicator, 0.1 mol / L dilute hydrochloric acid, and an organic solvent;

[0007] Taking the mass of component A as 100%, the mass percentages of the components in component A are as follows:

[0008] Hexamethylene diisocyanate (HDI) 37% to 39%;

[0009] Polybutylene glycol (PTMG) 61% to 63%;

[0010] Taking the mass of component B as 100%, the mass percentages of the components in component B are as follows:

[0011] Polybutylene glycol (PTMG) 87.6% to 91.6%;

[0012] Polyether 330N polyol (330N) 6.7% to 10.7%;

[0013] 4,4'-dihydroxydiphenyl disulfide 0.7% to 2.7%;

[0014] Taking the mass of the C component as 100%, the mass percentages of the components in the C component are:

[0015] Choline chloride 42%-44%;

[0016] Glycerol 56%-58%;

[0017] The organic solvent is N,N-dimethylformamide;

[0018] The molecular weight of the polybutylene glycol is 1760-2080;

[0019] The molecular weight of the polyether 330N polyol is 4600-4800;

[0020] The polybutylene glycol, hexamethylene diisocyanate and polyether 330N polyol need to be dehydrated.

[0021] A method for preparing an ultra-soft ionic liquid conductive self-healing polyurethane elastomer, the method comprising the steps of:

[0022] In the first step, hexamethylene diisocyanate (HDI) and polytetramethylene glycol (PTMG) in component A are dehydrated and then mixed, nitrogen environment protection is performed during mixing, and then the temperature is raised to 80-85° C., and stirred for reaction for 4-5 hours to obtain a polyurethane prepolymer at a stirring speed of 180-220 r / min;

[0023] The second step is to mix a portion of the polyurethane prepolymer obtained in the first step with isopropanol in a water bath environment at 45-55° C., with a mixing volume of L and a mixing time of 10-15 min, and then add a toluene solution of di-n-butylamine and a bromocresol blue indicator, and then titrate with 0.1 mol / L dilute hydrochloric acid until the solution no longer changes color within 30 seconds, and then terminate the titration. After the titration is completed, calculate the isocyanate content a in the polyurethane prepolymer;

[0024] The ratio of the polyurethane prepolymer to isopropanol is 3-4 g:500 mL;

[0025] The volume ratio of the mixed volume L of the polyurethane prepolymer and isopropanol to the toluene solution of di-n-butylamine is 2:1;

[0026] The ratio of the volume L of the polyurethane prepolymer and isopropanol after mixing to the bromocresol blue indicator is 1000mL:1g;

[0027] The ratio of the mass (g) of di-n-butylamine to the volume (ml) of solvent toluene is 129g:166ml;

[0028] In the third step, the polytetramethylene glycol (PTMG) and polyether 330N polyol (330N) in component B are dehydrated;

[0029] The fourth step is to dissolve the 4,4'-dihydroxydiphenyl disulfide in the B component in an organic solvent, and then mix it with a portion of the polyurethane prepolymer obtained in the first step, the dehydrated polytetramethylene glycol (PTMG) in the B component, and the polyether 330N polyol (330N), and the mixing temperature is 30-50°C;

[0030] The fifth step is to stir the mixed material in the fourth step at a speed of 1900-2100 r / min for 10-15 seconds, pour it into a polytetrafluoroethylene mold, cure it at 75-85° C. for 48 hours, and then dry it in a vacuum oven at 75-85° C. for 48 hours to remove the organic solvent, thereby obtaining a polyurethane elastomer;

[0031] Step 6: Mix the choline chloride and glycerol in the C material, heat to 95-105° C., and stir to dissolve for 2-3 hours to obtain an ionic liquid;

[0032] In the seventh step, the polyurethane elastomer prepared in the fifth step is immersed in an organic solvent for 10-20 minutes, and then the ionic liquid is evenly coated on the surface of the self-healing polyurethane substrate, and then dried in a forced air oven at 80°C for 6 hours to obtain an ultra-soft ionic liquid conductive self-healing polyurethane elastomer.

[0033] In the fourth step, the ratio of 4,4'-dihydroxydiphenyl disulfide, polyurethane prepolymer, polytetramethylene glycol (PTMG), and polyether 330N polyol satisfies:

[0034] (m1×a%) / 42=R×((m2 / N1)×2+(m3 / N2)×3+(m4 / N3)×2)

[0035] Wherein, m1 is the mass of polyurethane prepolymer, m2 is the mass of polytetramethylene glycol (PTMG), m3 is the mass of polyether 330N polyol, and m4 is the mass of 4,4' dihydroxy diphenyl disulfide;

[0036] N1, is the molecular weight of polytetramethylene glycol (PTMG);

[0037] N2 is the molecular weight of polyether 330N polyol;

[0038] N3 is the molecular weight of 4,4' dihydroxydiphenyl disulfide;

[0039] The value of the isocyanate group in the polyurethane prepolymer is defined as R1, and the sum of the hydroxyl groups in 4,4'-dihydroxydiphenyl disulfide, polytetramethylene glycol (PTMG) and polyether 330N polyol is R2, then R=R1 / R2, R=1.04-1.06.

[0040] Beneficial Effects

[0041] (1) The present invention provides an ultra-soft ionic liquid conductive self-healing polyurethane elastomer and a preparation method thereof, wherein the ultra-soft ionic liquid conductive self-healing polyurethane elastomer is a new type of high-performance conductive polyurethane elastomer. The material has a low Young's modulus and good elasticity and flexibility. The material can achieve efficient self-healing at room temperature and mild conditions, and its tensile strength can recover 60% of the initial value. In addition, the elastomeric material has excellent electrical conductivity, and electrical signals can be detected under large and small strains, and can be applied to flexible electrical sensor devices. The prepolymer and polyether 330N form irreversible covalent chemical cross-linking points to improve the mechanical properties of the polyurethane elastomer; and this cross-linking structure can improve its structural stability, thereby ensuring the mechanical property stability of the ultra-soft ionic liquid conductive self-healing polyurethane elastomer.

