High-barrier biodegradable mulching film and preparation method thereof

By using polylactic acid prepolymer, chitosan solution and functional fillers and other materials, the pollution problem of traditional plastic plastic film is solved, low-cost and high-performance plastic film replacement is achieved, and soil pollution is reduced. Environmental impact.

CN119039752AInactive Publication Date: 2024-11-29TAIZHOU HUANGYAN ZEYU NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411558660.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing biodegradable plastic film has high cost and poor overall performance, poor barrier properties and mechanical properties, and cannot effectively replace traditional plastic plastic film, resulting in soil pollution and environmental problems.

Method used

High barrier biodegradable plastic film is prepared by using 80-100 parts of polylactic acid prepolymer, 30-40 parts of chitosan solution, 10-20 parts of functional filler, 1-1.5 parts of chain extender and 0.5-1 part of antioxidant. Improve material performance through specific dehydration, enzymatic and sonication techniques.

Benefits of technology

Biodegradable plastic film with low cost, high barrier properties and excellent mechanical properties can effectively degrade and not contaminate the soil, improve soil fertility and extend the life of the plastic film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of agricultural mulching films, and particularly discloses a high-barrier-property biodegradable mulching film and a preparation method thereof.The high-barrier-property biodegradable mulching film is prepared from polylactic acid prepolymer, a chitosan solution, functional filler, a chain extender, an antioxidant and an ultraviolet light absorber; the preparation method comprises the following steps: weighing the raw materials in parts by weight, putting the raw materials into a high-speed blender, and mixing and stirring; putting the mixed and stirred raw materials into a double-screw extruder, extruding, and carrying out air cooling granulation; extruding the granules to form a tubular film blank, blowing the tubular film blank to form a film, and cooling and shaping to obtain the high-barrier biodegradable mulching film. The high-barrier biodegradable mulching film prepared by the invention has good mechanical property, high barrier property, excellent antibacterial property, aging resistance, long service life and biodegradability, and decomposers can increase the content of organic matters in soil and improve the fertility of the soil in the subsequent decomposition process, so that the high-barrier biodegradable mulching film is beneficial to the growth of crops.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of agricultural mulch films, and more specifically, to a high-barrier biodegradable mulch film and a preparation method thereof. Background Art

[0002] Agricultural plastic products play an indispensable role in agricultural development, among which agricultural mulch films are the most widely used. They play a huge role in reducing soil moisture evaporation, improving soil moisture utilization efficiency and promoting crop growth and development, which greatly promotes the development of the agricultural economy. Traditional agricultural mulch films with polyethylene (PE) as the main raw material play an important role in heat preservation, water retention, insect prevention and weed control, and reducing the consumption of agricultural resources (fertilizers, pesticides, etc.) due to their excellent mechanical properties and stable chemical properties. Therefore, they are widely used in agricultural production.

[0003] Traditional plastic mulch has promoted agricultural development, but it has also caused environmental pollution problems that cannot be ignored. It is extremely difficult to recycle and dispose of traditional plastic mulch after use, resulting in a large amount of non-degradable mulch residue in the soil. At the same time, the discarded and buried residues of traditional plastic mulch release harmful chemicals into the soil, which not only seriously damages the activity of soil microorganisms and the balance of microbial communities, but also significantly weakens soil fertility. At the same time, harmful substances in microplastics can be transmitted in the food chain and accumulated in the human body, bringing unpredictable risks to agricultural production and food safety.

[0004] Biodegradable mulch replaces traditional plastic mulch, which can reduce pollutants in the soil, protect the ecological environment, and improve the sustainable utilization of soil. However, the biodegradable films in the prior art generally have the following problems: 1. Compared with traditional polyethylene mulch, the cost of using biodegradable mulch is high; 2. The comprehensive performance of biodegradable mulch is worse than that of traditional mulch, and its barrier and mechanical properties are poor.

[0005] Therefore, there is an urgent need for an environmentally friendly, biodegradable, low-cost, and green mulch film with good comprehensive performance to replace the existing traditional plastic mulch film. Based on the above statement, the present application provides a high-barrier biodegradable mulch film and a preparation method thereof. Summary of the invention

[0006] In order to solve the problems of serious microplastic pollution and release of harmful chemicals into the soil caused by the residues of existing traditional plastic mulch films, the present application provides a high-barrier biodegradable mulch film and a preparation method thereof.

[0007] In the first aspect, the present application provides a high barrier biodegradable mulch film, which adopts the following technical solution: A high-barrier biodegradable mulch film comprises the following raw materials in parts by weight: 80-100 parts of polylactic acid prepolymer, 30-40 parts of chitosan solution, 10-20 parts of functional filler, 1-1.5 parts of chain extender, 0.5-1 parts of antioxidant, and 0.3-0.8 parts of ultraviolet absorber.

[0008] Preferably, the polylactic acid prepolymer is prepared by the following method: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6-8 hours at a temperature of 110-130°C and a pressure of 120-130 kPa; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 120-130°C and the pressure to 22-24 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200-250 r / min for 2-3 hours; A3. Add plasticizer to the reactor, raise the temperature to 150-170°C, and stir the reaction at a rate of 100-150 r / min for 1-2 hours to obtain the desired polylactic acid prepolymer.

[0009] Preferably, the composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 3-6:1, and the plasticizer is acetyl tributyl citrate; the mass ratio of the lactic acid, the composite catalyst and the plasticizer is 100:1-1.5:10-15.

[0010] Preferably, the chitosan solution is prepared by the following method: B1. Cleaning and crushing: Place the shell of the crustacean in distilled water and perform ultrasonic cleaning at a frequency of 20-40kHz to remove impurities. After the ultrasonic cleaning, wash it with distilled water for 3-5 times, dry it in an oven at 70-80°C, crush it with a pulverizer, and pass it through a 120-180 mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5-10%, treat with acid at 30-50°C for 4-6 hours, filter, take the filter cake, wash it with distilled water for 3-5 times, and then dry it to obtain a decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH in the reaction system is adjusted to 7-8, after stirring and enzymolyzing at 40-60°C for 2-4h, complex enzyme 2 is added, the pH in the reaction system is adjusted to 4-6, after stirring and enzymolyzing at 40-50°C for 3-6h, the filter is taken, the filter cake is washed with distilled water for 3-5 times and then dried to obtain the enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60-80°C for 0.5-1h, ultrasonicate at 30-50kHz for 1-3h, filter, and collect the filtrate to obtain a chitosan solution.

[0011] Preferably, the composite enzyme 1 in step B3 is a mixture of trypsin, papain and serine protease in a mass ratio of 1:1-1.5:2-2.5; the composite enzyme 2 in step B3 is a mixture of chitinase and chitin deacetylase in a mass ratio of 1:2.5-3.5; the mixed solvent in step B4 is a mixture of quaternary ammonium salt, citric acid and deionized water in a mass ratio of 0.6-0.8:0.3-0.5:3-5.

[0012] Preferably, in step B1, the mass ratio of crustacean shell to distilled water is 1:5-8; in step B2, the mass ratio of dry powder to dilute hydrochloric acid with a mass concentration of 5% is 1:4-6; in step B3, the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 is 10:30-40:0.05-0.08:0.08-0.12; in step B4, the mass ratio of enzymatic hydrolysis product to mixed solvent is 10:25-35.

