Hyperbranched phosphate compound as well as preparation method and application thereof
Through the interaction between the branched structure of the hyperbranched phosphate compound and the carbon nanotube, the problems of difficulty in dispersion and poor dispersion stability of carbon nanotubes are solved, and efficient dispersion and stability of carbon nanotubes are achieved.
Patent Information
- Application Number
- CN202311789904.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-25
- Publication Date
- 2024-11-29
AI Technical Summary
Due to its special structure, carbon nanotubes have difficulty in dispersion and poor dispersion stability. The existing dispersants have limitations in their applications, especially for linear structural carbon nanotubes with huge length-to-diameter ratios.
Using hyperbranched phosphate compounds as dispersants, polyether, polyester and polyamide groups are introduced through esterification of polyphosphoric acid and aromatic alcohols, and chain extension through small molecule polyols to form a branched structure to improve carbon nanometers. Tube interaction and adsorption stability.
The dispersion and dispersion stability of carbon nanotubes are significantly improved, and the defects of poor dispersion and unstable dispersion of existing dispersants are overcome, and the stable and efficient dispersion of carbon nanotubes is provided, and the synthesis process is simplified.
Smart Images

Figure CN119039595A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of carbon nanotube dispersion, and more specifically, to a hyperbranched phosphate compound and a preparation method and application thereof. Background Art
[0002] Carbon nanotubes have been around for more than 30 years since they were discovered by Japanese scientists in 1991. They have been widely used in electronics, aviation, energy, coatings and other fields due to their excellent electrical conductivity and mechanical properties. In the field of new energy, carbon nanotubes are used as conductive agents in lithium battery positive electrode materials (lithium iron phosphate positive electrode and ternary lithium battery positive electrode) and silicon negative electrode, mainly to improve the battery's capacity, rate, cycle and other performance. In particular, the rapid and large-scale development of new energy vehicles in recent years has led to an increase in the demand for carbon nanotubes in lithium-ion battery electrode materials year by year.
[0003] Carbon nanotubes are hollow tubular structures formed by the curling of graphitized carbon atoms. Due to the special structure, carbon nanotubes are difficult to disperse. The main reasons include: First, according to the number of layers of the curled graphitized carbon atoms, they can be divided into single-walled, few-walled and multi-walled carbon nanotubes. The smallest diameter can reach about 2nm, and the length can reach more than 50μm. This structure with a huge aspect ratio makes carbon nanotubes very easy to curl and entangle, making it more difficult to disperse. Secondly, the specific surface area of carbon nanotubes is generally 200-2000m 2 / g, which also makes dispersion extremely difficult. Finally, the carbon nanotubes composed of graphitized carbon atoms have a low polarity surface structure, which makes it difficult for the dispersant to interact with the carbon nanotubes. The dispersant has a low interaction strength with the carbon nanotubes and is easily desorbed, which not only makes it difficult to disperse the carbon nanotubes, but also makes the dispersion stability of the carbon nanotubes worse.
[0004] At present, for the dispersion of carbon nanotubes, polyvinyl pyrrolidone, carboxymethyl cellulose, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, etc. are generally used as dispersants in aqueous systems; in organic systems, polyvinyl pyrrolidone is mostly used, or some dispersants used to disperse carbon black in coatings and inks are used.
[0005] In some schemes, a method for preparing a polyvinyl pyrrolidone copolymer dispersant is involved. The method introduces a solvated chain structure into the dispersant, increases the steric hindrance of the dispersant, and improves the dispersion stability; the small molecule surfactant used has a good wetting effect and can quickly play a dispersing role when used as a dispersant; the linear structure it has can disperse carbon nanotubes, and the dispersion stability is good; in addition, the method uses a dispersant for dispersing carbon black to disperse carbon nanotubes. However, the dispersant prepared by the method contains a polyvinyl pyrrolidone structure, and the cyclic structure of pyrrolidone is unstable and easily decomposed in some cases, which makes the dispersant limited in application. In addition, the small molecule surfactant has a low dispersing ability for carbon nanotubes as a dispersant, and the dispersion stability is poor. During the storage process, the dispersed carbon nanotubes will stratify and settle in a short period of time. In addition, although the linear polymer dispersant can disperse carbon nanotubes, it will also have side effects such as thickening, and the dispersing effect is limited. In addition, the dispersant for dispersing carbon black is a dispersant developed based on granular carbon black, which is not applicable to carbon nanotubes with special structures, and the effect is even worse than that of polyvinyl pyrrolidone.