[0042] (2) The present invention provides a method for preparing an ultra-soft ionic liquid conductive self-healing polyurethane elastomer. In the method, both ends of hexamethylene diisocyanate (HDI) in material A contain isocyanate groups, and both ends of polytetramethylene glycol (PTMG) contain hydroxyl groups. After the preliminary synthesis of the prepolymer, the two can be polymerized with material B at room temperature to produce a polyurethane elastomer, and then the finished product can be obtained by evaporating the solvent. The method has simple steps, and the experimental formula can be changed according to production needs, so it can be industrially produced.

[0043] (3) The present invention provides a method for preparing an ultra-soft ionic liquid conductive self-healing polyurethane elastomer. The key to preserving the prepolymer is to maintain the preheating temperature of 50°C or below. The prepolymer will self-polymerize at a temperature of 50 to 70°C. Both ends of the prepolymer are capped with isocyanate (-NCO) and tend to polymerize with hydroxyl groups in chain extenders, crosslinkers and other components in the main raw materials at room temperature. This polymerization method can promote the forward reaction and accelerate the reaction rate. The produced material has excellent conductivity, and electrical signals can be detected under large and small strains, and can be applied to flexible electrical sensor devices.

[0044] (4) The present invention provides a method for preparing an ultra-soft ionic liquid conductive self-healing polyurethane elastomer. The method uses a specific organic solvent (such as N,N-dimethylformamide, dimethyl sulfoxide and chloroform, etc.) for the following purposes: first, to reduce the viscosity of the reaction system; second, to dissolve disulfide compounds and successfully introduce the disulfide compounds into the polyurethane elastomer system.

[0045] (5) The ultra-soft ionic liquid conductive self-healing polyurethane elastomer of the present invention is a new type of high-performance aging-resistant polyurethane elastomer, which forms chemical crosslinks with polyether 330N, can increase the crosslinking density and improve the mechanical properties of the polyurethane elastomer; and this crosslinking structure can improve its structural stability, thereby ensuring the mechanical property stability of the ultra-soft ionic liquid conductive self-healing polyurethane elastomer. The present invention also provides a method for preparing an ultra-soft ionic liquid conductive self-healing polyurethane elastomer, which introduces ionic liquid into the polyurethane elastomer system by surface modification to generate an ultra-soft ionic liquid conductive self-healing polyurethane elastomer. This method has simple steps, is relatively safe and environmentally friendly, and the experimental formula can be changed according to production needs, and can be industrially produced.

[0046] (6) The present invention relates to a conductive self-healing polyurethane modified by an ionic liquid surface and a preparation method thereof, which belongs to the field of medical care, is conductive, has good flexibility, and can self-repair the material at room temperature. The material has a low Young's modulus and has good elasticity and flexibility. The material can achieve efficient self-repair at room temperature and mild conditions, and its tensile strength can recover 60% of the initial value. In addition, the elastomeric material has excellent electrical conductivity, and electrical signals can be detected under large and small strains, and can be applied to flexible electrical sensor devices. The prepolymer and polyether 330N form irreversible covalent chemical cross-linking points, thereby improving the mechanical properties of the polyurethane elastomer; and this cross-linking structure can improve its structural stability, thereby ensuring the mechanical property stability of the conductive self-healing polyurethane modified by the ionic liquid surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is the infrared spectrum of the ultra-soft ionic liquid conductive self-healing polyurethane elastomer;

[0048] Figure 2 This is the room temperature self-healing result diagram of the ultra-soft ionic liquid conductive self-healing polyurethane elastomer;

[0049] Figure 3 This is the result diagram of large strain electrical signal of ultra-soft ionic liquid conductive self-healing polyurethane elastomer;

[0050] Figure 4 This is the small strain electrical signal result diagram of the ultra-soft ionic liquid conductive self-healing polyurethane elastomer. DETAILED DESCRIPTION

[0051] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments, but this is not intended to limit the present invention.

[0052] Example 1

[0053] A super-soft ionic liquid conductive self-healing polyurethane elastomer, the super-soft ionic liquid conductive self-healing polyurethane elastomer is composed of three raw material components A, B, and C. Taking the total mass of each of the raw materials A, B, and C as 100%, the components and their mass fractions in the raw material A are as follows: hexamethylene diisocyanate (HDI) 37% to 39%, polytetramethylene glycol (PTMG) 61% to 63%; the components and their mass fractions in the raw material B are as follows: polytetramethylene glycol (PTMG) TMG) 87.6% to 91.6%, polyether 330N polyol (330N) 6.7% to 10.7%; 4,4'-dihydroxydiphenyl disulfide 0.7% to 2.7%; the components and their mass fractions in the C raw material are as follows: choline chloride 42% to 44%, glycerol 56% to 58%; the auxiliary raw materials are organic solvents (such as N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, etc.) and indicators bromocresol blue and di-n-butylamine in toluene solution.

[0054] The molecular weight of the polybutylene glycol is 1760-2080, the molecular weight of the polyether 330N polyol is 4600-4800, and the chain extender is an N,N-dimethylformamide solution of polybutylene glycol and 4,4'-dihydroxydiphenyl disulfide.

[0055] The mass ratio of hexamethylene diisocyanate and polybutylene glycol used in the synthetic polyurethane prepolymer is 3:5.