[0013] Preferably, the functional filler is prepared by the following steps: C1. Dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 20-30 kHz for 0.5-1 h to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 20-30 kHz for 0.5-1 h to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 2.5-4.5:3.5-8:0.5-0.8, stir and dissolve at 40-50°C for 0.5-1h, ultrasonicate at a frequency of 30-50kHz for 1-3h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0014] Preferably, in step C1, the mass ratio of nano-silica to organic solvent is 1:10-12; the mass ratio of nano-cellulose to organic solvent is 1:10-12; the particle size of the nano-silica is 20-40 nm; the organic solvent is ethanol or acetone; and the cross-linking agent in step C2 is one of silane coupling agents KH-550, KH-560 or KH-570.

[0015] Preferably, the chain extender is an epoxy chain extender ADR; the antioxidant is one or a combination of butylated hydroxyanisole, dibutyl hydroxytoluene or tert-butylhydroquinone; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5-2.8:1.

[0016] In a second aspect, the present application provides a method for preparing a high-barrier biodegradable mulch film, using the following technical solution: A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000-3000 r / min for 0.5-1h; S2, putting the mixed raw materials into a twin-screw extruder, extruding at 150-200°C, and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160-180°C to a film thickness of 4-8 μm, and the high barrier biodegradable mulch film is obtained after cooling and shaping.

[0017] In summary, this application has the following beneficial effects: The present application first dehydrates lactic acid, further reacts under the action of a composite catalyst, and adds a plasticizer, tributyl acetyl citrate, to prepare a polylactic acid prepolymer. The composite catalyst adopts a mixture of diethyl phosphite and manganese acetate, which has a dual catalytic effect. A part of the structure activates the lactide monomer as an electrophilic reagent, and the other part activates the chain end of the polymerization reaction through hydrogen bonding, thereby activating the monomer and the chain end at the same time and promoting the polymerization reaction. The plasticizer tributyl acetyl citrate has good compatibility with polylactic acid. The addition of tributyl acetyl citrate can reduce the interaction force between polymer molecular chains, making the polymer chain segments easier to move, thereby increasing the flexibility and plasticity of the ground film. At the same time, the addition of tributyl acetyl citrate helps to improve the melt fluidity and thermal stability of the material, making the production process of the ground film smoother and improving production efficiency.

[0018] This application uses crustacean shells as raw materials for extracting chitosan solution, and obtains the required chitosan solution through acid treatment for decalcification, secondary enzymatic treatment and final solvent extraction. The ocean produces a huge amount of crustaceans, and using crustacean shells (shrimp, crab shells) as raw materials reduces dependence on limited petroleum resources, realizes the recycling of resources, and reduces production costs. Composite enzyme 1 is a mixture of trypsin, papain and serine protease. Through the combined use of the three enzymes, it can efficiently hydrolyze the protein in the crustacean shell, thereby improving the decomposition efficiency. At the same time, the mild reaction conditions help to protect the structure and properties of chitosan, and provide favorable conditions for the subsequent extraction and utilization of chitosan.

[0019] Compound enzyme 2 is a mixture of chitinase and chitin deacetylase. Chitin deacetylase can hydrolyze and remove the acetyl group on chitin, while chitinase can hydrolyze the glycosidic bond of chitin and decompose chitin into smaller fragments. The synergistic effect of these two enzymes can accelerate the conversion process of chitin to chitosan, thereby improving the preparation efficiency. Compared with the traditional concentrated alkali method, it not only reduces the residual harmful chemicals, is environmentally friendly, has mild reaction conditions and simple steps, but also has a higher degree of deacetylation and viscosity. The chitosan solution with high viscosity and high degree of deacetylation has more regular molecular chains and stronger intermolecular interactions. The resulting mulch film has high tensile strength and durability. At the same time, it can more effectively combine with microbial cell membranes, exert stronger antibacterial properties, have a broad antibacterial spectrum, and have a long-lasting antibacterial effect, which can more comprehensively protect soil and crops from microbial invasion.

[0020] The chitosan solution involved in the preparation of high-barrier biodegradable mulch can increase the organic matter content of the soil, improve soil fertility, and be beneficial to the growth of crops during the subsequent decomposition process.

[0021] In the present application, nano-silicon dioxide and nano-cellulose are dispersed in an organic solvent respectively, and then a cross-linking agent is added to stir and mix the reaction to obtain a functional filler. Nano-silicon dioxide has a large specific surface area and surface activity due to its tiny particle size. The density of the ground film obtained by adding nano-silicon dioxide is enhanced, which can reduce the permeability of water vapor and oxygen; the fibrous structure of nano-cellulose can form an effective physical barrier to effectively block the penetration of external moisture, gas and other substances; the granular structure of nano-silicon dioxide and the fibrous structure of nano-cellulose are intertwined to form a more dense and uniform physical barrier, further improving the barrier performance of the prepared ground film. At the same time, the synergistic effect of nano-silicon dioxide and nano-cellulose can also improve the mechanical properties and stability of the ground film, making it more durable and adaptable to various climatic conditions. 4. In the preparation process of the ground film, the present application adds auxiliary agents such as chain extenders, antioxidants, and ultraviolet absorbers. The addition of epoxy chain extender ADR can react with the functional groups on the linear polymer chain to expand the molecular chain and increase the molecular weight, thereby significantly improving the tensile strength, elongation at break and other mechanical properties of the ground film. The addition of antioxidants can prevent the subsequent mulch film from undergoing oxidation reactions during actual use, thereby delaying the aging process of the mulch film and extending the life of the mulch film. The addition of ultraviolet absorbers can absorb ultraviolet rays in sunlight during the subsequent use of the mulch film and convert them into harmless energy and release them, thereby protecting the mulch film material from damage by ultraviolet rays, thereby delaying the aging process of the mulch film and extending the life of the mulch film.

[0022] 5. The high-barrier biodegradable mulch film prepared in this application has good mechanical properties, high barrier properties, excellent antibacterial properties, anti-aging, long life, and is biodegradable. The degraded products are not only pollution-free to the soil, but also increase the soil organic matter content and improve soil fertility. DETAILED DESCRIPTION

[0023] The present application is further described in detail below with reference to the embodiments.

[0024] The raw materials used in the examples and comparative examples of the present application are as follows: Diethyl phosphite was purchased from Aladdin with the product number D109100; Manganese acetate was purchased from Aladdin with the catalog number M433192; Acetyl tributyl citrate was purchased from Aladdin with the product number T111251; Nanosilica was purchased from Aladdin, catalog number S104596; Nanocellulose was purchased from Zhejiang Jinjiahao Green Nanomaterials Co., Ltd.

[0025] Embodiments 1-3 provide a high-barrier biodegradable mulch film and a preparation method thereof.

[0026] Example 1 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 80 parts of polylactic acid prepolymer, 30 parts of chitosan solution, 10 parts of functional filler, 1 part of chain extender, 0.5 parts of antioxidant, and 0.3 parts of ultraviolet absorber.

[0027] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6 hours at a temperature of 110°C and a pressure of 120 kPa; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 120°C and the pressure to 22 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200 r / min for 2 h; A3. Add plasticizer to the reactor, raise the temperature to 150°C, and stir the reaction at a rate of 100 r / min for 1 hour to obtain the desired polylactic acid prepolymer.

[0028] The composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 3:1, and the plasticizer is acetyl tributyl citrate; the mass ratio of lactic acid, the composite catalyst and the plasticizer is 100:1:10.

[0029] Preparation of chitosan solution: B1. Cleaning and crushing: The shrimp shells were placed in distilled water and ultrasonically cleaned at a frequency of 20kHz to remove impurities. After the ultrasonic cleaning, the shrimp shells were washed with distilled water for 3 times, dried in an oven at 70°C, crushed with a pulverizer, and passed through a 120-mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5%, treat with acid at 30°C for 4 hours, filter, take the filter cake, wash it with distilled water for 3 times and dry it to obtain the decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH in the reaction system is adjusted to 7, after stirring and enzymolyzing at 40°C for 2 hours, complex enzyme 2 is added, the pH in the reaction system is adjusted to 4, after stirring and enzymolyzing at 40°C for 3 hours, the mixture is filtered, the filter cake is washed with distilled water 3 times and then dried to obtain an enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60°C for 0.5 h, ultrasonicate at a frequency of 30 kHz for 1 h, filter, and collect the filtrate to obtain a chitosan solution.

