Polypeptide hydrogel for solar interface evaporation and preparation method thereof

By depositing silver quantum dots on the surface of high entropy oxide plasma nanoparticles and combining with peptide modification, a polypeptide hydrogel with high photothermal conversion efficiency was prepared, which solved the problem of low evaporation efficiency of solar interfaces in the prior art, and achieved the Highly efficient solar energy utilization under limited conditions.

CN119039641APending Publication Date: 2024-11-29GUANGDONG UNIV OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411170425.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently capture and convert solar energy under limited conditions, especially in non-day or sunny days, where the solar interface evaporation efficiency is low and it is difficult to meet the demand for renewable energy.

Method used

By depositing silver quantum dots on the surface of high-entropy oxide plasma nanoparticles and chemically crosslinking with carboxyl and amine polypeptides, a polypeptide hydrogel with photothermal conversion ability was prepared, and gaseous media-induced deposition technology and Hydroxylation strategy to form materials with high photothermal conversion efficiency.

Benefits of technology

It realizes efficient absorption of solar energy and converts it into thermal energy in a limited environment, improves the efficiency and stability of solar interface evaporation, and enhances the ability to utilize solar energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039641A_ABST
    Figure CN119039641A_ABST
Patent Text Reader

Abstract

The invention discloses polypeptide hydrogel for solar interface evaporation and a preparation method of the polypeptide hydrogel. The method comprises the following steps: modifying Ag nanoparticles on high-entropy oxide plasma nanoparticles by using a gaseous medium induced deposition technology to enhance a plasma photothermal effect; the preparation method comprises the following steps: modifying polypeptides with carboxyl amino acids and amino amino acids respectively, mixing the two modified polypeptides, and carrying out chemical crosslinking to form the polypeptide hydrogel; and dispersing the modified metal oxide nanoparticles in a water-based adhesive, uniformly coating the surface of the polypeptide hydrogel with the water-based adhesive, and fixing the metal oxide nanoparticles on the surface of the polypeptide hydrogel after water is volatilized to obtain the polypeptide hydrogel with photothermal conversion capability. The polypeptide hydrogel prepared by the method is applied to the field of solar interface evaporation, and water is evaporated after sunlight is absorbed by the polypeptide hydrogel and converted into heat energy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of soft matter energy materials and relates to a polypeptide hydrogel, in particular to a polypeptide hydrogel for solar energy interface evaporation and a preparation method thereof. Background Art

[0002] As the global demand for renewable energy continues to increase, solar energy has received widespread attention as a clean and sustainable energy source. Especially in the context of climate change and the increasing importance of environmental protection, the development of efficient solar energy conversion systems is particularly urgent. Interfacial evaporation technology shows great potential in the utilization of solar energy and can achieve efficient thermal energy conversion and transmission. However, the intensity of solar energy is limited by the environment and can only achieve better results during the day and on sunny days. How to capture more sunlight under limited conditions and better convert the captured sunlight into thermal energy for interfacial evaporation is also a severe challenge. Summary of the invention

[0003] The first object of the present invention is to provide a method for preparing polypeptide hydrogel for solar interfacial evaporation.

[0004] The second object of the present invention is to provide a polypeptide hydrogel for solar interfacial evaporation prepared by the above preparation method, which has extremely high light-to-heat conversion efficiency.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] In a first aspect, the present invention provides a method for preparing a polypeptide hydrogel for solar interfacial evaporation, comprising the following steps:

[0007] (1) Deposition of silver (Ag) quantum dots on the surface of high entropy oxide plasma nanoparticles

[0008] Using gaseous medium induced deposition technology, Ag quantum dots are precisely embedded on the surface of nano-scale particles: first, high entropy oxide plasma nanoparticles rich in multi-components are ultrasonically dispersed in water; then, AgNO3 solution is added, stirred under a reducing gas flow, filtered, washed to remove surface residues, and then dried; the concentration of the AgNO3 solution is 0.1M-0.5M;

[0009] (2) Modifying horseshoe crab-derived polypeptides to obtain precursor solutions and prepare gels

[0010] Carboxyl-containing amino acids and amine-containing amino acids are used to carry out directed modification of horseshoe crab-derived polypeptides to obtain carboxyl-type polypeptides and amine-type polypeptides, and the two modified polypeptides are mixed to obtain a polypeptide hydrogel with water transport capability under the action of chemical cross-linking; the volume ratio of the carboxyl-type polypeptide and the amine-type polypeptide when mixed is 1-5;