[0056] The ratio of the mass (g) of the polyurethane prepolymer sample to be titrated to the volume (mL) of the isopropanol solvent is (3-4):500; the ratio of the mass (g) of the di-n-butylamine to the volume (mL) of the toluene solvent is 129:166; the volume ratio of the titration sample solution to the toluene solution of di-n-butylamine is 2:1; the ratio of the mass (g) of the indicator bromocresol blue to the volume (mL) of the solution is 1:1000;

[0057] A method for preparing the ultra-soft ionic liquid conductive self-healing polyurethane elastomer described in this embodiment, the specific steps of the method are as follows:

[0058] (1) 60 g of hexamethylene diisocyanate and 100 g of polybutylene glycol were added to a 250 mL three-necked flask, and the temperature was raised to 80° C. The raw materials were stirred at a rate of 200 r / min to mix them evenly, and the polyurethane prepolymer was obtained after reacting for 4 h;

[0059] (2) 0.3921 g of the prepolymer obtained in step (1) was dissolved in 50 mL of a toluene solution of di-n-butylamine, and heated at 50° C. for 10 min to fully dissolve it. Four drops of bromocresol blue indicator were added, and then 25 mL of isopropanol was added to completely dissolve the indicator. The isocyanate content in the prepolymer was determined to be 17.4% by titration using 0.1036 mol / L dilute hydrochloric acid.

[0060] The ratio of the mass (g) of bromocresol blue in the bromocresol blue indicator to the volume (mL) of the solvent sodium hydroxide is 1:1000, and the concentration of the sodium hydroxide is 0.1 mol / L;

[0061] (3) preheating the main raw materials of dehydrated polybutylene glycol and polyether 330N polyol to 70° C., and dissolving 1.9702 g of 4,4'-dihydroxydiphenyl disulfide in N,N-dimethylformamide solution in advance;

[0062] (4) Add 103.339 g of polybutylene glycol, 10.21 g of polyether 330N polyol and an N,N-dimethylformamide solution containing 1.9702 g of 4,4'-dihydroxydiphenyl disulfide in step (3) into a container in sequence, then add 33.8945 g of the prepolymer and stir the solution at a stirring rate of 2000 r / min for 60 s; pour into a polytetrafluoroethylene container and place in an oven at 70° C. for curing for 48 h, and then dry in a vacuum oven at 80° C. for 24 h to remove the organic solvent, thereby obtaining a polyurethane elastomer.

[0063] (5) 10 g of choline chloride and 13 g of glycerol were stirred at 100 °C and 400 rpm for 2 h to obtain an ionic liquid.

[0064] (6) Soak the prepared polyurethane elastomer in 100 ml of N,N-dimethylformamide for 20 min, then evenly coat 1 ml of ionic liquid on the surface of the self-healing polyurethane substrate, let it stand for 30 min, and then dry it in a forced air oven at 80 ° C for 6 h to obtain an ultra-soft ionic liquid conductive self-healing polyurethane elastomer;

[0065] The obtained elastomer was analyzed by infrared spectroscopy. Figure 1 As shown by Figure 1 It can be seen that at 3340cm -1 The peak of -NH- stretching vibration appeared at 1720 cm -1 The peak of -CO- stretching vibration appeared at 453 cm -1 A peak of -SS- vibration appears.

[0066] The obtained elastomer was subjected to large strain electrical signal test. The results are as follows Figure 2When the stretching rate reaches 200%, electrical signals can be detected in the range of 0.015mA to 0.018mA, indicating that the elastomer can conduct electricity under large strain.

[0067] The obtained elastomer was subjected to small strain electrical signal test. The results are as follows Figure 3 When the stretching rate reaches 120%, electrical signals can be detected in the range of 0.006mA to 0.007mA, indicating that the elastomer can conduct electricity under small strain.

[0068] The obtained elastic body was cut and then spliced, and a tensile test was performed after repairing at room temperature for 1 hour. The results are as follows: Figure 4 As shown, since the chemical cross-linking points are cut off during the cutting process, the elongation at break is difficult to recover to that of the initial sample, but its tensile strength is basically restored to 55% of the original.

[0069] Example 2

[0070] A super-soft ionic liquid conductive self-healing polyurethane elastomer, the super-soft ionic liquid conductive self-healing polyurethane elastomer is composed of three raw material components A, B, and C. Taking the total mass of each of the raw materials A, B, and C as 100%, the components and their mass fractions in the raw material A are as follows: hexamethylene diisocyanate (HDI) 37% to 39%, polytetramethylene glycol (PTMG) 61% to 63%; the components and their mass fractions in the raw material B are as follows: polytetramethylene glycol (PTMG) TMG) 87.6% to 91.6%, polyether 330N polyol (330N) 6.7% to 10.7%; 4,4'-dihydroxydiphenyl disulfide 0.7% to 2.7%; the components and their mass fractions in the C raw material are as follows: choline chloride 42% to 44%, glycerol 56% to 58%; the auxiliary raw materials are organic solvents (such as N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, etc.) and indicators bromocresol blue and di-n-butylamine in toluene solution.

[0071] The molecular weight of the polybutylene glycol is 1760-2080, the molecular weight of the polyether 330N polyol is 4600-4800, and the chain extender is an N,N-dimethylformamide solution of polybutylene glycol and 4,4'-dihydroxydiphenyl disulfide.

[0072] The mass ratio of hexamethylene diisocyanate and polybutylene glycol used in the synthetic polyurethane prepolymer is 3:5.

[0073] The ratio of the mass (g) of the polyurethane prepolymer sample to be titrated to the volume (mL) of the isopropanol solvent is (3-4):500; the ratio of the mass (g) of the di-n-butylamine to the volume (mL) of the toluene solvent is 129:166; the volume ratio of the titration sample solution to the toluene solution of di-n-butylamine is 2:1; the ratio of the mass (g) of the indicator bromocresol blue to the volume (mL) of the solution is 1:1000;

[0074] A method for preparing the ultra-soft ionic liquid conductive self-healing polyurethane elastomer described in this embodiment, the specific steps of the method are as follows:

[0075] (1) 60 g of hexamethylene diisocyanate and 100 g of polybutylene glycol were added to a 250 mL three-necked flask, and the temperature was raised to 80° C. The raw materials were stirred at a rate of 200 r / min to mix them evenly, and the polyurethane prepolymer was obtained after reacting for 4 h;

[0076] (2) 0.3945 g of the prepolymer obtained in step (1) was dissolved in 50 mL of a toluene solution of di-n-butylamine, and heated at 50° C. for 10 min to fully dissolve it. Four drops of bromocresol blue indicator were added, and then 25 mL of isopropanol was added to completely dissolve the indicator. The isocyanate content in the prepolymer was determined to be 16.9% by titration using 0.1036 mol / L dilute hydrochloric acid.