[0030] The composite enzyme 1 in step B3 is a mixture of trypsin (enzyme activity: 2500U / mg), papain (enzyme activity: 2000U / mg) and serine protease (enzyme activity: 1800U / mg) in a mass ratio of 1:1:2; the composite enzyme 2 in step B3 is a mixture of chitinase (enzyme activity: 2500U / mg) and chitin deacetylase (enzyme activity: 3000U / mg) in a mass ratio of 1:2.5; and the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid and deionized water in a mass ratio of 0.6:0.3:3.

[0031] The mass ratio of crustacean shell to distilled water in step B1 is 1:5; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:4; the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 in step B3 is 10:30:0.05:0.08; the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:25.

[0032] Preparation of functional fillers: C1, dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 2.5:3.5:0.5, stir and dissolve at 40°C for 0.5h, ultrasonicate at a frequency of 30kHz for 1h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0033] Wherein the mass ratio of nano-silicon dioxide to organic solvent in step C1 is 1:10; the mass ratio of nano-cellulose to organic solvent is 1:10; the particle size of nano-silicon dioxide is 30nm; the organic solvent is ethanol; the cross-linking agent in step C2 is silane coupling agent KH-550; The chain extender is epoxy chain extender ADR-4468; the antioxidant is butylated hydroxyanisole; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5:1.

[0034] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000 r / min for 0.5 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 150° C., and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160°C to a film thickness of 4 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0035] Example 2 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 90 parts of polylactic acid prepolymer, 35 parts of chitosan solution, 15 parts of functional filler, 1.25 parts of chain extender, 0.75 parts of antioxidant, and 0.55 parts of ultraviolet absorber.

[0036] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 7 hours at a temperature of 120°C and a pressure of 125 kPa; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 125°C and the pressure to 23 kPa, protect with nitrogen throughout the reaction, and stir the reaction at a rate of 225 r / min for 2.5 h; A3. Add plasticizer to the reactor, raise the temperature to 160°C, and stir the reaction at a rate of 125 r / min for 1.5 hours to obtain the desired polylactic acid prepolymer.

[0037] The composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 4.5:1, and the plasticizer is acetyl tributyl citrate; the mass ratio of lactic acid, the composite catalyst and the plasticizer is 100:1.25:12.5.

[0038] Preparation of chitosan solution: B1. Cleaning and crushing: The crab shells were placed in distilled water and ultrasonically cleaned at a frequency of 30kHz to remove impurities. After the ultrasonic cleaning, they were washed with distilled water for 4 times, dried in an oven at 75°C, crushed with a grinder, and passed through a 150-mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 7.5%, treat with acid at 40°C for 5 hours, filter, take the filter cake, wash it with distilled water 4 times and dry it to obtain the decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH in the reaction system is adjusted to 7.5, after stirring and enzymolysis at 50°C for 3 hours, complex enzyme 2 is added, the pH in the reaction system is adjusted to 5, and after stirring and enzymolysis at 45°C for 4.5 hours, the mixture is filtered, and the filter cake is washed with distilled water 4 times and dried to obtain an enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 70°C for 0.75h, ultrasonicate at a frequency of 40kHz for 2h, filter, and collect the filtrate to obtain a chitosan solution.

[0039] The composite enzyme 1 in step B3 is a mixture of trypsin (enzyme activity: 2500U / mg), papain (enzyme activity: 2000U / mg) and serine protease (enzyme activity: 1800U / mg) in a mass ratio of 1:1.25:2.25; the composite enzyme 2 in step B3 is a mixture of chitinase (enzyme activity: 2500U / mg) and chitin deacetylase (enzyme activity: 3000U / mg) in a mass ratio of 1:3; the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid and deionized water in a mass ratio of 0.7:0.4:4.

[0040] The mass ratio of crustacean shell to distilled water in step B1 is 1:6.5; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:5; the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 in step B3 is 10:35:0.065:0.1; the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:30.

[0041] Preparation of functional fillers: C1. Dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 25 kHz for 0.75 h to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 25 kHz for 0.75 h to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 3.5:6:0.65, stir and dissolve at 45°C for 0.75h, ultrasonicate at a frequency of 40kHz for 2h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0042] The mass ratio of nano-silicon dioxide to organic solvent in step C1 is 1:11; the mass ratio of nano-cellulose to organic solvent is 1:11; the particle size of nano-silicon dioxide is 30nm; the organic solvent is ethanol; and the cross-linking agent in step C2 is silane coupling agent KH-560.

[0043] The chain extender is epoxy chain extender ADR-4468; the antioxidant is butylated hydroxytoluene; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 2.2:1.

[0044] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2500 r / min for 0.75 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 175°C, and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 170°C to a film thickness of 6 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0045] Example 3 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 100 parts of polylactic acid prepolymer, 40 parts of chitosan solution, 20 parts of functional filler, 1.5 parts of chain extender, 1 part of antioxidant, and 0.8 parts of ultraviolet absorber.

[0046] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out dehydration reaction at a temperature of 130°C and a pressure of 130 kPa for 8 hours; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 130°C and the pressure to 24 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 250 r / min for 3 h; A3. Add plasticizer to the reactor, raise the temperature to 170°C, and stir the reaction at a rate of 150 r / min for 2 hours to obtain the desired polylactic acid prepolymer.

[0047] The composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 6:1, and the plasticizer is acetyl tributyl citrate; the mass ratio of lactic acid, the composite catalyst and the plasticizer is 100:1.5:15.

[0048] Preparation of chitosan solution: B1. Cleaning and crushing: The shrimp shells were placed in distilled water and ultrasonically cleaned at a frequency of 40kHz to remove impurities. After the ultrasonic cleaning, the shrimp shells were washed with distilled water for 5 times, dried in an oven at 80°C, crushed with a pulverizer, and passed through a 180-mesh sieve to obtain dry powder; B2. Decalcification treatment: the dry powder in step B1 is placed in dilute hydrochloric acid with a mass concentration of 10%, and the mixture is treated with acid at 50° C. for 6 h. The mixture is filtered, and the filter cake is washed with distilled water for 5 times and then dried to obtain a decalcified product. B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH in the reaction system is adjusted to 8, after stirring and enzymolysis at 60°C for 4 hours, complex enzyme 2 is added, the pH in the reaction system is adjusted to 6, and after stirring and enzymolysis at 50°C for 6 hours, the mixture is filtered, the filter cake is washed with distilled water 5 times and then dried to obtain an enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 80°C for 1 hour, ultrasonicate at a frequency of 50 kHz for 3 hours, filter, and collect the filtrate to obtain a chitosan solution.

[0049] The composite enzyme 1 in step B3 is a mixture of trypsin (enzyme activity: 2500U / mg), papain (enzyme activity: 2000U / mg) and serine protease (enzyme activity: 1800U / mg) in a mass ratio of 1:1.5:2.5; the composite enzyme 2 in step B3 is a mixture of chitinase (enzyme activity: 2500U / mg) and chitin deacetylase (enzyme activity: 3000U / mg) in a mass ratio of 1:3.5; the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid and deionized water in a mass ratio of 0.8:0.5:5.

