Polar polyethylene material and preparation method thereof
By introducing polar monomers into ethylene-polar olefin copolymers and polymerizing using rare earth metallocene catalytic system, combining hot pressing molding and adding crosslinking agents, the non-polarity problem of traditional polyethylene materials is solved, and the combination of the two-dimensional polyethylene materials is improved. The blend compatibility and mechanical properties of polar materials achieve efficient modification of polar polyolefin materials.
Patent Information
- Application Number
- CN202410955660.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-29
AI Technical Summary
The non-polar characteristics of traditional polyethylene materials limit their blending and bonding with other polar materials, resulting in limited application areas. Existing modification methods such as post-functionalization is harsh and inefficient, vinyl polar olefin copolymers The synthesis conditions are strict, which leads to rare reports in commercial polyethylene as an additive.
By introducing 5.9 mol% to 70.0 mol% of polar monomer into the ethylene-polar olefin copolymer, coordination polymerization is performed using a rare earth metallocene catalytic system to synthesize the ethylene-polar olefin copolymer and obtain the ethylene-polar olefin copolymer by hot pressing molding Polar polyethylene material, with crosslinking agents and antioxidants added to improve mechanical and surface properties.
It significantly improves the compatibility and interface effect of ethylene-polar olefin copolymers with commercial polyethylene, improves the surface and mechanical properties of polyethylene materials, enhances the blend compatibility with polar materials, and obtains good results. mechanical properties and surface properties.
Smart Images

Figure CN119039680A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polar polyolefin materials, and in particular relates to a polar polyethylene material and a preparation method thereof. Background Art
[0002] Polyethylene-based polymer materials are a large class of widely used polymer materials synthesized by homopolymerization of ethylene and copolymerization of ethylene with other monomers (such as styrene, α-olefins, cyclic olefins, etc.), including HDPE (high-density polyethylene), LDPE (low-density polyethylene), LLDPE (linear low-density polyethylene), POE (polyolefin elastomer) and other types, which are mainly used to manufacture various packaging materials, film materials, automotive parts, medical devices, etc. However, the non-polar characteristics of traditional polyethylene materials make them difficult to blend or bond with other polar materials (such as polar polymer materials, dyes, glass fibers, clay and metals, etc.), limiting the application areas of polyethylene-based polymer materials.
[0003] Introducing polar functional groups into polyolefins can solve the above problems, thereby improving the mechanical, electrical and processing properties of traditional polyolefins themselves and their adhesion, miscibility, conductivity, rheology and strength with polar materials. There are usually two methods for introducing polar functional groups into traditional polyethylene: (1) post-functionalization of polyethylene. (2) direct copolymerization of ethylene and polar olefins. Post-functionalization of polyethylene refers to chemical modification of commercial non-polar polyethylene materials, such as using free radical grafting reactions to attach polar groups to polyethylene chains. It usually requires harsh reaction conditions (temperature > 200°C), which will cause partial degradation and cross-linking of polyethylene. The post-functionalization method not only increases the production steps, but also has very limited varieties. The copolymerization of ethylene and polar olefins containing heteroatom groups is the most direct and effective method to introduce polar groups into the main chain of non-polar polyethylene, which is extremely challenging.
[0004] Compounding vinyl polar olefin copolymers with commercial polyethylene by melt blending is an efficient and economical way to improve the blending and adhesion of polyethylene with polar materials. However, due to the strict conditions required in the synthesis of vinyl polar olefin copolymers, there are few reports on the use of vinyl polar polyolefins as additives to modify commercial polyethylene. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a polar polyethylene material.
[0008] In order to solve the above technical problems, the present invention provides the following technical solution: the polar polyethylene material, in parts by mass, comprises:
[0009] 2 to 100 parts of ethylene-polar olefin copolymer;
[0010] 0-98 parts of polyethylene;
[0011] 0 to 5 parts of a cross-linking agent;
[0012] 0-0.2 parts of antioxidants;
[0013] Among them, the polar monomer insertion rate of the ethylene-polar olefin copolymer is 5.9 mol% to 70.0 mol%; the cross-linking agent includes one or more of BIPB, DCP, DPBMH, and DTBP; the antioxidant includes one or more of antioxidant 1010, antioxidant 1076, antioxidant 168, antioxidant B215, and antioxidant B225; and the degree of polymerization of the polyethylene is greater than 100.