[0077] The ratio of the mass (g) of bromocresol blue in the bromocresol blue indicator to the volume (mL) of the solvent sodium hydroxide is 1:1000, and the concentration of the sodium hydroxide is 0.1 mol / L;

[0078] (3) preheating the main raw materials of polybutylene glycol and polyether 330N polyol after dehydration to 70° C., and dissolving 1.9689 g of 4,4'-dihydroxydiphenyl disulfide in N,N-dimethylformamide solution in advance;

[0079] (4) Add 101.267 g of polybutylene glycol, 9.76 g of polyether 330N polyol and N,N-dimethylformamide solution containing 1.9689 g of 4,4'-dihydroxydiphenyl disulfide in step (3) into a container in sequence, then add 33.8762 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 60 seconds; pour into a polytetrafluoroethylene container and place in an oven at 70°C for curing for 48 hours, then dry in a vacuum oven at 80°C for 24 hours to remove the organic solvent, to obtain a polyurethane elastomer.

[0080] (5) 10 g of choline chloride and 13 g of glycerol were stirred at 100 °C and 400 rpm for 2 h to obtain an ionic liquid.

[0081] (6) The prepared polyurethane elastomer was placed in 100 ml of N,N-dimethylformamide and soaked for 20 minutes. Then, 1 ml of ionic liquid was evenly coated on the surface of the self-healing polyurethane substrate, left to stand for 30 minutes, and then dried in a forced air oven at 80°C for 6 hours to obtain an ultra-soft ionic liquid conductive self-healing polyurethane elastomer.

[0082] The obtained elastomer was subjected to infrared spectroscopy analysis. -1The peak of -NH- stretching vibration appeared at 1722 cm -1 The peak of -CO- stretching vibration appeared at 451cm -1 A peak of -SS- vibration appears.

[0083] The obtained elastomer was subjected to a large strain electrical signal test. When the stretching rate reached 220%, electrical signals could be detected in the range of 0.015 mA to 0.018 mA, indicating that the elastomer can conduct electricity under large strain.

[0084] The obtained elastomer was subjected to a small strain electrical signal test. When the stretching rate reached 100%, electrical signals could be detected in the range of 0.006 mA to 0.007 mA, indicating that the elastomer can conduct electricity under small strain.

[0085] The obtained elastomer was cut and then spliced, and then repaired at room temperature for 1 hour before a tensile test. Since the chemical cross-linking points were cut off during the cutting process, the elongation at break was difficult to recover to that of the initial sample, but its tensile strength was basically restored to 57% of the original.

[0086] Example 3

[0087] A super-soft ionic liquid conductive self-healing polyurethane elastomer, the super-soft ionic liquid conductive self-healing polyurethane elastomer is composed of three raw material components A, B, and C. Taking the total mass of each of the raw materials A, B, and C as 100%, the components and their mass fractions in the raw material A are as follows: hexamethylene diisocyanate (HDI) 37% to 39%, polytetramethylene glycol (PTMG) 61% to 63%; the components and their mass fractions in the raw material B are as follows: polytetramethylene glycol (PTMG) TMG) 87.6% to 91.6%, polyether 330N polyol (330N) 6.7% to 10.7%; 4,4'-dihydroxydiphenyl disulfide 0.7% to 2.7%; the components and their mass fractions in the C raw material are as follows: choline chloride 42% to 44%, glycerol 56% to 58%; the auxiliary raw materials are organic solvents (such as N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, etc.) and indicators bromocresol blue and di-n-butylamine in toluene solution.

[0088] The molecular weight of the polybutylene glycol is 1760-2080, the molecular weight of the polyether 330N polyol is 4600-4800, and the chain extender is an N,N-dimethylformamide solution of polybutylene glycol and 4,4'-dihydroxydiphenyl disulfide.

[0089] The mass ratio of hexamethylene diisocyanate and polybutylene glycol used in the synthetic polyurethane prepolymer is 3:5.

[0090] The ratio of the mass (g) of the polyurethane prepolymer sample to be titrated to the volume (mL) of the isopropanol solvent is (3-4):500; the ratio of the mass (g) of the di-n-butylamine to the volume (mL) of the toluene solvent is 129:166; the volume ratio of the titration sample solution to the toluene solution of di-n-butylamine is 2:1; the ratio of the mass (g) of the indicator bromocresol blue to the volume (mL) of the solution is 1:1000;

[0091] A method for preparing the ultra-soft ionic liquid conductive self-healing polyurethane elastomer described in this embodiment, the specific steps of the method are as follows:

[0092] (1) 60 g of hexamethylene diisocyanate and 100 g of polybutylene glycol were added to a 250 mL three-necked flask, and the temperature was raised to 80° C. The raw materials were stirred at a rate of 200 r / min to mix them evenly, and the polyurethane prepolymer was obtained after reacting for 4 h;

[0093] (2) 0.3876 g of the prepolymer obtained in step (1) was dissolved in 50 mL of a toluene solution of di-n-butylamine, and heated at 50° C. for 10 min to fully dissolve it. Four drops of bromocresol blue indicator were added, and then 25 mL of isopropanol was added to completely dissolve the indicator. The isocyanate content in the prepolymer was determined to be 16.5% by titration using 0.1036 mol / L dilute hydrochloric acid.