[0011] (3) Adding high entropy oxide plasma to the aqueous adhesive and then coating it on the hydrogel

[0012] The horseshoe crab protein is modified by hydroxylation strategy to derive a water-based adhesive; the high entropy oxide plasma nanoparticles modified in step (1) are ultrasonically dispersed into the water-based adhesive to obtain a high entropy oxide plasma dispersion, wherein the mass percentage of the high entropy oxide plasma nanoparticles is 0.5-1.0wt%; the dispersion is then evenly coated on the surface of the polypeptide hydrogel, and the water in the water-based adhesive is removed by heating to obtain a polypeptide hydrogel with photothermal conversion capability.

[0013] Preferably, the high entropy oxide plasma nanoparticles are selected from (CoCrFeMnNi)O, Gd2Ti2O7, Y2Ti2O7, CaMnO3, La2Zr2O7, Ba 0.5 Sr 0.5 Co 0.8 Fe 0.2 One or more of O3.

[0014] Preferably, the reducing gas is selected from one of H2, SO2, CO, H2S, and CH4.

[0015] Preferably, the carboxyl-containing amino acid is selected from one of α-aminoisobutyric acid, β-alanine, salicylic acid, γ-aminobutyric acid, and aconitic acid.

[0016] Preferably, the amino acid containing an amine group is selected from one of glucosamine, cystine, mecosine, 6-aminocaproic acid and dopamine.

[0017] Preferably, the coating amount of the dispersion on the polypeptide hydrogel in step (3) is 0.5-2 mL / cm 2 .

[0018] In a second aspect, the present invention also provides a polypeptide hydrogel for solar interfacial evaporation prepared by the above preparation method.

[0019] Compared with the prior art, the present invention provides a new idea of ​​combining polypeptide hydrogel with solar clean energy. High entropy oxide plasma as a photothermal conversion material has a wide solar absorption spectrum, high photothermal conversion efficiency and high water evaporation rate, and polypeptide hydrogel has good structural stability and efficient water transport performance. The present invention combines the modified high entropy oxide plasma nanoparticles with polypeptide hydrogel, which can absorb more solar radiation under the same environment, and obtain extremely high photothermal conversion efficiency to achieve the purpose of efficient solar interface evaporation, thereby improving the utilization of solar energy under limited environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 1.

[0021] Figure 2 This is a real picture of the polypeptide hydrogel with photothermal conversion capability in Example 1.

[0022] Figure 3 This is a graph of the evaporation rate of the polypeptide hydrogel of Examples 1-8 under 1 times the sunlight intensity.

[0023] Figure 4 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 2.

[0024] Figure 5 This is a real picture of the polypeptide hydrogel with photothermal conversion capability in Example 2.

[0025] Figure 6 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 3.

[0026] Figure 7 This is a real picture of the polypeptide hydrogel with photothermal conversion capability in Example 3.

[0027] Figure 8 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 4.

[0028] Fig. 9 This is a real picture of the polypeptide hydrogel with photothermal conversion capability in Example 4.

[0029] Fig.10 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 5.

[0030] Fig.11 This is a real picture of the polypeptide hydrogel with photothermal conversion capability in Example 5.

[0031] Fig.12 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 6.

[0032] Fig.13 This is a real picture of the polypeptide hydrogel with photothermal conversion capability in Example 6.

[0033] Fig.14 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 7.

[0034] Fig.15 This is a real picture of the polypeptide hydrogel with photothermal conversion capability in Example 7.

[0035] Fig.16This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 8.

[0036] Fig.17 This is a real picture of the polypeptide hydrogel with photothermal conversion capability in Example 8. DETAILED DESCRIPTION

[0037] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0038] The horseshoe crab-derived proteins and horseshoe crab-derived polypeptides used in the following examples were obtained by the following method:

[0039] Water-based extraction technology is applied to the muscle fiber tissue of the American horseshoe crab of Delaware to separate and extract the horseshoe crab protein with high purity; then, with the help of the decomposition mechanism mediated by biocatalytic enzymes, the shell structure of the American horseshoe crab of Delaware is deeply hydrolyzed to accurately obtain the horseshoe crab polypeptide components contained therein. Both water-based extraction technology and biocatalytic enzyme mediation adopt conventional technical means in this field.