[0006] In some other schemes, a dispersing additive based on a phosphate derivative is proposed, which is grafted with a phosphate group and a solvated chain by reacting a diisocyanate with a compound containing active hydrogen. The resulting dispersant structure contains a phosphate group, an aromatic ring, an amine group that can interact with carbon nanotubes, and solvated chains such as polyether, polyester, and polysiloxane. The compound with this structure is suitable for use as a wetting agent and a dispersant. However, from the perspective of molecular structure, the production process of the dispersant is complicated, the price of raw materials is relatively high, and due to the constraints of raw materials, production process, and structural design, the dispersant is suitable for granular dispersed phases, and is not suitable for linear carbon nanotubes with a huge aspect ratio. Summary of the invention
[0007] Based on the above facts, the purpose of the present invention is to provide a hyperbranched phosphate compound and a preparation method and application thereof, so as to at least solve the problems of difficult dispersion and poor dispersion stability of carbon nanotubes.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] In one aspect, the present invention provides a hyperbranched phosphate compound having the structural formula shown below:
[0010]
[0011] Wherein, R1 is a C1-C4 alkyl group, and R2-R7 are each independently a C1-C 18 An alkylene group, R8 is a group obtained by removing the alcohol hydroxyl group of an aromatic alcohol, and R9 is an organic group containing 1 to 12 carbon atoms;
[0012] a and b are each independently an integer from 0 to 100;
[0013] c, d, e, and f are each independently an integer from 1 to 100;
[0014] g, h, i, j, k are each independently an integer of 0-10, and at least one of g, h, i, j, k is not 0;
[0015] l is an integer from 1 to 10;
[0016] n is an integer from 1 to 6.
[0017] In another aspect, the present invention provides a method for preparing the hyperbranched phosphate compound as described above, comprising the steps of:
[0018] Esterifying polyphosphoric acid with aromatic alcohol to obtain phosphate ester;
[0019] Introducing one or more of polyether, polyester and polyamide groups into the structure of the phosphate;
[0020] The hyperbranched phosphate compound is obtained by chain extension with a small molecule polyol.
[0021] Furthermore, the aromatic alcohol is selected from one or more of phenoxyethanol, propylene glycol phenyl ether, benzyl alcohol, phenylethyl alcohol and 3-methoxybenzyl alcohol.
[0022] Furthermore, the structural formula of the polyether is shown below:
[0023]
[0024] Furthermore, the structural formula of the polyester is shown below:
[0025]
[0026] Furthermore, the structural formula of the polyamide is shown below:
[0027]
[0028] Furthermore, the small molecule polyol is selected from one or two of 1,4-butanediol, 1,6-hexanediol, N,N-di(2-hydroxypropyl)aniline, diethanolamine, trimethylolethane, trimethylolpropane, di(trimethylolpropane), glycerol, diethylene glycol, pentaerythritol, dipentaerythritol, xylitol, sorbitol, mannitol, phenylpropylene glycol and cyclohexanehexol.
[0029] Wherein, the definitions of the above R1-R7 and af are as shown above.
[0030] Furthermore, the method also includes the step of adjusting pH and viscosity after chain extension with small molecule polyol.
[0031] Furthermore, the step of adjusting the pH is to adjust the pH to 6-8.
[0032] In another aspect, the present invention provides a carbon nanotube dispersant prepared from a raw material comprising the hyperbranched phosphate compound as described above.
[0033] In another aspect, the present invention provides use of the hyperbranched phosphate compound described above in preparing a carbon nanotube dispersant.
[0034] In another aspect, the present invention provides a carbon nanotube slurry, which is obtained by dispersing carbon nanotubes in a solution of the carbon nanotube dispersant as described above and then grinding the solution.