[0050] The mass ratio of crustacean shell to distilled water in step B1 is 1:8; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:6; the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 in step B3 is 10:40:0.08:0.12; the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:35.

[0051] Preparation of functional fillers: C1, dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 30 kHz for 1 hour to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 30 kHz for 1 hour to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 4.5:8:0.8, stir and dissolve at 50°C for 1 hour, ultrasonicate at a frequency of 50 kHz for 3 hours, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0052] The mass ratio of nano-silicon dioxide to organic solvent in step C1 is 1:12; the mass ratio of nano-cellulose to organic solvent is 1:12; the particle size of nano-silicon dioxide is 30nm; the organic solvent is acetone; and the cross-linking agent in step C2 is silane coupling agent KH-570.

[0053] The chain extender is epoxy chain extender ADR-4468; the antioxidant is tert-butyl hydroquinone; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 2.8:1.

[0054] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 3000 r / min for 1 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 200°C, and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 180°C to a film thickness of 8 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0055] In order to verify the comprehensive performance of the high barrier biodegradable mulch film prepared in Examples 1-3 of the present application, the present application sets up Comparative Examples 1-8, which are as follows: Comparative Example 1 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 80 parts of polylactic acid prepolymer, 30 parts of chitosan solution, 10 parts of functional filler, 1 part of chain extender, 0.5 parts of antioxidant, 0.3 parts of ultraviolet absorber, and 6 parts of plasticizer.

[0056] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6 hours at a temperature of 110°C and a pressure of 120 kPa; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 120°C and the pressure to 22 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200 r / min for 2 h to obtain the desired polylactic acid prepolymer.

[0057] The composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 3:1; the mass ratio of lactic acid to the composite catalyst is 100:1.

[0058] Preparation of chitosan solution: B1. Cleaning and crushing: The shrimp shells were placed in distilled water and ultrasonically cleaned at a frequency of 20kHz to remove impurities. After the ultrasonic cleaning, the shrimp shells were washed with distilled water for 3 times, dried in an oven at 70°C, crushed with a pulverizer, and passed through a 120-mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5%, treat with acid at 30°C for 4 hours, filter, take the filter cake, wash it with distilled water for 3 times and dry it to obtain the decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH in the reaction system is adjusted to 7, after stirring and enzymolyzing at 40°C for 2 hours, complex enzyme 2 is added, the pH in the reaction system is adjusted to 4, after stirring and enzymolyzing at 40°C for 3 hours, the mixture is filtered, the filter cake is washed with distilled water 3 times and then dried to obtain an enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60°C for 0.5 h, ultrasonicate at a frequency of 30 kHz for 1 h, filter, and collect the filtrate to obtain a chitosan solution.

[0059] The composite enzyme 1 in step B3 is a mixture of trypsin (enzyme activity: 2500U / mg), papain (enzyme activity: 2000U / mg) and serine protease (enzyme activity: 1800U / mg) in a mass ratio of 1:1:2; the composite enzyme 2 in step B3 is a mixture of chitinase (enzyme activity: 2500U / mg) and chitin deacetylase (enzyme activity: 3000U / mg) in a mass ratio of 1:2.5; and the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid and deionized water in a mass ratio of 0.6:0.3:3.

[0060] The mass ratio of crustacean shell to distilled water in step B1 is 1:5; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:4; the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 in step B3 is 10:30:0.05:0.08; the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:25.

[0061] Preparation of functional fillers: C1, dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 2.5:3.5:0.5, stir and dissolve at 40°C for 0.5h, ultrasonicate at a frequency of 30kHz for 1h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0062] The mass ratio of nano-silicon dioxide to organic solvent in step C1 is 1:10; the mass ratio of nano-cellulose to organic solvent is 1:10; the particle size of nano-silicon dioxide is 30nm; the organic solvent is ethanol; and the cross-linking agent in step C2 is silane coupling agent KH-550.

[0063] The plasticizer is acetyl tributyl citrate; the chain extender is epoxy chain extender ADR-4468; the antioxidant is butylated hydroxyanisole; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5:1.

[0064] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, plasticizer, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000 r / min for 0.5 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 150° C., and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160°C to a film thickness of 4 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0065] Comparative Example 2 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 80 parts of polylactic acid prepolymer, 30 parts of chitosan solution, 10 parts of functional filler, 1 part of chain extender, 0.5 parts of antioxidant, and 0.3 parts of ultraviolet absorber.

[0066] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6 hours at a temperature of 110°C and a pressure of 120 kPa; A2. Add the catalyst into the reactor, adjust the reaction temperature to 120°C and the pressure to 22 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200 r / min for 2 h; A3. Add plasticizer to the reactor, raise the temperature to 150°C, and stir the reaction at a rate of 100 r / min for 1 hour to obtain the desired polylactic acid prepolymer.

[0067] The catalyst is diethyl phosphite, the plasticizer is acetyl tributyl citrate, and the mass ratio of lactic acid, the catalyst and the plasticizer is 100:1:10.

[0068] Preparation of chitosan solution: B1. Cleaning and crushing: The shrimp shells were placed in distilled water and ultrasonically cleaned at a frequency of 20kHz to remove impurities. After the ultrasonic cleaning, the shrimp shells were washed with distilled water for 3 times, dried in an oven at 70°C, crushed with a pulverizer, and passed through a 120-mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5%, treat with acid at 30°C for 4 hours, filter, take the filter cake, wash it with distilled water for 3 times and dry it to obtain the decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH in the reaction system is adjusted to 7, after stirring and enzymolyzing at 40°C for 2 hours, complex enzyme 2 is added, the pH in the reaction system is adjusted to 4, after stirring and enzymolyzing at 40°C for 3 hours, the mixture is filtered, the filter cake is washed with distilled water 3 times and then dried to obtain an enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60°C for 0.5 h, ultrasonicate at a frequency of 30 kHz for 1 h, filter, and collect the filtrate to obtain a chitosan solution.

[0069] The composite enzyme 1 in step B3 is a mixture of trypsin (enzyme activity: 2500U / mg), papain (enzyme activity: 2000U / mg) and serine protease (enzyme activity: 1800U / mg) in a mass ratio of 1:1:2; the composite enzyme 2 in step B3 is a mixture of chitinase (enzyme activity: 2500U / mg) and chitin deacetylase (enzyme activity: 3000U / mg) in a mass ratio of 1:2.5; and the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid and deionized water in a mass ratio of 0.6:0.3:3.

[0070] The mass ratio of crustacean shell to distilled water in step B1 is 1:5; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:4; the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 in step B3 is 10:30:0.05:0.08; the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:25.

[0071] Preparation of functional fillers: C1, dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 2.5:3.5:0.5, stir and dissolve at 40°C for 0.5h, ultrasonicate at a frequency of 30kHz for 1h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0072] The mass ratio of nano-silicon dioxide to organic solvent in step C1 is 1:10; the mass ratio of nano-cellulose to organic solvent is 1:10; the particle size of nano-silicon dioxide is 30nm; the organic solvent is ethanol; and the cross-linking agent in step C2 is silane coupling agent KH-550.

[0073] The chain extender is epoxy chain extender ADR-4468; the antioxidant is butylated hydroxyanisole; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5:1.

[0074] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000 r / min for 0.5 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 150° C., and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160°C to a film thickness of 4 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0075] Comparative Example 3 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 80 parts of polylactic acid prepolymer, 30 parts of chitosan solution, 10 parts of functional filler, 1 part of chain extender, 0.5 parts of antioxidant, and 0.3 parts of ultraviolet absorber.