[0040] Example 1

[0041] (1) Chemical surface modification of high entropy oxide plasma nanoparticles is performed as follows:

[0042] 2 g (CoCrFeMnNi)O was introduced into 100 mL deionized water and dispersed evenly by ultrasonic vibration. 2 mL of 0.1 M AgNO3 solution was added to the dispersion system, followed by stirring for 30 min under H2 atmosphere. Finally, it was filtered, washed to remove surface residues and dried.

[0043] (2) Dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of α-aminoisobutyric acid to activate the carboxyl group of the horseshoe crab polypeptide at pH = 5 for 2 hours to obtain a carboxyl horseshoe crab polypeptide; dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of glucosamine to activate the amino group of the horseshoe crab polymorphism at pH = 5 for 2 hours to obtain an amino horseshoe crab polypeptide.

[0044] (3) 10 mL of carboxyl horseshoe crab-derived polypeptide and 10 mL of amino-based polypeptide were added into the mold at a volume ratio of 1:1 overnight; the carboxyl horseshoe crab-derived polypeptide and the amino horseshoe crab-derived polypeptide underwent chemical cross-linking reaction to obtain a polypeptide hydrogel.

[0045] (4) 0.1 g of high entropy oxide plasma (CoCrFeMnNi)O nanoparticles was introduced into 19.9 g of hydroxylated horseshoe crab protein solution and dispersed evenly by ultrasonic vibration to obtain a high entropy oxide plasma dispersion with adhesion.

[0046] (5) Take the above dispersion at a rate of 0.5 mL cm -2 An amount of the dispersion is coated on the surface of the polypeptide hydrogel, and after the water in the dispersion evaporates, a polypeptide hydrogel with photothermal conversion ability is obtained.

[0047] The obtained polypeptide hydrogel with photothermal conversion ability is placed in a water body. Under sunlight, the high entropy oxide plasma will capture the sunlight, convert the captured sunlight into thermal energy using the high photothermal conversion efficiency, and evaporate the surface of the water body.

[0048] Figure 1 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 1. From the figure, it can be seen that the pores inside the polypeptide hydrogel are evenly distributed and have water transport capability.

[0049] Figure 2 This is a real picture of the polypeptide hydrogel with light-to-heat conversion capability in Example 1. It can be seen from the figure that the polypeptide hydrogel has a stable structure and can be used for solar interfacial evaporation.

[0050] Figure 3 The evaporation rate of the polypeptide hydrogel in Example 1 under 1 times the sunlight intensity is shown in Figure 1. The evaporation rate of the polypeptide hydrogel in Example 1 is 4.41 kg / m -2 h -1 .

[0051] Example 2

[0052] (1) Chemical surface modification of high entropy oxide plasma nanoparticles is performed as follows:

[0053] 2 g (CoCrFeMnNi)O was introduced into 100 mL deionized water and dispersed evenly by ultrasonic vibration. 2 mL of 0.3 M AgNO3 solution was added to the dispersion system, followed by stirring for 30 min under H2 atmosphere. Finally, it was filtered, washed to remove surface residues and dried.

[0054] (2) Dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of α-aminoisobutyric acid to activate the carboxyl group of the horseshoe crab polypeptide at pH = 5 for 2 hours to obtain a carboxyl horseshoe crab polypeptide; dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of glucosamine to activate the amino group of the horseshoe crab polymorphism at pH = 5 for 2 hours to obtain an amino horseshoe crab polypeptide.

[0055] (3) 10 mL of carboxyl horseshoe crab-derived polypeptide and 10 mL of amino-based polypeptide were added into the mold at a volume ratio of 1:1 overnight; the carboxyl horseshoe crab-derived polypeptide and the amino horseshoe crab-derived polypeptide underwent chemical cross-linking reaction to obtain a polypeptide hydrogel.

[0056] (4) 0.1 g of high entropy oxide plasma (CoCrFeMnNi)O nanoparticles was introduced into 19.9 g of hydroxylated horseshoe crab protein solution and dispersed evenly by ultrasonic vibration to obtain a high entropy oxide plasma dispersion with adhesion.

[0057] (5) Take the above dispersion at a rate of 0.5 mL cm -2 An amount of the dispersion is coated on the surface of the polypeptide hydrogel, and after the water in the dispersion evaporates, a polypeptide hydrogel with photothermal conversion ability is obtained.

[0058] The obtained polypeptide hydrogel with photothermal conversion ability is placed in a water body. Under sunlight, the high entropy oxide plasma will capture the sunlight, convert the captured sunlight into thermal energy using the high photothermal conversion efficiency, and evaporate the surface of the water body.