[0014] As a preferred embodiment of the polar polyethylene material described in the present invention, the chain structure of the ethylene-polar olefin copolymer includes one or more of random, conical, gradient, block, and alternating structures; the stereo configuration of the copolymer monomer segment includes one or more of syndiotactic, isotactic, and amorphous.
[0015] As a preferred embodiment of the polar polyethylene material of the present invention, the preparation method of the ethylene-polar olefin copolymer is to coordinately polymerize ethylene and polar monomers through a catalytic system; the method comprises the following steps: under a nitrogen atmosphere, polar monomers and impurity removers are loaded into a reactor, ethylene is introduced into the reactor, the temperature is raised and stirred for 0.2 to 2 hours; a rare earth metallocene catalyst system is injected into the reactor at one time to carry out a polymerization reaction; the polymerization is terminated with a mixed solution of ethanol and hydrochloric acid, and the product is washed with ethanol and dried to a constant weight to obtain an ethylene-polar olefin copolymer; wherein the impurity remover comprises triisobutylaluminum.
[0016] As a preferred embodiment of the polar polyethylene material of the present invention, the polymerization reaction temperature is 20 to 100° C. and the polymerization reaction time is 0.2 to 48 hours.
[0017] As a preferred embodiment of the polar polyethylene material of the present invention, the catalytic system is a rare earth metallocene catalytic system, including an organic boron compound or its salt compound, an organic aluminum compound and a rare earth metal complex.
[0018] As a preferred embodiment of the polar polyethylene material described in the present invention, the organic boron compound or its salt compound includes one or more of [Ph3C][B(C6F5)4], [PhNMe2H][BPh4], [NEt3H][BPh4], [PhNMe2H][B(C6F5)4], and B(C6F5)3; the organic aluminum compound includes one or more of trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, triisopropylaluminum, triisobutylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum, trioctylaluminum, triphenylaluminum, tri-p-tolylaluminum, tribenzylaluminum, ethyldibenzylaluminum and ethyldi(p-tolyl)aluminum.
[0019] As a preferred embodiment of the polar polyethylene material of the present invention, the rare earth metal complex is selected from one or more compounds represented by formula I and formula II:
[0020]
[0021] In the formula, Ln is a rare earth metal; X is independently selected from S, P, O, and N atoms; and R is independently selected from hydrogen, halogen, C1-C5 alkyl, and substituted or unsubstituted aryl.
[0022] As a preferred embodiment of the polar polyethylene material of the present invention, the polar monomer is a polar styrene monomer, wherein the polar atoms in the polar monomer include one or more of O, S, N, P, halogen, and Se.
[0023] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a polar polyethylene material.
[0024] In order to solve the above technical problems, the present invention provides the following technical solution, including: mixing the raw materials evenly and hot pressing to obtain the polar polyethylene material; wherein the hot pressing temperature is 170-185°C and the pressure is 10-20MPa.
[0025] As a preferred embodiment of the method for preparing the polar polyethylene material of the present invention, the mixing comprises first mixing at a rotation speed of 60 to 100 r / min for 2 to 5 min, and then mixing at a rotation speed of 100 to 130 r / min for 5 to 10 min; wherein the mixing temperature is 110 to 185°C.
[0026] Beneficial effects of the present invention:
[0027] (1) The present invention improves the compatibility and interfacial interaction between the ethylene-polar olefin copolymer and the commercial polyethylene matrix through the ethylene chain segments contained in the ethylene-polar olefin copolymer.
[0028] (2) The present invention improves the surface properties of commercial polyethylene materials and their blending compatibility with polar materials through the polar groups contained in the ethylene-polar olefin copolymer.
[0029] (3) The present invention improves the mechanical properties of the composite material by using a cross-linking agent.
[0030] (4) The polar polyolefin material prepared by the present invention has good mechanical properties, surface properties and blending compatibility with polar materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. Among them:
[0032] Figure 1 This is the H NMR spectrum of the material prepared in Example 1 of the present invention;
[0033] Figure 2 This is a scanning electron microscope image of the material prepared in Example 2 of the present invention;
[0034] Figure 3 This is a graph showing the mechanical properties test results of the material prepared in Example 2 of the present invention;
[0035] Figure 4 This is a graph showing the surface performance test results of the material prepared in Example 2 of the present invention;
[0036] Figure 5 This is a scanning electron microscope image of the material prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0038] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0039] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0040] The raw materials used in the present invention are all commercially available unless otherwise specified.