[0035] Furthermore, in the solution of the carbon nanotube dispersant, the solvent is selected from one or more of dimethylformamide, toluene, N-methylpyrrolidone, isopropyl alcohol, propylene glycol methyl ether acetate, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide.
[0036] Furthermore, in the carbon nanotube slurry, the mass percentage of the carbon nanotube dispersant is 0.1-2%.
[0037] Furthermore, the carbon nanotubes have a diameter of 7-11 nm and a length of 5-20 μm.
[0038] Furthermore, the carbon nanotubes have a diameter of 10-20 nm and a length of 10-30 μm.
[0039] The beneficial effects of the present invention are as follows:
[0040] The presence of the -POP- structure in the main structure of the hyperbranched phosphate compound provided by the present invention is helpful to improve the dispersion of carbon nanotubes. Further, according to the special structural characteristics of carbon nanotubes, more affinity groups that react with carbon nanotubes are introduced into the structure of the hyperbranched phosphate compound, so that when the hyperbranched phosphate compound is used as a carbon nanotube dispersant, the interaction between the dispersant and the carbon nanotubes can be improved, and the dispersibility can be enhanced. In addition, the adsorption sites are networked through the branched "anchoring" affinity group structure in the structure of the hyperbranched phosphate compound, and the probability of the networked "anchoring group" interacting with the functional groups on the surface of the carbon nanotube is increased, thereby further increasing the adsorption stability and dispersion ability. Furthermore, the hyperbranched structure formed by the solvation chain in the structure makes the dispersant more three-dimensional on the surface of the carbon nanotube, increases the distance between the carbon nanotubes, and reduces the van der Waals force between the carbon nanotubes, thereby making the dispersion of the carbon nanotubes more stable. DETAILED DESCRIPTION
[0041] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0042] According to a specific embodiment of the present invention, a hyperbranched phosphate compound is provided, having the structural formula shown below:
[0043]
[0044] Wherein, R1 is a C1-C4 alkyl group, and R2-R7 are each independently a C1-C 18 alkylene, R8 is a group obtained by removing the alcoholic hydroxyl group of aromatic alcohol (that is, the residue after removing the alcoholic hydroxyl group of aromatic alcohol), and R9 is an organic group containing 1-12 carbon atoms;
[0045] a and b are each independently an integer from 0 to 100;
[0046] c, d, e, and f are each independently an integer from 1 to 100;
[0047] g, h, i, j, k are each independently an integer of 0-10, and at least one of g, h, i, j, k is not 0;
[0048] l is an integer from 1 to 10;
[0049] n is an integer from 1 to 6.
[0050] Exemplarily, a and b are not 0 at the same time, and are each independently an integer of 7-60.
[0051] Exemplarily, c, d, e, and f are each independently an integer of 7-35.
[0052] Exemplarily, the structure of R8 contains 1-3 benzene rings.
[0053] Exemplarily, the aromatic alcohol is a monohydric alcohol. That is, the aromatic alcohol contains one alcoholic hydroxyl group. In some preferred examples, the aromatic alcohol includes but is not limited to one or more selected from phenoxyethanol, propylene glycol phenyl ether, benzyl alcohol, phenylethyl alcohol and 3-methoxybenzyl alcohol.
[0054] Exemplarily, R9 is a group obtained by removing the hydrogen from at least one hydroxyl group of a polyol (small molecule polyol) having 1 to 12 carbon atoms (ie, a residue obtained by removing the hydrogen from at least one hydroxyl group of a small molecule polyol).
[0055] In some more specific examples, the polyol having 1 to 12 carbon atoms (small molecule polyol) includes organic substances containing multiple hydroxyl groups, such as N,N-di(2-hydroxypropyl)aniline, diethanolamine, and the like.
[0056] Exemplarily, the small molecule polyol is selected from one or two of 1,4-butanediol, 1,6-hexanediol, N,N-di(2-hydroxypropyl)aniline, diethanolamine, trimethylolethane, trimethylolpropane, di(trimethylolpropane), glycerol, diethylene glycol, pentaerythritol, dipentaerythritol, xylitol, sorbitol, mannitol, phenylpropylene glycol and cyclohexanehexol.
[0057] In a preferred example, the above a and b can each independently be 0 or an integer of 1-100, and a and b are not 0 at the same time.