[0059] Figure 4 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 2. From the figure, it can be seen that the pores inside the polypeptide hydrogel are evenly distributed and have water transport capability.

[0060] Figure 5 This is a real picture of the polypeptide hydrogel with light-to-heat conversion capability in Example 2. It can be seen from the figure that the polypeptide hydrogel has a stable structure and can be used for solar interfacial evaporation.

[0061] Figure 3 The evaporation rate of the polypeptide hydrogel in Example 2 under 1 times the sunlight intensity is shown in Figure 2. The evaporation rate of the polypeptide hydrogel in Example 2 is 4.73 kg / m -2 h -1 .

[0062] Example 3

[0063] (1) Chemical surface modification of high entropy oxide plasma nanoparticles is performed as follows:

[0064] 2 g (CoCrFeMnNi)O was introduced into 100 mL deionized water and dispersed evenly by ultrasonic vibration. 2 mL of 0.5 M AgNO3 solution was added to the dispersion system, followed by stirring for 30 min under H2 atmosphere. Finally, it was filtered, washed to remove surface residues and dried.

[0065] (2) Dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of α-aminoisobutyric acid to activate the carboxyl group of the horseshoe crab polypeptide at pH = 5 for 2 hours to obtain a carboxyl horseshoe crab polypeptide; dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of glucosamine to activate the amino group of the horseshoe crab polymorphism at pH = 5 for 2 hours to obtain an amino horseshoe crab polypeptide.

[0066] (3) 10 mL of carboxyl horseshoe crab-derived polypeptide and 10 mL of amino-based polypeptide were added into the mold at a volume ratio of 1:1 overnight. The carboxyl horseshoe crab-derived polypeptide and the amino horseshoe crab-derived polypeptide underwent chemical cross-linking reaction to obtain polypeptide hydrogel.

[0067] (4) 0.1 g of high entropy oxide plasma (CoCrFeMnNi)O nanoparticles was introduced into 19.9 g of hydroxylated horseshoe crab protein solution and dispersed evenly by ultrasonic vibration to obtain a high entropy oxide plasma dispersion with adhesion.

[0068] (5) Take the above dispersion at a rate of 0.5 mL cm -2 An amount of the dispersion is coated on the surface of the polypeptide hydrogel, and after the water in the dispersion evaporates, a polypeptide hydrogel with photothermal conversion ability is obtained.

[0069] The obtained polypeptide hydrogel with photothermal conversion ability is placed in a water body. Under sunlight, the high entropy oxide plasma will capture the sunlight, convert the captured sunlight into thermal energy using the high photothermal conversion efficiency, and evaporate the surface of the water body.

[0070] Figure 6 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 3. From the figure, it can be seen that the pores inside the polypeptide hydrogel are evenly distributed and have water transport capability.

[0071] Figure 7 This is a real picture of the polypeptide hydrogel with light-to-heat conversion capability in Example 3. It can be seen from the figure that the polypeptide hydrogel has a stable structure and can be used for solar interfacial evaporation.

[0072] Figure 3 The evaporation rate of the polypeptide hydrogel in Example 3 under 1 times the sunlight intensity is shown in Figure 3. The evaporation rate of the polypeptide hydrogel in Example 3 is 4.88 kg / m -2 h -1 .

[0073] Example 4

[0074] (1) Chemical surface modification of high entropy oxide plasma nanoparticles is performed as follows:

[0075] 2 g (CoCrFeMnNi)O was introduced into 100 mL deionized water and dispersed evenly by ultrasonic vibration. 2 mL of 0.1 M AgNO3 solution was added to the dispersion system, followed by stirring for 30 min under H2 atmosphere. Finally, it was purified and washed to remove surface residues and dried.

[0076] (2) Dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of α-aminoisobutyric acid to activate the carboxyl group of the horseshoe crab polypeptide at pH = 5 for 2 hours to obtain a carboxyl horseshoe crab polypeptide; dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of glucosamine to activate the amino group of the horseshoe crab polymorphism at pH = 5 for 2 hours to obtain an amino horseshoe crab polypeptide.

[0077] (3) 5 mL of carboxyl horseshoe crab-derived polypeptide and 15 mL of amino-based polypeptide were added to the mold at a volume ratio of 1:3 and left overnight. The carboxyl horseshoe crab-derived polypeptide and the amino horseshoe crab-derived polypeptide underwent chemical cross-linking reaction to obtain polypeptide hydrogel.