[0041] Polyethylene is commercial polyethylene purchased from Yanshan Petrochemical, model 5000s.
[0042] The performance of the material prepared in the embodiment of the present invention was tested as follows:
[0043] 1) Determination of mechanical properties: The material was cold pressed at 10 MPa and cut into dumbbell-shaped specimens (length × width × thickness: 15 mm × 2 mm × 1 mm). The tensile strength and elongation at break of the material were measured by a WSM-20KN universal testing machine (Changchun Intelligent Instrument Equipment Co., Ltd.) at a tensile rate of 50 mm / min.
[0044] 2) Determination of surface properties: The material was cold pressed at 10 MPa to obtain a 1 mm thick film, and the water contact angle of the material was tested by a DSA 100S contact angle tester (Krues, Germany).
[0045] Example 1
[0046] This embodiment provides a method for preparing a polar polyethylene material, specifically:
[0047] (1) Preparation of catalyst: an organic boron compound [Ph3C][B(C6F5)4], an organic aluminum compound triisobutylaluminum, and a rare earth metal complex {(C7HS-Me2-Ph-SiMe3)Sc(CH2SiMe3)2(THF)} were uniformly mixed in a molar ratio of 1:10:1 and dissolved in a toluene solution for later use.
[0048] (2) Preparation of ethylene-m-methoxystyrene copolymer: m-methoxystyrene (0.62 g, 5 mmol) and a toluene solution of triisobutylaluminum (0.5 M, 0.2 ml) were placed in a glass kettle under a nitrogen atmosphere. The glass kettle was connected to an ethylene pipeline, and the gas in the kettle was replaced with ethylene gas (4 bar). The temperature was raised to 40°C and stirring was continued for 0.5 h. The prepared catalyst toluene solution (0.0059 g, 10 μmol) was injected into the glass kettle at once through a syringe. After the polymerization reaction lasted for 1 h, the polymerization was terminated with a mixed solution of ethanol and hydrochloric acid (hydrochloric acid content 10 wt%). The obtained product was washed three times with an ethanol solution and then vacuum dried at 40°C to constant weight; 0.60 g of a product with a molecular weight of 3.3×10 4g / mol, a molecular weight distribution of 1.4, and an ethylene-m-methoxystyrene copolymer with a polar monomer insertion rate of 11.5 mol%.
[0049] (3) Ethylene-m-methoxystyrene copolymer is hot-pressed at 170°C and 15 MPa to obtain a polar polyethylene material.
[0050] Figure 1 This is the hydrogen NMR spectrum of the material prepared in Example 1 of the present invention.
[0051] Example 2
[0052] The ethylene-m-methoxystyrene copolymer prepared in Example 1 (2 parts), commercial polyethylene (98 parts), and antioxidant 1010 (0.1 parts) were weighed, mixed at 170°C at a speed of 60 r / min for 3 minutes, and then at a speed of 100 r / min for 7 minutes. The mixture was hot-pressed at 170°C and a pressure of 15 MPa to obtain a polar polyethylene material.
[0053] Figure 2 This is a scanning electron microscope image of the material prepared in Example 2 of the present invention. Figure 3 This is a graph showing the mechanical properties test results of the copolymer prepared in Example 2 of the present invention. It can be seen that adding only 2 parts of the vinyl polar olefin copolymer can achieve the enhancement of commercial polyethylene, indicating the beneficial effect of the vinyl polar olefin copolymer on the mechanical properties of commercial polyethylene.
[0054] Figure 4 This is a graph showing the surface properties test results of the copolymer prepared in Example 2 of the present invention. It can be seen that compared with the water contact angle of 94.8° of commercial polyethylene, the water contact angle of the polar blend to which 2 parts of vinyl polar olefin copolymer are added is greatly reduced, indicating the beneficial effect of vinyl polar olefin copolymer on improving the surface properties of commercial polyethylene.