[0058] In a preferred example, the above g, h, i, j, and k can each independently be 0 or an integer of 1-10, and at least one of g, h, i, j, and k is not 0.
[0059] The hyperbranched phosphate compound provided in this embodiment is designed based on the special structural characteristics of carbon nanotubes, such as huge specific surface area, few surface functional groups, low surface polarity, and extremely large aspect ratio. This technical solution overcomes the defects of existing carbon nanotube dispersants, such as poor dispersibility and unstable dispersion. The provided hyperbranched phosphate compound can form a stable and efficient dispersion of carbon nanotubes, and the synthesis process is simple.
[0060] According to another specific embodiment of the present invention, there is provided a method for preparing a hyperbranched phosphate compound, comprising the following steps:
[0061] Esterifying polyphosphoric acid with aromatic alcohol to obtain phosphate ester;
[0062] Introducing one or more of polyether, polyester and polyamide groups into the structure of the phosphate;
[0063] The hyperbranched phosphate compound is obtained by chain extension with a small molecule polyol.
[0064] In the preparation method, polyphosphoric acid is used as the main skeleton, and phosphate groups, aromatic rings, etc. are introduced through esterification reaction to improve the dispersibility of the dispersant on carbon nanotubes; polyether / polyester / polyamide is introduced for solvation, and the steric hindrance provided by the solvation chain can increase the dispersion stability of the dispersant on the carbon nanotubes; and the carbon nanotube dispersant forms a branched structure through chain extension to further increase the adsorption sites and improve the adsorption stability.
[0065] In some examples, in the structure of the polyphosphoric acid, the phosphoric acid content (mass percentage) is 100%-130%. In this case, the aforementioned dispersion effect is better. In some preferred examples, in the structure of the polyphosphoric acid, the phosphoric acid content includes but is not limited to 100%-120%, 100%-118%, 100%-116%, 100%-115%, 100%-105%, 105%-120%, 105%-118%, 105%-116%, 105%-115%, 115%-120%, 115%-118%, 115%-116%, 105%, 115%, 116%, 118%, etc.
[0066] In some examples, the aromatic alcohol is a monohydric alcohol. Preferably, it is selected from one or more of phenoxyethanol, propylene glycol phenyl ether, benzyl alcohol, phenylethyl alcohol and 3-methoxybenzyl alcohol. The introduction of the benzene ring structure in the aromatic alcohol can make the hyperbranched phosphate compound have conjugated interactions with some functional groups on the surface of carbon materials such as carbon nanotubes, so as to better adsorb on the surface of carbon materials such as carbon nanotubes.
[0067] In this embodiment, the temperature and time of the esterification reaction can be adjusted according to the actual raw materials. For example, the temperature of the esterification reaction is preferably 100-120°C, and the time is preferably 1-2h. Exemplary esterification reaction temperatures include but are not limited to 100-115°C, 110-115°C, 115-120°C, 100°C, 110°C, 115°C, 120°C, etc.
[0068] In some examples, in the esterification reaction, the mass ratio of polyphosphoric acid to aromatic alcohol includes but is not limited to 1:1-1:3, 1:1.2-1:2.8, 1:1.5-1:2.5, etc.
[0069] In some preferred examples, the aromatic alcohol is selected from benzyl alcohol, a mixture of benzyl alcohol and 3-methoxybenzyl alcohol (preferably a mixture mass ratio of 1:1.5-1:2), a mixture of propylene glycol phenyl ether and phenoxyethanol (preferably a mixture mass ratio of 1:1-1:1.5), or a mixture of propylene glycol phenyl ether and benzyl alcohol (preferably a mixture mass ratio of 1:0.1-1:0.2). In this case, the obtained hyperbranched phosphate compound has a better adsorption effect on carbon materials such as carbon nanotubes.
[0070] In some examples, the polyether has a structural formula as shown below:
[0071]
[0072] Wherein, R1 is a C1-C4 alkyl group, and a and b are integers of 0-100.
[0073] In some examples, the molecular weight of the polyether is 500-5000. More specific examples may be 1000-5000, 1500-4000, 1500-2500, 1500-2000, 2000-4000, 2000-2500, 2500-4000, etc.