[0076] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6 hours at a temperature of 110°C and a pressure of 120 kPa; A2. Add the catalyst into the reactor, adjust the reaction temperature to 120°C and the pressure to 22 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200 r / min for 2 h; A3. Add plasticizer to the reactor, raise the temperature to 150°C, and stir the reaction at a rate of 100 r / min for 1 hour to obtain the desired polylactic acid prepolymer.

[0077] The catalyst is manganese acetate, the plasticizer is acetyl tributyl citrate, and the mass ratio of lactic acid, the catalyst and the plasticizer is 100:1:10.

[0078] Preparation of chitosan solution: B1. Cleaning and crushing: The shrimp shells were placed in distilled water and ultrasonically cleaned at a frequency of 20kHz to remove impurities. After the ultrasonic cleaning, the shrimp shells were washed with distilled water for 3 times, dried in an oven at 70°C, crushed with a pulverizer, and passed through a 120-mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5%, treat with acid at 30°C for 4 hours, filter, take the filter cake, wash it with distilled water for 3 times and dry it to obtain the decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH in the reaction system is adjusted to 7, after stirring and enzymolyzing at 40°C for 2 hours, complex enzyme 2 is added, the pH in the reaction system is adjusted to 4, after stirring and enzymolyzing at 40°C for 3 hours, the mixture is filtered, the filter cake is washed with distilled water 3 times and then dried to obtain an enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60°C for 0.5 h, ultrasonicate at a frequency of 30 kHz for 1 h, filter, and collect the filtrate to obtain a chitosan solution.

[0079] The composite enzyme 1 in step B3 is a mixture of trypsin (enzyme activity: 2500U / mg), papain (enzyme activity: 2000U / mg) and serine protease (enzyme activity: 1800U / mg) in a mass ratio of 1:1:2; the composite enzyme 2 in step B3 is a mixture of chitinase (enzyme activity: 2500U / mg) and chitin deacetylase (enzyme activity: 3000U / mg) in a mass ratio of 1:2.5; and the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid and deionized water in a mass ratio of 0.6:0.3:3.

[0080] The mass ratio of crustacean shell to distilled water in step B1 is 1:5; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:4; the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 in step B3 is 10:30:0.05:0.08; the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:25.

[0081] Preparation of functional fillers: C1, dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 2.5:3.5:0.5, stir and dissolve at 40°C for 0.5h, ultrasonicate at a frequency of 30kHz for 1h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0082] The mass ratio of nano-silicon dioxide to organic solvent in step C1 is 1:10; the mass ratio of nano-cellulose to organic solvent is 1:10; the particle size of nano-silicon dioxide is 30nm; the organic solvent is ethanol; and the cross-linking agent in step C2 is silane coupling agent KH-550.

[0083] The chain extender is epoxy chain extender ADR-4468; the antioxidant is butylated hydroxyanisole; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5:1.

[0084] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000 r / min for 0.5 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 150° C., and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160°C to a film thickness of 4 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0085] Comparative Example 4 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 80 parts of polylactic acid prepolymer, 30 parts of chitosan solution, 10 parts of functional filler, 1 part of chain extender, 0.5 parts of antioxidant, and 0.3 parts of ultraviolet absorber.

[0086] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6 hours at a temperature of 110°C and a pressure of 120 kPa; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 120°C and the pressure to 22 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200 r / min for 2 h; A3. Add plasticizer to the reactor, raise the temperature to 150°C, and stir the reaction at a rate of 100 r / min for 1 hour to obtain the desired polylactic acid prepolymer.

[0087] The composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 3:1, and the plasticizer is acetyl tributyl citrate; the mass ratio of lactic acid, the composite catalyst and the plasticizer is 100:1:10.

[0088] Preparation of chitosan solution: B1. Cleaning and crushing: The shrimp shells were placed in distilled water and ultrasonically cleaned at a frequency of 20kHz to remove impurities. After the ultrasonic cleaning, the shrimp shells were washed with distilled water for 3 times, dried in an oven at 70°C, crushed with a pulverizer, and passed through a 120-mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5%, treat with acid at 30°C for 4 hours, filter, take the filter cake, wash it with distilled water for 3 times and dry it to obtain the decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and compound enzyme 2, adjust the pH of the reaction system to 4, stir and enzymolyze at 40°C for 3h, then filter, take the filter cake, wash it with distilled water 3 times and dry it to obtain the enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60°C for 0.5 h, ultrasonicate at a frequency of 30 kHz for 1 h, filter, and collect the filtrate to obtain a chitosan solution.

[0089] The composite enzyme 2 in step B3 is a mixture of chitinase (enzyme activity: 2500U / mg) and chitin deacetylase (enzyme activity: 3000U / mg) in a mass ratio of 1:2.5; the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid, and deionized water in a mass ratio of 0.6:0.3:3.

[0090] The mass ratio of crustacean shell to distilled water in step B1 is 1:5; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:4; the mass ratio of decalcified product, distilled water and complex enzyme 2 in step B3 is 10:30:0.13; and the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:25.

[0091] Preparation of functional fillers: C1, dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 2.5:3.5:0.5, stir and dissolve at 40°C for 0.5h, ultrasonicate at a frequency of 30kHz for 1h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0092] The mass ratio of nano-silicon dioxide to organic solvent in step C1 is 1:10; the mass ratio of nano-cellulose to organic solvent is 1:10; the particle size of nano-silicon dioxide is 30nm; the organic solvent is ethanol; and the cross-linking agent in step C2 is silane coupling agent KH-550.

[0093] The chain extender is epoxy chain extender ADR-4468; the antioxidant is butylated hydroxyanisole; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5:1.

[0094] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000 r / min for 0.5 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 150° C., and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160°C to a film thickness of 4 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0095] Comparative Example 5 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 80 parts of polylactic acid prepolymer, 30 parts of chitosan solution, 10 parts of functional filler, 1 part of chain extender, 0.5 parts of antioxidant, and 0.3 parts of ultraviolet absorber.

[0096] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6 hours at a temperature of 110°C and a pressure of 120 kPa; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 120°C and the pressure to 22 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200 r / min for 2 h; A3. Add plasticizer to the reactor, raise the temperature to 150°C, and stir the reaction at a rate of 100 r / min for 1 hour to obtain the desired polylactic acid prepolymer.

[0097] The composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 3:1, and the plasticizer is acetyl tributyl citrate; the mass ratio of lactic acid, the composite catalyst and the plasticizer is 100:1:10.

[0098] Preparation of chitosan solution: B1. Cleaning and crushing: The shrimp shells were placed in distilled water and ultrasonically cleaned at a frequency of 20kHz to remove impurities. After the ultrasonic cleaning, the shrimp shells were washed with distilled water for 3 times, dried in an oven at 70°C, crushed with a pulverizer, and passed through a 120-mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5%, treat with acid at 30°C for 4 hours, filter, take the filter cake, wash it with distilled water for 3 times and dry it to obtain the decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH of the reaction system is adjusted to 7, and the enzymolysis is stirred at 40° C. for 2 h and then filtered. The filter cake is washed with distilled water 3 times and then dried to obtain an enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60°C for 0.5 h, ultrasonicate at a frequency of 30 kHz for 1 h, filter, and collect the filtrate to obtain a chitosan solution.

[0099] The composite enzyme 1 in step B3 is a mixture of trypsin (enzyme activity: 2500U / mg), papain (enzyme activity: 2000U / mg) and serine protease (enzyme activity: 1800U / mg) in a mass ratio of 1:1:2; the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid and deionized water in a mass ratio of 0.6:0.3:3.

[0100] The mass ratio of crustacean shell to distilled water in step B1 is 1:5; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:4; the mass ratio of decalcified product, distilled water and complex enzyme 1 in step B3 is 10:30:0.13; and the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:25.