[0055] Example 3
[0056] The ethylene-m-methoxystyrene copolymer prepared in Example 1 (2 parts), commercial polyethylene (98 parts), crosslinking agent BIPB (0.9 parts), antioxidant 1010 (0.1 parts) were weighed, mixed at 120°C at a speed of 60 r / min for 3 minutes, and then at a speed of 100 r / min for 7 minutes. The mixture was hot-pressed at 170°C and a pressure of 15 MPa to obtain a polar polyethylene material.
[0057] Figure 5 This is a scanning electron microscope image of the material prepared in Example 3 of the present invention. The performance test of the material prepared in the above example is carried out, and the comparison results with Example 1 are shown in Table 1.
[0058] Table 1
[0059] Tensile strength(MPa) Water contact angle (°) Example 1 34.4 78.8 Example 2 41.2 81.0 Example 3 44.9 81.2 Commercial Polyethylene 37.8 94.8
[0060] As can be seen from the above table, blending vinyl polar olefin copolymers with commercial polyethylene can significantly increase the surface properties and mechanical properties of commercial polyethylene. This is because the introduction of polar atoms and benzene ring rigid structures increases the polarity and rigidity of polyethylene materials. After adding a cross-linking agent to the blended material, the mechanical properties of the blended material are further improved. This is because after cross-linking, chemical chain bridges are built between polyethylene molecules to form a network and body structure, which prevents the molecules from shifting, thereby improving the mechanical properties of the material.
[0061] Example 4
[0062] The difference between this embodiment and embodiment 3 is that the polar monomer insertion rate of the ethylene-m-methoxystyrene copolymer is adjusted to 5.9 mol %, and the rest of the preparation process is the same as that of embodiment 3 to obtain a polar polyethylene material.
[0063] Example 5
[0064] The difference between this embodiment and embodiment 3 is that the polar monomer insertion rate of the ethylene-m-methoxystyrene copolymer is adjusted to 7.2 mol %, and the rest of the preparation process is the same as that of embodiment 3 to obtain a polar polyethylene material.
[0065] Example 6
[0066] The difference between this embodiment and embodiment 3 is that the polar monomer insertion rate of the ethylene-m-methoxystyrene copolymer is adjusted to 70.0 mol %, and the rest of the preparation process is the same as that of embodiment 3 to obtain a polar polyethylene material.
[0067] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 3 are shown in Table 2.
[0068] Table 2
[0069]
[0070]
[0071] As can be seen from the above table, adjusting the insertion rate of polar monomers in ethylene-polar olefin copolymers has a significant effect on the performance of polar polyethylene materials. This is because as the insertion rate of polar monomers increases, the rigid structure of the introduced benzene rings increases, and the reinforcing effect on polyethylene increases. The increase in polar atoms in the material improves its surface properties. According to the results in the above table, the best technical effect can be obtained when the insertion rate of polar monomers in the present invention is 11.5 mol%.
[0072] Example 7
[0073] The difference between this embodiment and embodiment 3 is that the ratio of commercial polyethylene / polar polyolefin blend is adjusted from (98 parts / 2 parts) to (97 parts / 3 parts), and the rest of the preparation process is the same as that of embodiment 3 to obtain a polar polyethylene material.
[0074] Example 8
[0075] The difference between this embodiment and embodiment 3 is that the ratio of commercial polyethylene / polar polyolefin blend is adjusted from (98 parts / 2 parts) to (95 parts / 5 parts), and the rest of the preparation process is the same as that of embodiment 3 to obtain a polar polyethylene material.
[0076] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 3 are shown in Table 3.
[0077] Table 3
[0078] Tensile strength(MPa) Water contact angle (°) Example 3 44.9 81.2 Example 7 42.5 81.1 Example 8 40.9 80.2
[0079] As can be seen from the above table, adjusting the ratio of commercial polyethylene / polar polyolefin blends has a significant effect on the properties of polar polyethylene materials, because the content of polar atoms in the blended material increases and its surface properties are greatly improved. According to the results in the above table, the best technical effect can be obtained when the ratio of commercial polyethylene / polar polyolefin blends in the present invention is 95 parts / 5 parts.
[0080] Example 9
[0081] The difference between this embodiment and embodiment 3 is that the amount of the cross-linking agent BIPB is adjusted to 0.6 parts, and the rest of the preparation process is the same as that of embodiment 3 to obtain a polar polyethylene material.