[0074] In some examples, the polyether is polyoxyethylene monomethyl ether or polyethylene glycol polypropylene glycol monotert-butyl ether. In some more specific examples, the polyether is polyoxyethylene monomethyl ether with a molecular weight of 1500-2500 or polyethylene glycol polypropylene glycol monotert-butyl ether with a molecular weight of 2000-4000.
[0075] In some examples, the polyester has a structural formula as shown below:
[0076]
[0077] Among them, R2, R3, and R4 are C1-C 18 The alkylene group is selected from the group consisting of c and d, each of which is an integer from 1 to 100.
[0078] In some examples, the molecular weight of the polyester is 1000-5000, preferably 1000-3000, 1000-2000, 1000, 2000, etc.
[0079] In some specific examples, the polyester is polycaprolactone. In some more specific examples, the polyester is polycaprolactone with a molecular weight of 1000-2000.
[0080] In some examples, the polyamide has a structural formula as shown below:
[0081]
[0082] Among them, R5, R6, and R7 are C1-C 18 The alkylene group, e and f are integers of 1-100.
[0083] Exemplarily, the molecular weight of the polyamide is 1000-2000.
[0084] In this embodiment, one or more of the polyether, polyester and polyamide groups can be introduced by adding one or more of the polyether, polyester and polyamide to the reaction material, keeping warm or heating to 100-120°C, and reacting. At this time, the temperature and time of the reaction can be adjusted according to the actual raw materials. Exemplarily, the reaction temperature is preferably 110-120°C, 100-110°C, 100°C, 110°C, 120°C, etc., and the time is preferably 1-3h, 2h, etc.
[0085] In some examples, the mass ratio of the polyphosphoric acid to one or more of polyether, polyester and polyamide includes but is not limited to 1:2-1:5, 1.2.1-1:4.5, 1:2.1-1:3, 1:2.5-1:4.5, etc.
[0086] In some examples, the small molecule polyol is selected from one or two of 1,4-butanediol, 1,6-hexanediol, N,N-di(2-hydroxypropyl)aniline, diethanolamine, trimethylolethane, trimethylolpropane, di(trimethylolpropane), glycerol, diethylene glycol, pentaerythritol, dipentaerythritol, xylitol, sorbitol, mannitol, phenylpropylene glycol and cyclohexanehexol.
[0087] In this embodiment, the method of introducing small molecule polyols for chain extension is preferably to add small molecule polyols to the reaction materials, and continue to introduce one or more of the polyether, polyester and polyamide groups for reaction at the reaction temperature. The reaction time is preferably 1-3h, 1.5-2.5h, 1.5h, 2h, 2.5h, etc.
[0088] In some examples, the mass ratio of the polyphosphoric acid to the small molecule polyol includes but is not limited to 5:1-25:1, 8:1-22:1, 8.5:1-22:1, 8.5:1-20:1, and the like.
[0089] In some examples, the method further comprises the step of adjusting pH and viscosity after chain extension with a small molecule polyol. Wherein, the step of adjusting pH is preferably to adjust pH to 6-8. The neutralizing agent for adjusting pH includes but is not limited to one or more selected from ammonia, ethanolamine, aniline, o-toluidine, biphenyl-4-amine, naphthylamine, 3-morpholine propylamine, 1-methyl-3-morpholine-4-propylamine, 2-methyl-2-morpholine-4-ylpropane-1-amine, 4-aminotriphenylamine, 4-aminotriazole, and 2,2'-diaminobenzidine.
[0090] The step of adjusting the viscosity is to adjust by adding a solvent, and the solvent is exemplarily selected from one or more of toluene, N-methylpyrrolidone (NMP), isopropyl alcohol, propylene glycol methyl ether acetate (PGMEA), N,N-dimethylformamide (DMF), N,N-dimethylacetamide and dimethyl sulfoxide.
[0091] According to another specific embodiment of the present invention, a carbon nanotube dispersant is provided. The carbon nanotube dispersant is prepared from a raw material comprising the hyperbranched phosphate compound as described above.
