PET (Polyethylene Terephthalate) composite foam board and preparation method thereof
Through the blending of PET and PBT resins and the addition of antioxidants and nucleating agents, the melt flowability and cell problems of PET/PBT composite materials during the production process are solved, and the number of cells, small pore sizes and mechanical properties are achieved. The preparation of good PET composite foam boards improves the crystallization performance and anti-aging ability of the material.
Patent Information
- Application Number
- CN202411385942.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
AI Technical Summary
During the production process, existing PET/PBT composite materials have high melt flow index and small viscosity, making it difficult to form high compressed and melt strength. The small crystallinity of PET materials leads to a small number of bubble cells, large pore size, and poor mechanical properties. Good question.
By blending PET and PBT resins, antioxidants, nucleating agents and chain extenders are added, and specific ratios and processing conditions (such as drying, high-speed stirring, twin-screw extrusion, etc.) are used to improve the crystallization performance of the material. , cell uniformity and mechanical properties, and CO2 is used as a foaming agent to control the cell size.
The PET composite foam board with a large number of bubble cells and uniform distribution, small pore size and good mechanical properties is achieved, which improves the anti-aging ability and closed cell properties of the foam board, and ensures the generation and performance of foamed sheets.
Smart Images

Figure BDA0005070982190000011 
Figure BDA0005070982190000021 
Figure BDA0005070982190000022
Abstract
Description
Technical Field
[0001] The invention belongs to the field of PET foam board preparation, and in particular relates to a PET composite foam board and a preparation method thereof. Background Art
[0002] The chemical formula of polyethylene terephthalate is (C10H8O4)n. Its English name is polyethylene glycolterephthalate, or PET for short. It is a high polymer. It is made by exchanging dimethyl terephthalate with ethylene glycol or esterifying terephthalic acid with ethylene glycol to synthesize dihydroxyethyl terephthalate, and then polycondensing it. It is a crystalline saturated polyester, a milky white or light yellow, highly crystalline polymer with a smooth and glossy surface. It is a common resin in life. It has excellent physical and mechanical properties in a wide temperature range, and its operating temperature can reach 120°C. It has excellent electrical insulation, and its electrical properties are still good even at high temperature and high frequency, but its corona resistance is poor, and its creep resistance, fatigue resistance, friction resistance, and dimensional stability are all very good. Polybutylene terephthalate, also known as polybutylene terephthalate (PBT for short), belongs to the polyester series. It is a polyester made by polycondensation of terephthalic acid and 1,4-butanediol. It is an important thermoplastic polyester and one of the five major engineering plastics. Polybutylene terephthalate is a milky white, translucent to opaque, semi-crystalline thermoplastic polyester with high heat resistance. It is not resistant to strong acids and alkalis, but is resistant to organic solvents, flammable, and decomposes at high temperatures. It is widely used in the fields of automobiles, mechanical equipment, precision instrument components, electronic appliances, textiles, etc. The existing PET / PBT composite materials still have the following defects in the production process: the melt flow index is high, the viscosity is low, and it is difficult to form a high pressure and melt strength during the extrusion process; PET is a crystalline material. When the crystallinity is low, the number of product bubbles is small and the pore size is large. Summary of the invention
[0003] In view of the above-mentioned deficiencies in the prior art, the problem solved by the present invention is to provide a PET composite foam board with a large number of uniformly distributed pores, small pore size, good mechanical properties and high melt strength, and a preparation method thereof.
[0004] To solve the above problems, the technical solution adopted by the present invention is as follows:
[0005] A PET composite foam board comprises the following components and weight parts:
[0006]
[0007]
[0008] Further, it includes the following components and parts by weight:
[0009]
[0010] Furthermore, the PET resin is polyester chips available on the market, and its intrinsic viscosity is 0.6-2.0 dl / g.
[0011] Furthermore, the PBT resin is a polyester chip sold on the market, and its intrinsic viscosity is 0.6-1.5 dl / g.
[0012] Furthermore, the antioxidant is one of tris(2,4-di-tert-butylphenyl)phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and bis(2.4-di-tert-butylphenyl)pentaerythritol diphosphite, or a mixture of several thereof.
[0013] Furthermore, the nucleating agent is one or a mixture of talc, calcium carbonate, sodium stearate, sodium benzoate, and polytetrafluoroethylene.
[0014] Furthermore, the chain extender is one or a mixture of acrylic polymer, anhydride, epoxy, oxazole, and imide.
[0015] A method for preparing a PET composite foam board, comprising the following steps:
[0016] S1, weigh each raw material according to the above ratio;
[0017] S2, drying PET and PBT resins at 140°C for 4-6 hours;
[0018] S3. Add all the raw materials into a high-speed mixer and mix them evenly. Then add them into the extruder hopper and flow into the extruder screw at a uniform speed. The temperature and speed of the twin screw are set to 275°C and 60rpm, the temperature and speed of the single screw are set to 240°C and 10rpm, and 0.4% CO2 is used as a foaming agent for extrusion foaming. Finally, cool and form into a modified PET foam sheet.