[0094] The ratio of the mass (g) of bromocresol blue in the bromocresol blue indicator to the volume (mL) of the solvent sodium hydroxide is 1:1000, and the concentration of the sodium hydroxide is 0.1 mol / L;

[0095] (3) preheating the main raw materials of polybutylene glycol and polyether 330N polyol after dehydration to 70° C., and dissolving 1.9876 g of 4,4'-dihydroxydiphenyl disulfide in N,N-dimethylformamide solution in advance;

[0096] (4) Add 102.786 g of polybutylene glycol, 9.87 g of polyether 330N polyol and N,N-dimethylformamide solution containing 1.9876 g of 4,4'-dihydroxydiphenyl disulfide in step (3) into a container in sequence, then add 31.8657 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 60 seconds; pour into a polytetrafluoroethylene container and place in an oven at 70°C for curing for 48 hours, then dry in a vacuum oven at 80°C for 24 hours to remove the organic solvent, to obtain a polyurethane elastomer.

[0097] (5) 10 g of choline chloride and 13 g of glycerol were stirred at 100 °C and 400 rpm for 2 h to obtain an ionic liquid.

[0098] (6) The prepared polyurethane elastomer was placed in 100 ml of N,N-dimethylformamide and soaked for 20 minutes. Then, 1 ml of ionic liquid was evenly coated on the surface of the self-healing polyurethane substrate, left to stand for 30 minutes, and then dried in a forced air oven at 80°C for 6 hours to obtain an ultra-soft ionic liquid conductive self-healing polyurethane elastomer.

[0099] The obtained elastomer was subjected to infrared spectroscopy analysis. -1 The peak of -NH- stretching vibration appeared at 1721cm -1 The peak of -CO- stretching vibration appears at 450 cm -1 A peak of -SS- vibration appears.

[0100] The obtained elastomer was subjected to a large strain electrical signal test. When the stretching rate reached 240%, electrical signals could be detected in the range of 0.015 mA to 0.018 mA, indicating that the elastomer can conduct electricity under large strain.

[0101] The obtained elastomer was subjected to a small strain electrical signal test. When the stretching rate reached 100%, electrical signals could be detected in the range of 0.006 mA to 0.007 mA, indicating that the elastomer can conduct electricity under small strain.

[0102] The obtained elastomer was cut and then spliced, and then repaired at room temperature for 1 hour before a tensile test. Since the chemical cross-linking points were cut off during the cutting process, the elongation at break was difficult to recover to that of the initial sample, but its tensile strength was basically restored to 60% of the original.

[0103] Example 4

[0104] A super-soft ionic liquid conductive self-healing polyurethane elastomer, the super-soft ionic liquid conductive self-healing polyurethane elastomer is composed of three raw material components A, B, and C. Taking the total mass of each of the raw materials A, B, and C as 100%, the components and their mass fractions in the raw material A are as follows: (HDI) 37%-39%, polytetramethylene glycol (PTMG) 61%-63%; the components and their mass fractions in the raw material B are as follows: polytetramethylene glycol (PTMG) 87.6%-91.6%, polyether 330N polyol (330N) 6.7%-10.7%; 4,4'-dihydroxydiphenyl disulfide 0.7%-2.7%; the components and their mass fractions in the raw material C are as follows: choline chloride 42%-44%, glycerol 56%-58%; the auxiliary raw materials are organic solutions (such as N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, etc.) and toluene solutions of indicator bromocresol blue and di-n-butylamine.

[0105] The molecular weight of the polybutylene glycol is 1760-2080, the molecular weight of the polyether 330N polyol is 4600-4800, and the chain extender is an N,N-dimethylformamide solution of polybutylene glycol and 4,4'-dihydroxydiphenyl disulfide.

[0106] The mass ratio of hexamethylene diisocyanate and polybutylene glycol used in the synthetic polyurethane prepolymer is 3:5.

[0107] The ratio of the mass (g) of the polyurethane prepolymer sample to be titrated to the volume (mL) of the isopropanol solvent is (3-4):500; the ratio of the mass (g) of the di-n-butylamine to the volume (mL) of the toluene solvent is 129:166; the volume ratio of the titration sample solution to the toluene solution of di-n-butylamine is 2:1; the ratio of the mass (g) of the indicator bromocresol blue to the volume (mL) of the solution is 1:1000;

[0108] A method for preparing the ultra-soft ionic liquid conductive self-healing polyurethane elastomer described in this embodiment, the specific steps of the method are as follows:

[0109] (1) 60 g of hexamethylene diisocyanate and 100 g of polybutylene glycol were added to a 250 mL three-necked flask, and the temperature was raised to 80° C. The raw materials were stirred at a rate of 200 r / min to mix them evenly, and the polyurethane prepolymer was obtained after reacting for 4 h;

[0110] (2) 0.3795 g of the prepolymer obtained in step (1) was dissolved in 50 mL of a toluene solution of di-n-butylamine, and heated at 50° C. for 10 min to fully dissolve it. Four drops of bromocresol blue indicator were added, and then 25 mL of isopropanol was added to completely dissolve the indicator. The isocyanate content in the prepolymer was determined to be 16.7% by titration using 0.1036 mol / L dilute hydrochloric acid.

[0111] The ratio of the mass (g) of bromocresol blue in the bromocresol blue indicator to the volume (mL) of the solvent sodium hydroxide is 1:1000, and the concentration of the sodium hydroxide is 0.1 mol / L;

[0112] (3) preheating the main raw materials of polybutylene glycol and polyether 330N polyol after dehydration to 70° C., and dissolving 1.9920 g of 4,4'-dihydroxydiphenyl disulfide in N,N-dimethylformamide solution in advance;

[0113] (4) Add 102.549 g of polybutylene glycol, 10.33 g of polyether 330N polyol and N,N-dimethylformamide solution containing 1.9920 g of 4,4'-dihydroxydiphenyl disulfide in step (3) into a container in sequence, then add 32.7547 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 60 seconds; pour into a polytetrafluoroethylene container and place in an oven at 70°C for curing for 48 hours, then dry in a vacuum oven at 80°C for 24 hours to remove the organic solvent, to obtain a polyurethane elastomer.