[0082] Example 10
[0083] The difference between this embodiment and embodiment 3 is that the amount of the cross-linking agent BIPB is adjusted to 0.3 parts, and the rest of the preparation process is the same as that of embodiment 3 to obtain a polar polyethylene material.
[0084] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 4.
[0085] Table 4
[0086] Tensile strength(MPa) Water contact angle (°) Example 3 44.9 81.2 Example 9 43.5 80.8 Example 10 42.4 80.7
[0087] As can be seen from the table above, adjusting the amount of crosslinking agent BIPB has a significant effect on the performance of polar polyethylene materials. This is because as the amount of crosslinking agent decreases, the crosslinking effect weakens and the mechanical properties decrease. According to the results in the table above, the best technical effect can be obtained when the amount of crosslinking agent BIPB in the present invention is 0.9 parts.
[0088] Embodiment 11
[0089] The difference between this embodiment and embodiment 3 is that the blending time is adjusted to 60 r / min for 1 min and 100 r / min for 4 min, and the rest of the preparation process is the same as that of embodiment 3 to obtain a polar polyethylene material.
[0090] Example 12
[0091] The difference between this embodiment and embodiment 3 is that the blending time is adjusted to 60 r / min for 2 min and 100 r / min for 5 min, and the rest of the preparation process is the same as that of embodiment 3 to obtain a polar polyethylene material.
[0092] The performance of the material prepared in the above embodiment was tested, and the comparison results with those in Example 1 are shown in Table 5.
[0093] Table 5
[0094] Tensile strength(MPa) Water contact angle (°) Example 3 44.9 81.2 Embodiment 11 39.5 81.1 Example 12 40.6 81.0
[0095] As can be seen from the table above, adjusting the blending time has a significant effect on the performance of the polar polyethylene material, which is due to insufficient blending time and severe phase separation. According to the results in the table above, the best technical effect can be obtained when the blending time in the present invention is 60r / min for 3min and 100r / min for 7min.
[0096] Comparative Example 1
[0097] The difference between this comparative example and Example 3 is that the raw material ethylene-m-methoxystyrene copolymer is adjusted to ethylene-styrene copolymer, and the molecular weight of ethylene-styrene copolymer is 8.6×10 4 g / mol, the molecular weight distribution is 1.5, the polar monomer insertion rate is 11.0 mol%, and the rest of the preparation process is the same as that in Example 3 to obtain a non-polar polyethylene material.
[0098] Comparative Example 2
[0099] The difference between this comparative example and Example 3 is that the raw material ethylene-m-methoxystyrene copolymer is adjusted to ethylene-styrene copolymer, and the molecular weight of ethylene-styrene copolymer is 9.4×10 4 g / mol, the molecular weight distribution is 1.4, the polar monomer insertion rate is 12.4 mol%, and the rest of the preparation process is the same as that in Example 3 to obtain a non-polar polyethylene material.
[0100] Comparative Example 3
[0101] The difference between this comparative example and Example 3 is that the raw material ethylene-m-methoxystyrene copolymer is adjusted to ethylene-styrene copolymer, and the molecular weight of ethylene-styrene copolymer is 10.3×10 4 g / mol, the molecular weight distribution is 1.3, the polar monomer insertion rate is 13.2 mol%, and the rest of the preparation process is the same as that in Example 3 to obtain a non-polar polyethylene material.
[0102] The performance of the material obtained in the above comparative example was tested, and the comparison results with those of Example 1 are shown in Table 6.
[0103] Table 6
[0104] Tensile strength(MPa) Water contact angle (°) Example 3 44.9 81.2 Comparative Example 1 39.4 92.2 Comparative Example 2 40.2 91.6 Comparative Example 3 41.0 90.8
[0105] It can be seen from the above table that when polar materials lack polar atoms, the surface properties of the materials are greatly reduced.
[0106] In summary, the present invention improves the compatibility and interfacial interaction between the ethylene-polar olefin copolymer and the commercial polyethylene matrix through the ethylene chain segments contained in the ethylene-polar olefin copolymer; improves the surface properties of the commercial polyethylene material and its blending compatibility with polar materials through the polar groups contained in the ethylene-polar olefin copolymer; and improves the mechanical properties of the composite material through the crosslinking agent BIPB. The polar polyolefin material prepared by the present invention has good mechanical properties, surface properties and blending compatibility with polar materials.