[0078] (4) 0.1 g of high entropy oxide plasma (CoCrFeMnNi)O nanoparticles was introduced into 19.9 g of hydroxylated horseshoe crab protein solution and dispersed evenly by ultrasonic vibration to obtain a high entropy oxide plasma dispersion with adhesion.

[0079] (5) Take the above dispersion at a rate of 0.5 mL cm -2 An amount of the dispersion is coated on the surface of the polypeptide hydrogel, and after the water in the dispersion evaporates, a polypeptide hydrogel with photothermal conversion ability is obtained.

[0080] The obtained polypeptide hydrogel with photothermal conversion ability is placed in a water body. Under sunlight, the high entropy oxide plasma will capture the sunlight, convert the captured sunlight into thermal energy using the high photothermal conversion efficiency, and evaporate the surface of the water body.

[0081] Figure 8 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 4. From the figure, it can be seen that the pores inside the polypeptide hydrogel are evenly distributed and have water transport capability.

[0082] Fig. 9 This is a real picture of the polypeptide hydrogel with light-to-heat conversion capability in Example 4. From the figure, it can be seen that the polypeptide hydrogel has a stable structure and can be used for solar interfacial evaporation.

[0083] Figure 3 The evaporation rate of the polypeptide hydrogel in Example 4 under 1 times the sunlight intensity is shown in Figure 4. The evaporation rate of the polypeptide hydrogel in Example 4 is 4.32 kg / m -2 h -1 .

[0084] Example 5

[0085] (1) Chemical surface modification of high entropy oxide plasma nanoparticles is performed as follows:

[0086] 2 g (CoCrFeMnNi)O was introduced into 100 mL deionized water and dispersed evenly by ultrasonic vibration. 2 mL of 0.1 M AgNO3 solution was added to the dispersion system, followed by stirring for 30 min under H2 atmosphere. Finally, it was filtered, washed to remove surface residues and dried.

[0087] (2) Dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of α-aminoisobutyric acid to activate the carboxyl group of the horseshoe crab polypeptide at pH = 5 for 2 hours to obtain a carboxyl horseshoe crab polypeptide; dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of glucosamine to activate the amino group of the horseshoe crab polymorphism at pH = 5 for 2 hours to obtain an amino horseshoe crab polypeptide.

[0088] (3) 3.33 mL of carboxyl horseshoe crab-derived polypeptide and 16.67 mL of amino-based polypeptide were added to the mold at a volume ratio of 1:5 and left overnight. The carboxyl horseshoe crab-derived polypeptide and the amino horseshoe crab-derived polypeptide underwent chemical cross-linking reaction to obtain polypeptide hydrogel.

[0089] (4) 0.1 g of high entropy oxide plasma (CoCrFeMnNi)O nanoparticles was introduced into 19.9 g of hydroxylated horseshoe crab protein solution and dispersed evenly by ultrasonic vibration to obtain a high entropy oxide plasma dispersion with adhesion.

[0090] (5) Take the above dispersion at a rate of 0.5 mL cm -2 An amount of the dispersion is coated on the surface of the polypeptide hydrogel, and after the water in the dispersion evaporates, a polypeptide hydrogel with photothermal conversion ability is obtained.

[0091] The obtained polypeptide hydrogel with photothermal conversion ability is placed in a water body. Under sunlight, the high entropy oxide plasma will capture the sunlight, convert the captured sunlight into thermal energy using the high photothermal conversion efficiency, and evaporate the surface of the water body.

[0092] Fig.10 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 5. From the figure, it can be seen that the pores inside the polypeptide hydrogel are evenly distributed and have water transport capability.

[0093] Fig.11 This is a real picture of the polypeptide hydrogel with light-to-heat conversion capability in Example 5. From the figure, it can be seen that the polypeptide hydrogel has a stable structure and can be used for solar interfacial evaporation.

[0094] Figure 3 The evaporation rate of the polypeptide hydrogel in Example 5 under 1 times the sunlight intensity is shown in Figure 2. The evaporation rate of the polypeptide hydrogel in Example 5 is 3.81 kg / m -2 h -1 .

[0095] Example 6

[0096] (1) Chemical surface modification of high entropy oxide plasma nanoparticles is performed as follows:

[0097] 2 g (CoCrFeMnNi)O was introduced into 100 mL deionized water and dispersed evenly by ultrasonic vibration. 2 mL of 0.1 M AgNO3 solution was added to the dispersion system, followed by stirring for 30 min under H2 atmosphere. Finally, it was filtered, washed to remove surface residues and dried.