[0114] (5) 10 g of choline chloride and 13 g of glycerol were stirred at 100 °C and 400 rpm for 2 h to obtain an ionic liquid.

[0115] (6) The prepared polyurethane elastomer was placed in 100 ml of N,N-dimethylformamide and soaked for 20 minutes. Then, 1 ml of ionic liquid was evenly coated on the surface of the self-healing polyurethane substrate, left to stand for 30 minutes, and then dried in a forced air oven at 80°C for 6 hours to obtain an ultra-soft ionic liquid conductive self-healing polyurethane elastomer.

[0116] The obtained elastomer was subjected to infrared spectroscopy analysis. -1 The peak of -NH- stretching vibration appeared at 1722 cm -1 The peak of -CO- stretching vibration appeared at 454 cm -1 A peak of -SS- vibration appears.

[0117] The obtained elastomer was subjected to a large strain electrical signal test. When the stretching rate reached 230%, electrical signals could be detected in the range of 0.015 mA to 0.018 mA, indicating that the elastomer can conduct electricity under large strain.

[0118] The obtained elastomer was subjected to a small strain electrical signal test. When the stretching rate reached 110%, electrical signals could be detected in the range of 0.006 mA to 0.007 mA, indicating that the elastomer can conduct electricity under small strain.

[0119] The obtained elastomer was cut and then spliced, and then repaired at room temperature for 1 hour before a tensile test. Since the chemical cross-linking points were cut off during the cutting process, the elongation at break was difficult to recover to that of the initial sample, but its tensile strength was basically restored to 59% of the original.

[0120] Example 5

[0121] A super-soft ionic liquid conductive self-healing polyurethane elastomer, the super-soft ionic liquid conductive self-healing polyurethane elastomer is composed of three raw material components A, B, and C. Taking the total mass of each of the raw materials A, B, and C as 100%, the components and their mass fractions in the raw material A are as follows: hexamethylene diisocyanate (HDI) 37% to 39%, polytetramethylene glycol (PTMG) 61% to 63%; the components and their mass fractions in the raw material B are as follows: polytetramethylene glycol (PTMG) TMG) 87.6% to 91.6%, polyether 330N polyol (330N) 6.7% to 10.7%; 4,4'-dihydroxydiphenyl disulfide 0.7% to 2.7%; the components and their mass fractions in the C raw material are as follows: choline chloride 42% to 44%, glycerol 56% to 58%; the auxiliary raw materials are organic solvents (such as N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, etc.) and indicators bromocresol blue and di-n-butylamine in toluene solution.

[0122] The molecular weight of the polybutylene glycol is 1760-2080, the molecular weight of the polyether 330N polyol is 4600-4800, and the chain extender is an N,N-dimethylformamide solution of polybutylene glycol and 4,4'-dihydroxydiphenyl disulfide.

[0123] The mass ratio of hexamethylene diisocyanate and polybutylene glycol used in the synthetic polyurethane prepolymer is 3:5.

[0124] The ratio of the mass (g) of the polyurethane prepolymer sample to be titrated to the volume (mL) of the isopropanol solvent is (3-4):500; the ratio of the mass (g) of the di-n-butylamine to the volume (mL) of the toluene solvent is 129:166; the volume ratio of the titration sample solution to the toluene solution of di-n-butylamine is 2:1; the ratio of the mass (g) of the indicator bromocresol blue to the volume (mL) of the solution is 1:1000;

[0125] A method for preparing the ultra-soft ionic liquid conductive self-healing polyurethane elastomer described in this embodiment, the specific steps of the method are as follows:

[0126] (1) 60 g of hexamethylene diisocyanate and 100 g of polybutylene glycol were added to a 250 mL three-necked flask, and the temperature was raised to 80° C. The raw materials were stirred at a rate of 200 r / min to mix them evenly, and the polyurethane prepolymer was obtained after reacting for 4 h;

[0127] (2) 0.3937 g of the prepolymer obtained in step (1) was dissolved in 50 mL of a toluene solution of di-n-butylamine, and heated at 50° C. for 10 min to fully dissolve it. Four drops of bromocresol blue indicator were added, and then 25 mL of isopropanol was added to completely dissolve the indicator. The isocyanate content in the prepolymer was determined to be 16.9% by titration using 0.1036 mol / L dilute hydrochloric acid.

[0128] The ratio of the mass (g) of bromocresol blue in the bromocresol blue indicator to the volume (mL) of the solvent sodium hydroxide is 1:1000, and the concentration of the sodium hydroxide is 0.1 mol / L;

[0129] (3) preheating the main raw materials of polybutylene glycol and polyether 330N polyol after dehydration to 70° C., and dissolving 1.9976 g of 4,4'-dihydroxydiphenyl disulfide in N,N-dimethylformamide solution in advance;

[0130] (4) Add 103.761 g of polybutylene glycol, 10.76 g of polyether 330N polyol and N,N-dimethylformamide solution containing 1.9976 g of 4,4'-dihydroxydiphenyl disulfide in step (3) into a container in sequence, then add 33.2432 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 60 seconds; pour into a polytetrafluoroethylene container and place in an oven at 70°C for curing for 48 hours, then dry in a vacuum oven at 80°C for 24 hours to remove the organic solvent, to obtain a polyurethane elastomer.

[0131] (5) 10 g of choline chloride and 13 g of glycerol were stirred at 100 °C and 400 rpm for 2 h to obtain an ionic liquid.

[0132] (6) The prepared polyurethane elastomer was soaked in 100 ml of N,N-dimethylformamide for 20 min, and then 1 ml of ionic liquid was evenly coated on the surface of the self-healing polyurethane substrate, left to stand for 30 min, and then dried in a forced air oven at 80 °C for 6 h to obtain an ultra-soft liquid conductive self-healing polyurethane elastomer.