[0107] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A polar polyethylene material, Features: The polar polyethylene material, in parts by mass, comprises: 2 to 100 parts of ethylene-polar olefin copolymer; 0-98 parts of polyethylene; 0 to 5 parts of a cross-linking agent; 0-0.2 parts of antioxidants; Among them, the polar monomer insertion rate of the ethylene-polar olefin copolymer is 5.9 mol% to 70.0 mol%; the cross-linking agent includes one or more of BIPB, DCP, DPBMH, and DTBP; the antioxidant includes one or more of antioxidant 1010, antioxidant 1076, antioxidant 168, antioxidant B215, and antioxidant B225; and the degree of polymerization of the polyethylene is greater than 100.
2. The polar polyethylene material according to claim 1, Features: The chain structure of the ethylene-polar olefin copolymer includes one or more of random, tapered, gradient, block, and alternating structures; the stereo configuration of the copolymer monomer segment includes one or more of syndiotactic, isotactic, and amorphous.
3. The polar polyethylene material according to claim 1, Features: The preparation method of the ethylene-polar olefin copolymer is to carry out coordination polymerization of ethylene and polar monomers through a catalytic system; The method comprises the following steps: under a nitrogen atmosphere, loading a polar monomer and an impurity remover into a reactor, introducing ethylene into the reactor, heating and stirring for 0.2 to 2 hours; injecting a rare earth metallocene catalyst system into the reactor at once to carry out a polymerization reaction; terminating the polymerization with a mixed solution of ethanol and hydrochloric acid, washing the product with ethanol, and drying to a constant weight to obtain an ethylene-polar olefin copolymer; wherein the impurity remover comprises triisobutylaluminum.
4. The polar polyethylene material according to claim 3, Features: The polymerization reaction temperature is 20-100° C. and the polymerization reaction time is 0.2-48 hours.
5. The polar polyethylene material according to claim 3, Features: The catalytic system is a rare earth metallocene catalytic system, which comprises an organic boron compound or a salt compound thereof, an organic aluminum compound and a rare earth metal complex.
6. The polar polyethylene material according to claim 5, Features: The organic boron compound or its salt compound includes [Ph 3 C][B(C 6 F 5 ) 4 ]、[PhNMe 2 H][BPh 4 ]、[NEt 3 H][BPh 4 ]、[PhNMe 2 H][B(C 6 F 5 ) 4 ]、B(C 6 F 5 ) 3 The organoaluminum compound comprises one or more of trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, triisopropylaluminum, triisobutylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum, trioctylaluminum, triphenylaluminum, tri-p-tolylaluminum, tribenzylaluminum, ethyldibenzylaluminum and ethyldi(p-tolyl)aluminum.
7. The polar polyethylene material according to claim 5, Features: The rare earth metal complex is selected from one or more compounds represented by formula I and formula II: In the formula, Ln is a rare earth metal; X is independently selected from S, P, O, and N atoms; and R is independently selected from hydrogen, halogen, C1-C5 alkyl, and substituted or unsubstituted aryl.
8. The method for preparing the polar polyethylene material according to claim 3, Features: The polar monomer is a polar styrene monomer, wherein the polar atoms in the polar monomer include one or more of O, S, N, P, halogen, and Se.
9. A method for preparing the polar polyethylene material as claimed in claim 1, Features: The method comprises the following steps: uniformly mixing various raw materials and hot pressing to obtain polar polyethylene material; wherein the hot pressing temperature is 170-185° C. and the pressure is 10-20 MPa.
10. The method for preparing the polar polyethylene material according to claim 9, Features: The mixing includes mixing at a rotation speed of 60 to 100 r / min for 2 to 5 min, and then mixing at a rotation speed of 100 to 130 r / min for 5 to 10 min; wherein the mixing temperature is 110 to 185°C.
Citation Information
Patent Citations
Ethylene-polar styrene quasi random copolymer and preparation method thereof
CN107141391A
Branched ethylene-polar styrene copolymer as well as preparation method and application thereof
CN115710327A
Flame-retardant insulating composition resistant to heat and radiation and electrical cable produced with the same
KR1020100092244A