[0098] (2) Dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of α-aminoisobutyric acid to activate the carboxyl group of the horseshoe crab polypeptide at pH = 5 for 2 hours to obtain a carboxyl horseshoe crab polypeptide; dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of glucosamine to activate the amino group of the horseshoe crab polymorphism at pH = 5 for 2 hours to obtain an amino horseshoe crab polypeptide.

[0099] (3) 20 mL of carboxyl horseshoe crab-derived polypeptide and 20 mL of amino-based polypeptide were added into the mold at a volume ratio of 1:1 overnight. The carboxyl horseshoe crab-derived polypeptide and the amino horseshoe crab-derived polypeptide underwent chemical cross-linking reaction to obtain polypeptide hydrogel.

[0100] (4) 0.1 g of high entropy oxide plasma (CoCrFeMnNi)O nanoparticles was introduced into 19.9 g of hydroxylated horseshoe crab protein solution and dispersed evenly by ultrasonic vibration to obtain a high entropy oxide plasma dispersion with adhesion.

[0101] (5) Take the above dispersion at a rate of 0.5 mL cm -2 An amount of the dispersion is coated on the surface of the polypeptide hydrogel, and after the water in the dispersion evaporates, a polypeptide hydrogel with photothermal conversion ability is obtained.

[0102] The obtained polypeptide hydrogel with photothermal conversion ability is placed in a water body. Under sunlight, the high entropy oxide plasma will capture the sunlight, convert the captured sunlight into thermal energy using the high photothermal conversion efficiency, and evaporate the surface of the water body.

[0103] Fig.12 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 6. From the figure, it can be seen that the pores inside the polypeptide hydrogel are evenly distributed and have water transport capability.

[0104] Fig.13 This is a real picture of the polypeptide hydrogel with light-to-heat conversion capability in Example 6. It can be seen from the figure that the polypeptide hydrogel has a stable structure and can be used for solar interfacial evaporation.

[0105] Figure 3 The evaporation rate of the polypeptide hydrogel in Example 6 under 1 times the sunlight intensity is shown in Figure 2. The evaporation rate of the polypeptide hydrogel in Example 6 is 3.56 kg / m -2 h -1 .

[0106] Example 7

[0107] (1) Chemical surface modification of high entropy oxide plasma nanoparticles is performed as follows:

[0108] 2 g (CoCrFeMnNi)O was introduced into 100 mL deionized water and dispersed evenly by ultrasonic vibration. 2 mL of 0.1 M AgNO3 solution was added to the dispersion system, followed by stirring for 30 min under H2 atmosphere. Finally, it was filtered, washed to remove surface residues and dried.

[0109] (2) Dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of α-aminoisobutyric acid to activate the carboxyl group of the horseshoe crab polypeptide at pH = 5 for 2 hours to obtain a carboxyl horseshoe crab polypeptide; dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of glucosamine to activate the amino group of the horseshoe crab polymorphism at pH = 5 for 2 hours to obtain an amino horseshoe crab polypeptide.

[0110] (3) 10 mL of carboxyl horseshoe crab-derived polypeptide and 10 mL of amino-based polypeptide were added into the mold at a volume ratio of 1:1 overnight. The carboxyl horseshoe crab-derived polypeptide and the amino horseshoe crab-derived polypeptide underwent chemical cross-linking reaction to obtain polypeptide hydrogel.

[0111] (4) 0.16 g of high entropy oxide plasma (CoCrFeMnNi)O nanoparticles were introduced into 19.84 g of hydroxylated horseshoe crab protein solution and dispersed evenly by ultrasonic vibration to obtain a high entropy oxide plasma dispersion with adhesion.

[0112] (5) Take the above dispersion according to 1 mL cm -2 An amount of the dispersion is coated on the surface of the polypeptide hydrogel, and after the water in the dispersion evaporates, a polypeptide hydrogel with photothermal conversion ability is obtained.

[0113] The obtained polypeptide hydrogel with photothermal conversion ability is placed in a water body. Under sunlight, the high entropy oxide plasma will capture the sunlight, convert the captured sunlight into thermal energy using the high photothermal conversion efficiency, and evaporate the surface of the water body.

[0114] Fig.14 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 7. From the figure, it can be seen that the pores inside the polypeptide hydrogel are evenly distributed and have water transport capability.