[0133] The obtained elastomer was subjected to infrared spectroscopy analysis. -1 The peak of -NH- stretching vibration appeared at 1721cm -1 The peak of -CO- stretching vibration appeared at 453 cm -1 A peak of -SS- vibration appears.

[0134] The obtained elastomer was subjected to a large strain electrical signal test. When the stretching rate reached 260%, electrical signals could be detected in the range of 0.015 mA to 0.018 mA, indicating that the elastomer can conduct electricity under large strain.

[0135] The obtained elastomer was subjected to a small strain electrical signal test. When the stretching rate reached 110%, electrical signals could be detected in the range of 0.006 mA to 0.007 mA, indicating that the elastomer can conduct electricity under small strain.

[0136] The obtained elastomer was cut and then spliced, and then repaired at room temperature for 1 hour before a tensile test. Since the chemical cross-linking points were cut off during the cutting process, the elongation at break was difficult to recover to that of the initial sample, but its tensile strength was basically restored to 55% of the original.

[0137] Example 6

[0138] A super-soft ionic liquid conductive self-healing polyurethane elastomer, the super-soft ionic liquid conductive self-healing polyurethane elastomer is composed of three raw material components A, B, and C. Taking the total mass of each of the raw materials A, B, and C as 100%, the components and their mass fractions in the raw material A are as follows: hexamethylene diisocyanate (HDI) 37% to 39%, polytetramethylene glycol (PTMG) 61% to 63%; the components and their mass fractions in the raw material B are as follows: polytetramethylene glycol (PTMG) TMG) 87.6% to 91.6%, polyether 330N polyol (330N) 6.7% to 10.7%; 4,4'-dihydroxydiphenyl disulfide 0.7% to 2.7%; the components and their mass fractions in the C raw material are as follows: choline chloride 42% to 44%, glycerol 56% to 58%; the auxiliary raw materials are organic solvents (such as N,N-dimethylformamide, dimethyl sulfoxide, tetrahydrofuran, etc.) and indicators bromocresol blue and di-n-butylamine in toluene solution.

[0139] The molecular weight of the polybutylene glycol is 1760-2080, the molecular weight of the polyether 330N polyol is 4600-4800, and the chain extender is an N,N-dimethylformamide solution of polybutylene glycol and 4,4'-dihydroxydiphenyl disulfide.

[0140] The mass ratio of hexamethylene diisocyanate and polybutylene glycol used in the synthetic polyurethane prepolymer is 3:5.

[0141] The ratio of the mass (g) of the polyurethane prepolymer sample to be titrated to the volume (mL) of the isopropanol solvent is (3-4):500; the ratio of the mass (g) of the di-n-butylamine to the volume (mL) of the toluene solvent is 129:166; the volume ratio of the titration sample solution to the toluene solution of di-n-butylamine is 2:1; the ratio of the mass (g) of the indicator bromocresol blue to the volume (mL) of the solution is 1:1000;

[0142] A method for preparing the ultra-soft ionic liquid conductive self-healing polyurethane elastomer described in this embodiment, the specific steps of the method are as follows:

[0143] (1) 60 g of hexamethylene diisocyanate and 100 g of polybutylene glycol were added to a 250 mL three-necked flask, and the temperature was raised to 80° C. The raw materials were stirred at a rate of 200 r / min to mix them evenly, and the polyurethane prepolymer was obtained after reacting for 4 h;

[0144] (2) 0.3822 g of the prepolymer obtained in step (1) was dissolved in 50 mL of a toluene solution of di-n-butylamine, and heated at 50° C. for 10 min to fully dissolve it. Four drops of bromocresol blue indicator were added, and then 25 mL of isopropanol was added to completely dissolve the indicator. The isocyanate content in the prepolymer was determined to be 17.2% by titration using 0.1036 mol / L dilute hydrochloric acid.

[0145] The ratio of the mass (g) of bromocresol blue in the bromocresol blue indicator to the volume (mL) of the solvent sodium hydroxide is 1:1000, and the concentration of the sodium hydroxide is 0.1 mol / L;

[0146] (3) preheating the main raw materials of polybutylene glycol and polyether 330N polyol after dehydration to 70° C., and dissolving 1.9896 g of 4,4'-dihydroxydiphenyl disulfide in N,N-dimethylformamide solution in advance;

[0147] (4) Add 103.275 g of polybutylene glycol, 11.09 g of polyether 330N polyol and N,N-dimethylformamide solution containing 1.9896 g of 4,4'-dihydroxydiphenyl disulfide in step (3) into a container in sequence, then add 31.9548 g of prepolymer and stir the solution at a stirring rate of 2000 r / min for 60 seconds; pour into a polytetrafluoroethylene container and place in an oven at 70°C for curing for 48 hours, then dry in a vacuum oven at 80°C for 24 hours to remove the organic solvent, to obtain a polyurethane elastomer.

[0148] (5) 10 g of choline chloride and 13 g of glycerol were stirred at 100 °C and 400 rpm for 2 h to obtain an ionic liquid.

[0149] (6) The prepared polyurethane elastomer was placed in 100 ml of N,N-dimethylformamide and soaked for 20 minutes. Then, 1 ml of ionic liquid was evenly coated on the surface of the self-healing polyurethane substrate, left to stand for 30 minutes, and then dried in a forced air oven at 80°C for 6 hours to obtain an ultra-soft ionic liquid conductive self-healing polyurethane elastomer.

[0150] The obtained elastomer was subjected to infrared spectroscopy analysis. -1 The peak of -NH- stretching vibration appeared at 1721cm -1 The peak of -CO- stretching vibration appeared at 453 cm -1 A peak of -SS- vibration appears.