[0092] It can be seen that the carbon nanotube dispersant has the characteristics of the hyperbranched phosphate compound as described above, which will not be described in detail here.
[0093] According to another specific embodiment of the present invention, there is provided a use of the hyperbranched phosphate compound as described above in the preparation of a carbon nanotube dispersant.
[0094] According to another specific embodiment of the present invention, a carbon nanotube slurry is provided, which is obtained by dispersing carbon nanotubes in a solution of the carbon nanotube dispersant as described above and then grinding the dispersion.
[0095] Exemplarily, in the carbon nanotube dispersant solution, the solid content of the carbon nanotube dispersant is 20-70 wt %.
[0096] The amount of carbon nanotube dispersant used is related to the performance of the size of the carbon nanotubes. Exemplarily, in the carbon nanotube slurry, the mass percentage of the carbon nanotube dispersant is 0.1-2%. In some specific embodiments, in the carbon nanotube slurry, the mass percentage of the carbon nanotube dispersant is 0.1-1%, 0.5-2%, 1-2%, 0.5%, 1%, 2%, etc.
[0097] In some examples, the carbon nanotubes have a diameter of 7-11 nm and a length of 5-20 μm.
[0098] In some other examples, the carbon nanotubes have a diameter of 10-20 nm and a length of 10-30 μm.
[0099] In some examples, in the carbon nanotube slurry, the mass percentage of carbon nanotubes is 3-5%, 3-4%, 4-5%, 4%, 5%, etc.
[0100] In some examples, the mass percentage of the solvent in the carbon nanotube slurry is 93-96%, 93-95%, 94-95%, 93%, 94%, 95%, etc.
[0101] In some specific embodiments, in the carbon nanotube slurry, the mass percentage of carbon nanotubes is 3-5%, the mass percentage of carbon nanotube dispersant is 0.5-2%, and the mass percentage of solvent is 93-96%.
[0102] In some examples, the preparation of the carbon nanotube slurry includes the following steps:
[0103] Adding the carbon nanotube dispersant to the solvent, and adding the carbon nanotubes under stirring;
[0104] After the carbon nanotubes are completely infiltrated, high-speed dispersion is performed at 2000 rpm to obtain a pre-dispersed carbon nanotube slurry;
[0105] The carbon nanotube slurry is obtained by sand grinding.
[0106] In some examples, in the solution of the carbon nanotube dispersant, the solvent is selected from one or more of dimethylformamide, toluene, N-methylpyrrolidone, isopropyl alcohol, propylene glycol methyl ether acetate, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide.
[0107] In some examples, the carbon nanotubes have a diameter of 7-11 nm and a length of 5-20 μm.
[0108] In some other examples, the carbon nanotubes have a diameter of 10-20 nm and a length of 10-30 μm.
[0109] In this embodiment, the carbon nanotube slurry can be used in lithium battery cells as a conductive agent.
[0110] Exemplarily, the carbon nanotube slurry is used as a conductive agent in lithium battery positive electrode materials (lithium iron phosphate positive electrode and ternary lithium battery positive electrode) and silicon negative electrode for new energy fields.
[0111] The technical solution of the present invention is described below in conjunction with some specific embodiments:
[0112] Example 1
[0113] A method for preparing a hyperbranched phosphate compound comprises the following steps:
[0114] 1) In a dry and clean reactor, add 88g of polyphosphoric acid with a phosphoric acid content of 115%, heat to 100°C, add 140g of benzyl alcohol, and react at the temperature for 1h;
[0115] 2) Maintaining the reaction temperature at 100°C, 261 g of polyoxyethylene monomethyl ether with a molecular weight of 2000 was added to the reactor and the reaction was kept warm for 2 hours;
[0116] 3) Add 10 g of phenylpropylene glycol into the reactor and continue to react at 100° C. for 2 h;
[0117] 4) 0.3 g of aniline was added to the reaction kettle to adjust the pH of the polymer to 7.2, and then the water in the polymer was removed by vacuum extraction, and propylene glycol methyl ether acetate was added to adjust the viscosity to obtain a hyperbranched phosphate compound with an effective content (non-volatile content) of 40%.