[0101] Preparation of functional fillers: C1, dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 2.5:3.5:0.5, stir and dissolve at 40°C for 0.5h, ultrasonicate at a frequency of 30kHz for 1h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0102] The mass ratio of nano-silicon dioxide to organic solvent in step C1 is 1:10; the mass ratio of nano-cellulose to organic solvent is 1:10; the particle size of nano-silicon dioxide is 30nm; the organic solvent is ethanol; and the cross-linking agent in step C2 is silane coupling agent KH-550.

[0103] The chain extender is epoxy chain extender ADR-4468; the antioxidant is butylated hydroxyanisole; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5:1.

[0104] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000 r / min for 0.5 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 150° C., and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160°C to a film thickness of 4 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0105] Comparative Example 6 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 80 parts of polylactic acid prepolymer, 30 parts of chitosan solution, 10 parts of functional filler, 1 part of chain extender, 0.5 parts of antioxidant, and 0.3 parts of ultraviolet absorber.

[0106] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6 hours at a temperature of 110°C and a pressure of 120 kPa; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 120°C and the pressure to 22 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200 r / min for 2 h; A3. Add plasticizer to the reactor, raise the temperature to 150°C, and stir the reaction at a rate of 100 r / min for 1 hour to obtain the desired polylactic acid prepolymer.

[0107] The composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 3:1, and the plasticizer is acetyl tributyl citrate; the mass ratio of lactic acid, the composite catalyst and the plasticizer is 100:1:10.

[0108] Preparation of chitosan solution: B1. Cleaning and crushing: The shrimp shells were placed in distilled water and ultrasonically cleaned at a frequency of 20kHz to remove impurities. After the ultrasonic cleaning, the shrimp shells were washed with distilled water for 3 times, dried in an oven at 70°C, crushed with a pulverizer, and passed through a 120-mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5%, treat with acid at 30°C for 4 hours, filter, take the filter cake, wash it with distilled water for 3 times and dry it to obtain the decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and compound enzyme 2 are placed in a reaction vessel, the pH in the reaction system is adjusted to 4, and the enzymolysis is stirred at 40°C for 3 hours, and the compound enzyme 1 is added to adjust the pH in the reaction system to 7, and the enzymolysis is stirred at 40°C for 2 hours, and then filtered, the filter cake is washed with distilled water 3 times and dried to obtain the enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60°C for 0.5 h, ultrasonicate at a frequency of 30 kHz for 1 h, filter, and collect the filtrate to obtain a chitosan solution.

[0109] The composite enzyme 1 in step B3 is a mixture of trypsin (enzyme activity: 2500U / mg), papain (enzyme activity: 2000U / mg) and serine protease (enzyme activity: 1800U / mg) in a mass ratio of 1:1:2; the composite enzyme 2 in step B3 is a mixture of chitinase (enzyme activity: 2500U / mg) and chitin deacetylase (enzyme activity: 3000U / mg) in a mass ratio of 1:2.5; and the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid and deionized water in a mass ratio of 0.6:0.3:3.

[0110] The mass ratio of crustacean shell to distilled water in step B1 is 1:5; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:4; the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 in step B3 is 10:30:0.05:0.08; the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:25.

[0111] Preparation of functional fillers: C1, dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 2.5:3.5:0.5, stir and dissolve at 40°C for 0.5h, ultrasonicate at a frequency of 30kHz for 1h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0112] Wherein the mass ratio of nano-silicon dioxide to organic solvent in step C1 is 1:10; the mass ratio of nano-cellulose to organic solvent is 1:10; the particle size of nano-silicon dioxide is 30nm; the organic solvent is ethanol; the cross-linking agent in step C2 is silane coupling agent KH-550; The chain extender is epoxy chain extender ADR-4468; the antioxidant is butylated hydroxyanisole; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5:1.

[0113] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000 r / min for 0.5 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 150° C., and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160°C to a film thickness of 4 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0114] Comparative Example 7 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 80 parts of polylactic acid prepolymer, 30 parts of chitosan solution, 10 parts of functional filler, 1 part of chain extender, 0.5 parts of antioxidant, and 0.3 parts of ultraviolet absorber.

[0115] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6 hours at a temperature of 110°C and a pressure of 120 kPa; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 120°C and the pressure to 22 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200 r / min for 2 h; A3. Add plasticizer to the reactor, raise the temperature to 150°C, and stir the reaction at a rate of 100 r / min for 1 hour to obtain the desired polylactic acid prepolymer.

[0116] The composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 3:1, and the plasticizer is acetyl tributyl citrate; the mass ratio of lactic acid, the composite catalyst and the plasticizer is 100:1:10.

[0117] Preparation of chitosan solution: B1. Cleaning and crushing: The shrimp shells were placed in distilled water and ultrasonically cleaned at a frequency of 20kHz to remove impurities. After the ultrasonic cleaning, the shrimp shells were washed with distilled water for 3 times, dried in an oven at 70°C, crushed with a pulverizer, and passed through a 120-mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5%, treat with acid at 30°C for 4 hours, filter, take the filter cake, wash it with distilled water for 3 times and dry it to obtain the decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH in the reaction system is adjusted to 7, after stirring and enzymolyzing at 40°C for 2 hours, complex enzyme 2 is added, the pH in the reaction system is adjusted to 4, after stirring and enzymolyzing at 40°C for 3 hours, the mixture is filtered, the filter cake is washed with distilled water 3 times and then dried to obtain an enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60°C for 0.5 h, ultrasonicate at a frequency of 30 kHz for 1 h, filter, and collect the filtrate to obtain a chitosan solution.

[0118] The composite enzyme 1 in step B3 is a mixture of trypsin (enzyme activity: 2500U / mg), papain (enzyme activity: 2000U / mg) and serine protease (enzyme activity: 1800U / mg) in a mass ratio of 1:1:2; the composite enzyme 2 in step B3 is a mixture of chitinase (enzyme activity: 2500U / mg) and chitin deacetylase (enzyme activity: 3000U / mg) in a mass ratio of 1:2.5; and the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid and deionized water in a mass ratio of 0.6:0.3:3.

[0119] The mass ratio of crustacean shell to distilled water in step B1 is 1:5; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:4; the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 in step B3 is 10:30:0.05:0.08; the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:25.

[0120] Preparation of functional fillers: C1, dispersing the nanocellulose in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nanocellulose dispersion; C2. Mix the nanocellulose dispersion with the cross-linking agent in a mass ratio of 6:0.5, stir and dissolve at 40°C for 0.5h, ultrasonicate at a frequency of 30kHz for 1h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0121] The mass ratio of nanocellulose to organic solvent in step C1 is 1:10; the organic solvent is ethanol; and the crosslinking agent in step C2 is silane coupling agent KH-550.

[0122] The chain extender is epoxy chain extender ADR-4468; the antioxidant is butylated hydroxyanisole; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5:1.

[0123] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000 r / min for 0.5 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 150° C., and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160°C to a film thickness of 4 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0124] Comparative Example 8 A high-barrier biodegradable ground film, comprising the following raw materials in percentage by weight: 80 parts of polylactic acid prepolymer, 30 parts of chitosan solution, 10 parts of functional filler, 1 part of chain extender, 0.5 parts of antioxidant, and 0.3 parts of ultraviolet absorber.

[0125] Preparation of polylactic acid prepolymer: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6 hours at a temperature of 110°C and a pressure of 120 kPa; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 120°C and the pressure to 22 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200 r / min for 2 h; A3. Add plasticizer to the reactor, raise the temperature to 150°C, and stir the reaction at a rate of 100 r / min for 1 hour to obtain the desired polylactic acid prepolymer.