[0151] The obtained elastomer was subjected to a large strain electrical signal test. When the stretching rate reached 240%, electrical signals could be detected in the range of 0.015 mA to 0.018 mA, indicating that the elastomer can conduct electricity under large strain.

[0152] The obtained elastomer was subjected to a small strain electrical signal test. When the stretching rate reached 100%, electrical signals could be detected in the range of 0.006 mA to 0.007 mA, indicating that the elastomer can conduct electricity under small strain.

[0153] The obtained elastomer was cut and then spliced, and then repaired at room temperature for 1 hour before a tensile test. Since the chemical cross-linking points were cut off during the cutting process, the elongation at break was difficult to recover to that of the initial sample, but its tensile strength was basically restored to 57% of the original.

[0154] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An ultra-soft ionic liquid conductive self-healing polyurethane elastomer, characterized in that: The raw materials of the ultra-soft ionic liquid conductive self-repairing polyurethane elastomer include component A, component B and component C; Taking the mass of component A as 100%, the mass percentages of the components in component A are as follows: Hexamethylene diisocyanate 37% to 39%; Polybutylene glycol 61% to 63%; Taking the mass of component B as 100%, the mass percentages of the components in component B are as follows: Polybutylene glycol 87.6%~91.6%; Polyether 330N polyol 6.7% to 10.7%; 4,4'-dihydroxydiphenyl disulfide 0.7% to 2.7%; Taking the mass of the C component as 100%, the mass percentages of the components in the C component are: Choline chloride 42%-44%; Glycerol 56%~58%.

2. The ultra-soft ionic liquid conductive self-healing polyurethane elastomer according to claim 1, characterized in that: The molecular weight of the polybutylene glycol is 1760-2080; The molecular weight of the polyether 330N polyol is 4600-4800.

3. A method for preparing an ultra-soft ionic liquid conductive self-healing polyurethane elastomer, the method comprising the steps of: In the first step, the hexamethylene diisocyanate and polybutylene glycol in component A are dehydrated and then mixed, and a nitrogen environment is provided during the mixing, and then the temperature is raised to 80-85° C. and stirred for reaction for 4-5 hours to obtain a polyurethane prepolymer; The second step is to mix part of the polyurethane prepolymer obtained in the first step with isopropanol in a water bath environment at 45-55° C., with a mixing volume of L and a mixing time of 10-15 min, and then add a toluene solution of di-n-butylamine and a bromocresol blue indicator, and then titrate with 0.1 mol / L dilute hydrochloric acid until the solution no longer changes color within 30 seconds, and then terminate the titration. After the titration is completed, calculate the isocyanate content a in the polyurethane prepolymer; The third step is to dehydrate the polybutylene glycol and polyether 330N polyol in component B; The fourth step is to dissolve the 4,4'-dihydroxydiphenyl disulfide in the B component in N,N-dimethylformamide, and then mix it with part of the polyurethane prepolymer obtained in the first step, the dehydrated polybutylene glycol in the B component, and the polyether 330N polyol, at a mixing temperature of 30-50°C; Step 5, stirring the materials mixed in step 4, and then curing them at 75-85° C. for 24-48 hours, and then drying them in a vacuum oven at 75-85° C. for 24-48 hours to obtain a polyurethane elastomer; Step 6: Mix the choline chloride and glycerol in the C material, heat to 95-105° C., and stir to dissolve for 2-3 hours to obtain an ionic liquid; In the seventh step, the polyurethane elastomer prepared in the fifth step is soaked in N,N-dimethylformamide for 10-20 minutes, and then the ionic liquid obtained in the sixth step is evenly coated on the surface of the soaked polyurethane elastomer, and dried to obtain an ultra-soft ionic liquid conductive self-healing polyurethane elastomer.

4. The method for preparing a super-soft ionic liquid conductive self-healing polyurethane elastomer according to claim 3, characterized in that: In the second step, the ratio of polyurethane prepolymer to isopropyl alcohol is 3-4 g:500 mL; The volume ratio of the mixed volume L of the polyurethane prepolymer and isopropanol to the toluene solution of di-n-butylamine is 2:1; The ratio of the volume L of the polyurethane prepolymer and isopropanol after mixing to the bromocresol blue indicator is 1000mL:1g; The ratio of the mass of the di-n-butylamine to the volume of the solvent toluene is 129 g:166 ml.

5. The method for preparing a super-soft ionic liquid conductive self-healing polyurethane elastomer according to claim 3, characterized in that: In the fourth step, the ratio of 4,4'-dihydroxydiphenyl disulfide, polyurethane prepolymer, polytetramethylene glycol (PTMG), and polyether 330N polyol satisfies: (m1×a%) / 42=R×((m2 / N1)×2+(m3 / N2)×3+(m4 / N3)×2) Wherein, m1 is the mass of polyurethane prepolymer, m2 is the mass of polybutylene glycol, m3 is the mass of polyether 330N polyol, and m4 is the mass of 4,4' dihydroxy diphenyl disulfide; N1, is the molecular weight of polybutylene glycol; N2 is the molecular weight of polyether 330N polyol; N3 is the molecular weight of 4,4' dihydroxydiphenyl disulfide; The value of the isocyanate group in the polyurethane prepolymer is defined as R1, and the sum of the hydroxyl groups in 4,4'-dihydroxydiphenyl disulfide, polybutylene glycol and polyether 330N polyol is defined as R2, then R=R1 / R2, and R=1.04-1.06.

Citation Information

Patent Citations

  • Polymerizable eutectic solvent for self-repairing material, conductive elastomer and preparation method of conductive elastomer

    CN111253520A

  • Self-healing ionic polyurethane as well as preparation method and application thereof

    CN113292701A

  • High-strength self-repairing anti-freezing ionic gel strain sensor and preparation method thereof

    CN114805737A

  • Polyphenolic compound modified polyurethane elastomer and preparation method thereof

    CN116143995A

  • High-strength self-repairing ionic gel and preparation method thereof

    CN116284676A