[0118] Example 2
[0119] A method for preparing a hyperbranched phosphate compound comprises the following steps:
[0120] 1) In a dry and clean reactor, add 78g of polyphosphoric acid with a phosphoric acid content of 116%, heat to 115°C, add 62g of benzyl alcohol and 120g of 3-methoxybenzyl alcohol, and react at the temperature for 1.5h;
[0121] 2) Raise the reaction temperature to 120°C, then add 230 g of polycaprolactone with a molecular weight of 1500 into the reactor and keep the temperature for 2 hours;
[0122] 3) Add 8.5 g of N,N-di(2-hydroxypropyl)aniline into the reactor and continue to react at 120°C for 2 h;
[0123] 4) 0.5 g of naphthylamine was added to the reaction kettle to adjust the pH of the polymer to 7.1, and then the water in the polymer was removed by vacuuming, and N-methylpyrrolidone was added to adjust the viscosity to obtain a hyperbranched phosphate compound with an effective content (non-volatile content) of 25%.
[0124] Example 3
[0125] A method for preparing a hyperbranched phosphate compound comprises the following steps:
[0126] 1) In a dry and clean reactor, add 65 g of polyphosphoric acid with a phosphoric acid content of 118%, heat to 100° C., add 73 g of propylene glycol phenyl ether and 66 g of phenoxyethanol, and react at the controlled temperature for 1.5 h;
[0127] 2) Raise the reaction temperature to 110° C., then add 289 g of polyethylene glycol polypropylene glycol mono-tert-butyl ether with a molecular weight of 3000 into the reactor, and keep the temperature to react for 2 hours;
[0128] 3) Add 4.1 g of trimethylolpropane into the reactor and continue to react at 110°C for 1.5 h;
[0129] 4) 0.3 g of aniline was added to the reaction kettle to adjust the pH of the polymer to 7.4, and then the water in the polymer was removed by vacuuming, and then toluene was added to adjust the viscosity to obtain a hyperbranched phosphate compound with an effective content (non-volatile content) of 30%.
[0130] Example 4
[0131] A method for preparing a hyperbranched phosphate compound comprises the following steps:
[0132] 1) In a dry and clean reactor, add 93g of polyphosphoric acid with a phosphoric acid content of 105%, heat to 110°C, add 167g of propylene glycol phenyl ether and 30g of benzyl alcohol, and react at the temperature for 1h;
[0133] 2) Add 206 g of polyamide with a molecular weight of 2000 into the reactor and keep the reaction temperature for 2 hours;
[0134] 3) Add 4.4 g of pentaerythritol to the reactor and continue to heat and react for 2.5 h;
[0135] 4) Add 0.2 g of 2,2'-diaminobenzidine to the reaction kettle, adjust the polymer pH to 7.6, then remove the water in the polymer by vacuuming, and then add N,N-dimethylformamide to adjust the viscosity to obtain a hyperbranched phosphate compound with an effective content (non-volatile content) of 50%.
[0136] Dispersant application evaluation:
[0137] The hyperbranched phosphate compounds prepared in Examples 1-4 and commercially available carbon nanotube dispersants (comparative example, molecular structure as shown in Formula 1 below) were used to disperse carbon nanotubes to prepare carbon nanotube slurries, and the dispersing performance differences of the dispersants were compared.
[0138]
[0139] Wherein, in Formula 1, a is an integer of 6-30, b is an integer of 0-30, n is an integer of 1 or 2, R1 is a group obtained by the reaction of monohydroxymethylphenol with ethoxylation, and R2 is H or NH4.
[0140] The dispersion method is as follows:
[0141] ① First weigh the solvent and add it into the stirring container, then add the carbon nanotube dispersant;
[0142] ② After stirring evenly, slowly add carbon nanotubes (tube diameter 7-11nm, tube length 5-20μm) under low-speed stirring at about 500rpm;
[0143] ③ After the carbon nanotubes are completely infiltrated, high-speed dispersion at about 2000 rpm is started to obtain pre-dispersed carbon nanotube slurry;
[0144] ④ On a 0.6L Langling sand mill, use 0.6mm zirconium beads and sand grind for 2h at 20-30℃ to obtain carbon nanotube slurry.