[0126] The composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 3:1, and the plasticizer is acetyl tributyl citrate; the mass ratio of lactic acid, the composite catalyst and the plasticizer is 100:1:10.

[0127] Preparation of chitosan solution: B1. Cleaning and crushing: The shrimp shells were placed in distilled water and ultrasonically cleaned at a frequency of 20kHz to remove impurities. After the ultrasonic cleaning, the shrimp shells were washed with distilled water for 3 times, dried in an oven at 70°C, crushed with a pulverizer, and passed through a 120-mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5%, treat with acid at 30°C for 4 hours, filter, take the filter cake, wash it with distilled water for 3 times and dry it to obtain the decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH in the reaction system is adjusted to 7, after stirring and enzymolyzing at 40°C for 2 hours, complex enzyme 2 is added, the pH in the reaction system is adjusted to 4, after stirring and enzymolyzing at 40°C for 3 hours, the mixture is filtered, the filter cake is washed with distilled water 3 times and then dried to obtain an enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60°C for 0.5 h, ultrasonicate at a frequency of 30 kHz for 1 h, filter, and collect the filtrate to obtain a chitosan solution.

[0128] The composite enzyme 1 in step B3 is a mixture of trypsin (enzyme activity: 2500U / mg), papain (enzyme activity: 2000U / mg) and serine protease (enzyme activity: 1800U / mg) in a mass ratio of 1:1:2; the composite enzyme 2 in step B3 is a mixture of chitinase (enzyme activity: 2500U / mg) and chitin deacetylase (enzyme activity: 3000U / mg) in a mass ratio of 1:2.5; and the mixed solvent in step B4 is a mixture of 2,3-epoxypropyltrimethylammonium chloride, citric acid and deionized water in a mass ratio of 0.6:0.3:3.

[0129] The mass ratio of crustacean shell to distilled water in step B1 is 1:5; the mass ratio of dry powder to 5% dilute hydrochloric acid in step B2 is 1:4; the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 in step B3 is 10:30:0.05:0.08; the mass ratio of enzymatic hydrolysis product to mixed solvent in step B4 is 10:25.

[0130] Preparation of functional fillers: C1, dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 20 kHz for 0.5 h to obtain a nano-silicon dioxide dispersion; C2. Mix the nano-silicon dioxide dispersion and the cross-linking agent in a mass ratio of 6:0.5, stir and dissolve at 40°C for 0.5h, ultrasonicate at a frequency of 30kHz for 1h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

[0131] The mass ratio of nano-silicon dioxide to organic solvent in step C1 is 1:10; the particle size of nano-silicon dioxide is 30 nm; the organic solvent is ethanol; and the cross-linking agent in step C2 is silane coupling agent KH-550.

[0132] The chain extender is epoxy chain extender ADR-4468; the antioxidant is butylated hydroxyanisole; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5:1.

[0133] A method for preparing a high-barrier biodegradable mulch film comprises the following steps: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000 r / min for 0.5 h; S2, putting the mixed and stirred raw materials into a twin-screw extruder, extruding at 150° C., and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160°C to a film thickness of 4 μm, and the high barrier biodegradable film is obtained after cooling and shaping.

[0134] Performance Testing The comprehensive properties of the high barrier biodegradable mulch films prepared in Examples 1-3 of the present application and Comparative Examples 1-8 were tested respectively.

[0135] Mechanical properties The tensile strength and elongation at break were tested according to GB / T 1040.3-2006. The test results are shown in Table 1 below.

[0136] Table 1 Mechanical properties of high barrier biodegradable mulch films

[0137] It can be seen from the data shown in Table 1 that the mechanical properties of the high barrier biodegradable mulch films prepared in Examples 1-3 are better than those of the high barrier biodegradable mulch films prepared in Comparative Examples 1-7.

[0138] Compared with Comparative Example 1, Example 1 replaces the plasticizer acetyl tributyl citrate in the process of making the homemade polylactic acid prepolymer and adds it in the S1 step of the mulch film preparation process on the basis of Example 1. The mechanical property test results of Comparative Example 1 are worse than those of Example 1, indicating that the plasticizer acetyl tributyl citrate is added in the process of preparing the polylactic acid prepolymer. Acetyl tributyl citrate can reduce the interaction force between polymer molecular chains and make the polymer chain segments move more easily, thereby increasing the flexibility and plasticity of the mulch film and improving the mechanical properties of the mulch film. However, the effect is not good when the plasticizer acetyl tributyl citrate is only added in the subsequent preparation process of the mulch film instead of reacting with the polylactic acid prepolymer in advance.

[0139] Compared with Comparative Examples 4-6, Example 1 is based on Example 1, and the enzymatic hydrolysis of compound enzyme 1 is deleted in the process of preparing chitosan solution. Comparative Example 5 is based on Example 1, and the enzymatic hydrolysis of compound enzyme 2 is deleted in the process of preparing chitosan solution. Comparative Example 6 is based on Example 1, and the enzymatic hydrolysis of compound enzyme 2 is firstly adopted and then the enzymatic hydrolysis of compound enzyme 1 is adopted. It indicates that compound enzyme 1 is first adopted to hydrolyze the protein of crustacean shell to improve the decomposition efficiency, and then compound enzyme 2 is adopted to hydrolyze the acetyl group and glycosidic bond on chitin to accelerate the conversion of chitin to chitosan. The chitosan obtained by the two enzymatic hydrolysis has a higher deacetylation degree and viscosity. The chitosan solution with high viscosity and high deacetylation degree is used in the subsequent mulch film production process, which can improve the mechanical properties of the mulch film prepared.

[0140] 2. Antibacterial properties: The determination method refers to the standard QB / T2591-2003 "Test method for antibacterial properties of antibacterial plastics and antibacterial effects". Escherichia coli (ATCC8099) and Staphylococcus aureus (ATCC6538) were inoculated into the high barrier biodegradable mulch films prepared in Examples 1-3 and Comparative Examples 1-8, covered with a polyethylene film, and cultured at (37±1)°C and relative humidity>90% for 24 hours. The antibacterial rate was calculated based on the actual number of live bacteria recovered. The determination results are shown in Table 2.

[0141] Table 2 Antibacterial properties of high barrier biodegradable mulch films

[0142] From the data shown in Table 2 above, it can be seen that the antibacterial properties of the high barrier biodegradable mulch prepared in Examples 1-3 are better than the antibacterial properties of the high barrier biodegradable mulch prepared in Comparative Examples 1-8. Compared with Comparative Examples 4-6, Example 1 is based on Example 1, and the part of the enzymatic hydrolysis of compound enzyme 1 is deleted in the process of preparing the chitosan solution. Comparative Example 5 is based on Example 1, and the part of the enzymatic hydrolysis of compound enzyme 2 is deleted in the process of preparing the chitosan solution. Comparative Example 6 is based on Example 1. First, compound enzyme 2 is used for enzymatic hydrolysis and then compound enzyme 1 is used for enzymatic hydrolysis. It shows that compound enzyme 1 is first used to hydrolyze the protein of the crustacean shell to improve the decomposition efficiency, and then compound enzyme 2 is used to hydrolyze the acetyl group and glycosidic bond on chitin to accelerate the conversion of chitin to chitosan. The chitosan obtained by the two enzymatic hydrolysis has a higher deacetylation degree and viscosity. The chitosan solution with high viscosity and high deacetylation degree is used in the subsequent mulch film production process, which can improve the antibacterial properties of the mulch film obtained.