[0019] The beneficial effects of the present invention are as follows:
[0020] 1. The present invention blends PET and PBT resins. Compared with PET resin, PBT has excellent molecular chain flexibility. The matching of intrinsic viscosities can achieve compatibility to the greatest extent. The PBT resin is evenly distributed in PET, thereby improving the crystallization performance and pore uniformity of the sheet.
[0021] 2. The present invention improves the oxidation ability of a PET composite foam board by using an antioxidant, effectively inhibits the thermal degradation of PET during long-term screw extrusion to a certain extent, and increases the anti-aging ability of the foam board.
[0022] 3. The crystallization rate of the material is accelerated by the nucleating agent, and at the same time a higher degree of crystallinity is obtained, the number of pores is increased, the pore size is reduced, and the mechanical properties of the foam are improved to a certain extent.
[0023] 4. The present invention increases the melt strength of PET by using a chain extender so that the cells will not burst during the foaming process, thereby ensuring the formation of the foamed sheet and the closed-cell nature of the cells. DETAILED DESCRIPTION
[0024] The present invention is described in further detail below.
[0025] Examples 1-6 of the present invention are prepared as follows:
[0026] Weigh each raw material according to the ratio, dry the PET and PBT resins at 140°C for 4-6 hours. Then add all the raw materials into a high-speed mixer and mix for 10 minutes. The speed of the high-speed mixer is 180 rpm, and the gap between the stirring blade and the barrel wall is less than 0.5 cm. Mix the materials evenly in the mixer to obtain a mixed material. The effect of the even mixing is that the various particles are basically uniform visually, without obvious lumps and aggregations.
[0027] The mixed material is added into a twin-screw extruder from a main feeding port, the screw aspect ratio of the twin-screw extruder is 40:1, the twin-screw speed is 60 rpm, and the temperatures of each reaction section from the feed section to the die of the twin-screw extruder are 240°C, 275°C, 275°C, 275°C, 275°C, 275°C, 275°C, and 275°C, respectively. The mixed material is melt-extruded through the twin-screw extruder, and liquid carbon dioxide is injected into the carbon dioxide injection port of the seventh zone. Then, the mixed material enters a single-screw extruder, the screw aspect ratio of the single-screw extruder is 40:1, the single-screw speed is 10 rpm, the single-screw interval temperature is set to 240°C, and the die head temperature is 270°C. After the material exits the die head, it is foamed and cooled and shaped by traction of a pressing plate, and finally cooled and formed into a modified PET foam sheet.
[0028] The foamed product was welded to test its various properties. The product-related performance tests and test methods are detailed in Table 2.
[0029] Table 1 below: The formulations of Examples 1-6 are as follows.
[0030]
[0031] Table 2: The relevant performance tests of Examples 1-6 are as follows.
[0032]
[0033]
[0034] It can be seen from Examples 1-6 that the products obtained by the synergistic effect of PET\PBT and the components of nucleating agent, antioxidant and chain extender have excellent mechanical properties and are suitable for PET foaming production. Among them, as the amount of PBT added increases, the mechanical properties and modulus of the foamed board in directions 1 and 2 decrease slightly, while the mechanical properties and modulus in direction 3 increase.
[0035] Compared with the PET foamed board, the foamed board prepared in Examples 1-6 has improved mechanical properties and modulus in all directions.
[0036] The number and pore size of the foamed board affect the mechanical properties of the board. It can be seen that the foamed boards prepared in Examples 1-6 have smaller pore sizes and more uniform pore distribution compared with the PET foamed boards.
[0037] The data show that the PET composite foam board prepared by the present invention has a very good effect in the PET foaming modification process.
[0038] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A PET composite foam board, characterized in that: It includes the following components and weight parts:
2. The PET composite foam board according to claim 1, characterized in that: It includes the following components and weight parts:
3. The PET composite foam board according to claim 1, characterized in that: The PET resin is polyester chips sold on the market, and its intrinsic viscosity is 0.6-2.0 dl / g.
4. The PET composite foam board according to claim 1, characterized in that: The PBT resin is a polyester chip sold on the market, and its intrinsic viscosity is 0.6-1.5 dl / g.
5. The PET composite foam board according to claim 1, characterized in that: The antioxidant is one of tris(2,4-di-tert-butylphenyl)phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and bis(2.4-di-tert-butylphenyl)pentaerythritol diphosphite or a mixture of several of them.
6. The PET composite foam board according to claim 1, characterized in that: The nucleating agent is one or a mixture of talcum powder, calcium carbonate, sodium stearate, sodium benzoate and polytetrafluoroethylene.
7. The PET composite foam board according to claim 1, characterized in that: The chain extender is one or a mixture of acrylic polymer, anhydride, epoxy, oxazole and imide.
8. A method for preparing the PET composite foam board according to claim 1, characterized in that: Here are the steps: S1. Weigh each raw material according to the above ratio; S2, drying PET and PBT resins at 140°C for 4-6 hours; S3. Add all the raw materials into a high-speed mixer and mix them evenly. Then add them into the extruder hopper and flow into the extruder screw at a uniform speed. The temperature and speed of the twin screw are set to 275°C and 60rpm, the temperature and speed of the single screw are set to 240°C and 10rpm, and 0.4% CO2 is used as a foaming agent for extrusion foaming. Finally, cool and form into a modified PET foam sheet.