[0115] Fig.15 This is a real picture of the polypeptide hydrogel with light-to-heat conversion capability in Example 7. From the figure, it can be seen that the polypeptide hydrogel has a stable structure and can be used for solar interfacial evaporation.

[0116] Figure 3 The evaporation rate of the polypeptide hydrogel in Example 7 under 1 times the sunlight intensity is shown in Figure 2. The evaporation rate of the polypeptide hydrogel in Example 7 is 5.13 kg / m -2 h -1 .

[0117] Example 8

[0118] (1) Chemical surface modification of high entropy oxide plasma nanoparticles is performed as follows:

[0119] 2 g (CoCrFeMnNi)O was introduced into 100 mL deionized water and dispersed evenly by ultrasonic vibration. 2 mL of 0.1 M AgNO3 solution was added to the dispersion system, followed by stirring for 30 min under H2 atmosphere. Finally, it was filtered, washed to remove surface residues and dried.

[0120] (2) Dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of α-aminoisobutyric acid to activate the carboxyl group of the horseshoe crab polypeptide at pH = 5 for 2 hours to obtain a carboxyl horseshoe crab polypeptide; dissolve 0.5 g horseshoe crab polypeptide in 100 mL of deionized water, add 1 mmol of glucosamine to activate the amino group of the horseshoe crab polymorphism at pH = 5 for 2 hours to obtain an amino horseshoe crab polypeptide.

[0121] (3) 10 mL of carboxyl horseshoe crab-derived polypeptide and 10 mL of amino-based polypeptide were added into the mold at a volume ratio of 1:1 overnight. The carboxyl horseshoe crab-derived polypeptide and the amino horseshoe crab-derived polypeptide underwent chemical cross-linking reaction to obtain polypeptide hydrogel.

[0122] (4) 0.2 g of high entropy oxide plasma (CoCrFeMnNi)O nanoparticles were introduced into 19.8 g of hydroxylated horseshoe crab protein solution and dispersed evenly by ultrasonic vibration to obtain a high entropy oxide plasma dispersion with adhesion.

[0123] (5) Take the above dispersion at 2 mL cm -2 An amount of the dispersion is coated on the surface of the polypeptide hydrogel, and after the water in the dispersion evaporates, a polypeptide hydrogel with photothermal conversion ability is obtained.

[0124] The obtained polypeptide hydrogel with photothermal conversion ability is placed in a water body. Under sunlight, the high entropy oxide plasma will capture the sunlight, convert the captured sunlight into thermal energy using the high photothermal conversion efficiency, and evaporate the surface of the water body.

[0125] Fig.16 This is a scanning electron micrograph of the polypeptide hydrogel with photothermal conversion capability in Example 8. From the figure, it can be seen that the pores inside the polypeptide hydrogel are evenly distributed and have water transport capability.

[0126] Fig.17 This is a real picture of the polypeptide hydrogel with light-to-heat conversion capability in Example 8. It can be seen from the figure that the polypeptide hydrogel has a stable structure and can be used for solar interfacial evaporation.

[0127] Figure 3 The evaporation rate of the polypeptide hydrogel in Example 8 under 1 times the sunlight intensity is shown in Figure 1. The evaporation rate of the polypeptide hydrogel in Example 8 is 4.95 kg / m -2 h -1 .

[0128] Performance Test:

[0129] The indoor evaporation test was carried out under artificial light. The average irradiance on the sample surface was 1kW m -2 , measured by an optical power meter. In the evaporation test, the upper surface of the evaporator with the polypeptide hydrogel floating on the water surface was exposed to the open air. The indoor temperature was controlled at 26°C and the humidity was controlled at a relative humidity of 78%. The water loss mass was then measured every 5 minutes using a balance to obtain the evaporation rate. The absorbance of PB and OPB in the full solar spectrum was calculated using the solar radiation spectrum and the UV-visible-near infrared absorption spectrum. Using the experimental data, the photothermal conversion rate and energy utilization rate of Examples 1-8 can be obtained.