[0143] 3. Barrier effect test The oxygen permeability test is conducted by using a gas permeometer, the test gas is high-purity oxygen, the constant temperature is 23°C, and the humidity is 0; the water vapor permeability is based on the national standard GB / T16928, the relative humidity (RH) is 90%, and the temperature is 38°C.

[0144] Table 3 Barrier properties of high barrier biodegradable mulch films

[0145] It can be seen from the data shown in Table 3 that the water vapor barrier performance of the high barrier biodegradable mulch films prepared in Examples 1-3 is better than the mechanical properties of the high barrier biodegradable mulch films prepared in Comparative Examples 1-8.

[0146] Compared with Example 1 and Comparative Examples 7-8, Comparative Example 7 is based on Example 1, but nano-silicon dioxide is not added when preparing the functional filler, and Comparative Example 8 is based on Example 1, but nano-cellulose is not added when preparing the functional filler. The water vapor barrier performance test results of Comparative Examples 7-8 are worse than those of Example 1, indicating that the granular structure of nano-silicon dioxide and the fibrous structure of nano-cellulose are intertwined to form a more dense and uniform physical barrier, further improving the barrier performance of the prepared ground film.

[0147] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A high barrier biodegradable mulch film, characterized in that: The invention comprises the following raw materials in parts by weight: 80-100 parts of polylactic acid prepolymer, 30-40 parts of chitosan solution, 10-20 parts of functional filler, 1-1.5 parts of chain extender, 0.5-1 parts of antioxidant and 0.3-0.8 parts of ultraviolet absorber.

2. The high barrier biodegradable mulch film according to claim 1, characterized in that: The polylactic acid prepolymer is prepared by the following method: A1. Put lactic acid into a reactor and carry out a dehydration reaction for 6-8 hours at a temperature of 110-130°C and a pressure of 120-130 kPa; A2. Add the composite catalyst into the reactor, adjust the reaction temperature to 120-130°C and the pressure to 22-24 kPa, protect the reaction with nitrogen throughout the reaction, and stir the reaction at a rate of 200-250 r / min for 2-3 hours; A3. Add plasticizer to the reactor, raise the temperature to 150-170°C, and stir the reaction at a rate of 100-150 r / min for 1-2 hours to obtain the desired polylactic acid prepolymer.

3. The high barrier biodegradable mulch film according to claim 2, characterized in that: The composite catalyst is a mixture of diethyl phosphite and manganese acetate in a mass ratio of 3-6:1, and the plasticizer is acetyl tributyl citrate; the mass ratio of the lactic acid, the composite catalyst and the plasticizer is 100:1-1.5:10-15.

4. The high barrier biodegradable mulch film according to claim 1, characterized in that: The chitosan solution is prepared in the following manner: B1. Cleaning and crushing: Place the shell of the crustacean in distilled water and perform ultrasonic cleaning at a frequency of 20-40kHz to remove impurities. After the ultrasonic cleaning, wash it with distilled water for 3-5 times, dry it in an oven at 70-80°C, crush it with a pulverizer, and pass it through a 120-180 mesh sieve to obtain dry powder; B2. Decalcification treatment: place the dry powder in step B1 in dilute hydrochloric acid with a mass concentration of 5-10%, treat with acid at 30-50°C for 4-6 hours, filter, take the filter cake, wash it with distilled water for 3-5 times, and then dry it to obtain a decalcified product; B3, enzymolysis: the decalcified product in step B2, distilled water and complex enzyme 1 are placed in a reaction vessel, the pH in the reaction system is adjusted to 7-8, after stirring and enzymolyzing at 40-60°C for 2-4h, complex enzyme 2 is added, the pH in the reaction system is adjusted to 4-6, after stirring and enzymolyzing at 40-50°C for 3-6h, the filter is taken, the filter cake is washed with distilled water for 3-5 times and then dried to obtain the enzymolysis product; B4. Place the enzymatic hydrolysis product in a mixed solvent, stir and dissolve at 60-80°C for 0.5-1h, ultrasonicate at 30-50kHz for 1-3h, filter, and collect the filtrate to obtain a chitosan solution.

5. The high barrier biodegradable mulch film according to claim 4, characterized in that: The compound enzyme 1 in step B3 is a mixture of trypsin, papain and serine protease in a mass ratio of 1:1-1.5:2-2.5; the compound enzyme 2 in step B3 is a mixture of chitinase and chitin deacetylase in a mass ratio of 1:2.5-3.5; the mixed solvent in step B4 is a mixture of quaternary ammonium salt, citric acid and deionized water in a mass ratio of 0.6-0.8:0.3-0.5:3-5.

6. The high barrier biodegradable mulch film according to claim 4, characterized in that: In the step B1, the mass ratio of crustacean shell to distilled water is 1:5-8; in the step B2, the mass ratio of dry powder to diluted hydrochloric acid with a mass concentration of 5% is 1:4-6; in the step B3, the mass ratio of decalcified product, distilled water, complex enzyme 1 and complex enzyme 2 is 10:30-40:0.05-0.08:0.08-0.12; in the step B4, the mass ratio of enzymatic hydrolysis product to mixed solvent is 10:25-35.

7. The high barrier biodegradable mulch film according to claim 1, characterized in that: The functional filler is prepared by the following steps: C1. Dispersing nano-silicon dioxide in an organic solvent, and ultrasonicating at a frequency of 20-30 kHz for 0.5-1 h to obtain a nano-silicon dioxide dispersion; dispersing nano-cellulose in an organic solvent, and ultrasonicating at a frequency of 20-30 kHz for 0.5-1 h to obtain a nano-cellulose dispersion; C2. Mix nano-silicon dioxide dispersion, nano-cellulose dispersion and cross-linking agent in a mass ratio of 2.5-4.5:3.5-8:0.5-0.8, stir and dissolve at 40-50°C for 0.5-1h, ultrasonicate at a frequency of 30-50kHz for 1-3h, filter, and dry the filtrate under reduced pressure to remove the solvent to obtain the desired functional filler.

8. The high barrier biodegradable mulch film according to claim 7, characterized in that: In the step C1, the mass ratio of nano-silicon dioxide to organic solvent is 1:10-12; the mass ratio of nano-cellulose to organic solvent is 1:10-12; the particle size of the nano-silicon dioxide is 20-40nm; the organic solvent is ethanol or acetone; and the cross-linking agent in the step C2 is one of silane coupling agents KH-550, KH-560 or KH-570.

9. The high barrier biodegradable mulch film according to claim 1, characterized in that: The chain extender is an epoxy chain extender ADR; the antioxidant is one or a combination of butylated hydroxyanisole, dibutyl hydroxytoluene or tert-butylhydroquinone; and the ultraviolet absorber is a mixture of ultraviolet absorber UV-P and ultraviolet absorber UV-326 in a mass ratio of 1.5-2.8:

1.

10. A method for preparing a high barrier biodegradable mulch film according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Weigh polylactic acid prepolymer, chitosan solution, functional filler, chain extender, antioxidant, and ultraviolet absorber by weight, put them into a high-speed blender, and mix and stir at a speed of 2000-3000 r / min for 0.5-1h; S2, putting the mixed raw materials into a twin-screw extruder, extruding at 150-200°C, and air-cooling and granulating; S3, the pellets are extruded to form a tubular film blank, the tubular film blank is inflated at 160-180°C to a film thickness of 4-8 μm, and the high barrier biodegradable mulch film is obtained after cooling and shaping.

Citation Information

Patent Citations

  • High strength and high heat resistance polylactic acid composite material and preparation method thereof

    CN101962468A

  • Biodegradable polylactic acid antibacterial film and preparation method thereof

    CN112029249A

Cited By

  • Biodegradable plastic derived from shrimp shell waste and method of preparation thereof

    KR103007372B1