[0145] In the above dispersion method, the amount of dispersant, solvent and carbon nanotubes (all refer to the percentage relative to the total mass of dispersant, solvent and carbon nanotubes) and their selection and specifications are shown in Table 1.
[0146] The viscosity of the carbon nanotube slurry and the viscosity after storage for one month were tested using a rotational viscometer at 25°C. The results are shown in Table 1:
[0147] Table 1 Comparison of viscosity of carbon nanotube slurry prepared by different dispersants
[0148]
[0149] From the results in Table 1, when the hyperbranched phosphate compounds prepared in various embodiments are used as carbon nanotube dispersants, the initial viscosity, viscosity after storage for one month, and viscosity variation of carbon nanotube slurries prepared by dispersing carbon nanotubes in several different solvent systems are significantly lower than those of commercially available dispersants. This indicates that the hyperbranched phosphate carbon nanotube dispersants prepared in the present invention have a good dispersing effect on carbon nanotubes.
[0150] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A hyperbranched phosphate compound, characterized in that It has the structural formula shown below: Wherein, R1 is a C1-C4 alkyl group, and R2-R7 are each independently a C1-C 18 An alkylene group, R8 is a group obtained by removing the alcohol hydroxyl group of an aromatic alcohol, and R9 is an organic group containing 1 to 12 carbon atoms; a and b are each independently an integer from 0 to 100; c, d, e, and f are each independently an integer from 1 to 100; g, h, i, j, k are each independently an integer of 0-10, and at least one of g, h, i, j, k is not 0; l is an integer from 1 to 10; n is an integer from 1 to 6.
2. The method for preparing a hyperbranched phosphate compound according to claim 1, wherein The steps include: Esterifying polyphosphoric acid with aromatic alcohol to obtain phosphate ester; Introducing one or more of polyether, polyester and polyamide groups into the structure of the phosphate; The hyperbranched phosphate compound is obtained by chain extension with a small molecule polyol.
3. The preparation method according to claim 2, characterized in that: The aromatic alcohol is selected from one or more of phenoxyethanol, propylene glycol phenyl ether, benzyl alcohol, phenylethyl alcohol and 3-methoxybenzyl alcohol; and / or The structural formula of the polyether is shown below: and / or The structural formula of the polyester is shown below: and / or The structural formula of the polyamide is shown below: and / or The small molecule polyol is selected from one or two of 1,4-butanediol, 1,6-hexanediol, N,N-di(2-hydroxypropyl)aniline, diethanolamine, trimethylolethane, trimethylolpropane, di(trimethylolpropane), glycerol, diethylene glycol, pentaerythritol, dipentaerythritol, xylitol, sorbitol, mannitol, phenylpropylene glycol and cyclohexanehexol; Wherein, the definitions of the above R1-R7 and af are as shown in claim 1.
4. The preparation method according to claim 2, characterized in that: The method further comprises the steps of adjusting pH and viscosity after chain extension with a small molecule polyol; Preferably, the pH is adjusted to 6-8.
5. A carbon nanotube dispersant, characterized in that: The method is prepared from raw materials comprising the hyperbranched phosphate compound as claimed in claim 1.
6. Use of the hyperbranched phosphate compound according to claim 1 in preparing a carbon nanotube dispersant.
7. A carbon nanotube slurry, characterized in that: The carbon nanotubes are dispersed in a solution of the carbon nanotube dispersant as claimed in claim 5 and then ground.
8. The carbon nanotube slurry according to claim 7, characterized in that: In the solution of the carbon nanotube dispersant, the solvent is selected from one or more of dimethylformamide, toluene, N-methylpyrrolidone, isopropyl alcohol, propylene glycol methyl ether acetate, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethyl sulfoxide.
9. The carbon nanotube slurry according to claim 7, characterized in that: The carbon nanotubes have a diameter of 7-11 nm and a length of 5-20 μm; or The carbon nanotubes have a diameter of 10-20 nm and a length of 10-30 μm.
10. The carbon nanotube slurry according to any one of claims 7 to 9, characterized in that: In the carbon nanotube slurry, the mass percentage of the carbon nanotube dispersant is 0.1-2%.