[0130] Table 1 Test results of the embodiment

[0131] Example Solar absorption rate Photothermal conversion rate Energy utilization Example 1 95.5% 94.6% 94.8% Example 2 96.7% 96.1% 96.1% Example 3 97.3% 97.3% 97.3% Example 4 95.5% 94.6% 94.8% Example 5 95.5% 94.6% 92.8% Example 6 95.5% 94.6% 91.1% Example 7 95.5% 95.7% 98.1% Example 8 95.5% 95.3% 97.6%

[0132] As can be seen from Table 1, as the concentration of added AgNO3 increases, the number of Ag quantum dots deposited on the surface of the high entropy oxide plasma increases, resulting in a polypeptide hydrogel with photothermal conversion ability having higher solar light absorption rate, photothermal conversion efficiency and energy utilization rate. In addition, as the volume of carboxyl horseshoe crab-derived polypeptides and amino horseshoe crab-derived polypeptides increases, thicker polypeptide hydrogels are obtained. These thicker polypeptide hydrogels have longer water transport channels, resulting in decreased energy utilization. When the volume ratio of carboxyl horseshoe crab-derived polypeptides and amino horseshoe crab-derived polypeptides is changed, the internal structure of the polypeptide hydrogel will be affected, thereby affecting the final evaporation rate. Finally, as the coating amount increases from 0.5 mL cm -2 to 2mLcm-2 , the photothermal conversion efficiency and energy utilization of the peptide hydrogel first increased and then decreased. This is because when the high entropy oxide plasma coating amount is small, the peptide hydrogel cannot capture enough sunlight for solar interfacial evaporation. When the high entropy oxide plasma coating amount is 2mL cm -2 When the amount of high entropy oxide plasma is too high, it will block the water channel, making it difficult for water vapor to escape. In summary, the optimal coating amount of high entropy oxide plasma is 1mLcm -2 .

[0133] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing polypeptide hydrogel for solar interfacial evaporation, characterized in that: It includes the following steps: (1) Using gaseous medium induced deposition technology, Ag quantum dots are precisely embedded on the surface of nano-scale particles: first, high entropy oxide plasma nanoparticles rich in multi-components are ultrasonically dispersed in water; then, AgNO3 solution is added, stirred under a reducing gas flow, filtered, washed to remove surface residues, and then dried; the concentration of the AgNO3 solution is 0.1M-0.5M; (2) using carboxyl-containing amino acids and amine-containing amino acids to modify horseshoe crab-derived polypeptides to obtain carboxyl polypeptides and amine polypeptides, respectively, mixing the two modified polypeptides, and obtaining a polypeptide hydrogel with water transport capability under chemical cross-linking; the volume ratio of the carboxyl polypeptides to the amine polypeptides when mixed is 1-5; (3) Modifying horseshoe crab-derived protein by hydroxylation strategy to derive a water-based adhesive; ultrasonically dispersing the modified high-entropy oxide plasma nanoparticles in the water-based adhesive to obtain a high-entropy oxide plasma dispersion, wherein the mass percentage of the high-entropy oxide plasma nanoparticles is 0.5-1.0wt%; and uniformly coating the dispersion on the surface of the polypeptide hydrogel, heating to remove water in the dispersion, thereby obtaining a polypeptide hydrogel with photothermal conversion capability.

2. The method for preparing a polypeptide hydrogel for solar interfacial evaporation according to claim 1, characterized in that: The high entropy oxide plasma nanoparticles are selected from (CoCrFeMnNi)O, Gd2Ti2O7, Y2Ti2O7, CaMnO3, La2Zr2O7, Ba 0.5 Sr 0.5 Co 0.8 Fe 0.2 One or more of O3.

3. The method for preparing a polypeptide hydrogel for solar interfacial evaporation according to claim 1, characterized in that: The reducing gas is selected from one of H2, SO2, CO, H2S, and CH4.

4. The method for preparing a polypeptide hydrogel for solar interfacial evaporation according to claim 1, characterized in that: The carboxyl-containing amino acid is selected from one of α-aminoisobutyric acid, β-alanine, salicylic acid, γ-aminobutyric acid, and aconitic acid.

5. The method for preparing a polypeptide hydrogel for solar interfacial evaporation according to claim 1, characterized in that: The amino acid containing an amine group is selected from one of glucosamine, cystine, mecosine, 6-aminocaproic acid and dopamine.

6. The method for preparing a polypeptide hydrogel for solar interfacial evaporation according to claim 1, characterized in that: The coating amount of the dispersion on the polypeptide hydrogel in step (3) is 0.5-2 mL / cm 2 .

7. A polypeptide hydrogel for solar interfacial evaporation prepared by the preparation method according to any one of claims 1 to 6.

Citation Information

Cited By

  • Laser-induced cationic polypeptide cluster compound gas-phase preparation method

    CN122524524A

  • A method for laser-induced cationic polypeptide cluster complex gas-phase production

    CN122524524B