Anti-corrosion coating for marine environment and coating method of anti-corrosion coating

Through composite coating technology of graphene and copper oxide, corrosion and biological adhesion of steel facilities in the marine environment is solved, efficient anti-corrosion and anti-fouling effects are achieved, extending the service life of the facilities and reducing maintenance costs. .

CN119039818AInactive Publication Date: 2024-11-29MIANYANG JINWEI MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411279676.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Steel facilities in the marine environment are susceptible to corrosion and biological adhesion damage, resulting in increased navigational drag, accelerated corrosion, equipment failure and increased maintenance frequency, resulting in significant economic and military losses.

Method used

The composite coating of graphene as a corrosion factor and cuprous oxide or corrosion inhibitor as a bactericidal factor is used, combined with thermal zinc spray or aluminum composite coating, forms a multi-layer coating structure, providing physical barriers and chemical protection to prevent oxygen and corrosion Media penetration inhibits biological attachment.

Benefits of technology

It significantly improves the corrosion resistance and biological adhesion resistance of metal materials, extends the service life of the facility, and reduces maintenance costs and navigation fuel consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039818A_ABST
    Figure CN119039818A_ABST
Patent Text Reader

Abstract

The invention provides an anticorrosive paint for a marine environment, which is characterized in that the anticorrosive paint comprises a primer, an intermediate paint and a finish paint, the primer, the intermediate paint and the finish paint are composite coatings loaded with anticorrosive factors and bactericidal factors for preventing biological adhesion, and the anticorrosive factors are from graphene; and the sterilization factor is from cuprous oxide, a corrosion inhibitor or a bactericide. The coating method of the anticorrosive paint comprises the following steps: S1, manual rust removal; s2, primer coating; s3, intermediate paint is coated; and S4, finish paint is coated. Graphene has a physical barrier effect and can prevent permeation of oxygen and a corrosive medium, so that the permeation performance of the anticorrosive coating is reduced, the corrosion resistance of the coating is improved, the corrosion inhibition and passivation effects on a metal material are realized, and efficient corrosion protection is provided; cuprous oxide is mainly used for ship bottom antifouling (for killing low-grade marine animals) and insect killing; the corrosion inhibitor or the bactericide can effectively inhibit adhesion and growth of marine organisms on the surface of the coating, so that efficient organism adhesion prevention protection is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of anti-corrosion coatings and anti-biological attachment coatings, and in particular to an anti-corrosion coating for use in a marine environment and a coating method thereof. Background Art

[0002] Seawater, sunshine, sea breeze, marine life and marine atmosphere are highly corrosive to marine and coastal facilities. Maritime equipment is mostly made of steel, such as submarine oil and gas pipelines, drilling platforms, cross-sea bridges, offshore wind power stations, nuclear power plants, port machinery and equipment, and ships. This is because steel has the characteristics of wide availability, low price, good mechanical properties, and good machinability. However, steel is extremely susceptible to severe corrosion and its service life is reduced. In addition, the ocean also has a demand for marine anti-biological attachment. Biological attachment is a general term for animals, plants and microorganisms that attach to the surface of underwater artificial facilities and marine structures such as ships and cause damage or adverse effects, such as barnacles, oysters and mussels. Biological attachment is fatal to ships, mainly including:

[0003] (1) Increase the ship's navigation resistance, reduce the navigation speed, and increase fuel consumption;

[0004] (2) Change the surface properties of metal materials and accelerate metal corrosion;

[0005] (3) Harming the piping system and affecting the normal operation of equipment;

[0006] (4) The number of times ships need to go into dry dock for maintenance increases, resulting in significant losses such as reduced ship efficiency and shortened service life.

[0007] Corrosion and fouling have become a serious problem faced by marine engineering. The projects of anti-corrosion and anti-biological attachment on the surface of ships and other marine structures have great social and economic value and military significance. Summary of the invention

[0008] In order to overcome the deficiencies and shortcomings of the prior art, an anti-corrosion coating for use in a marine environment and a coating method thereof are provided.

[0009] The first aspect of the present invention is to provide an anti-corrosion coating for use in a marine environment, comprising a primer, an intermediate paint and a topcoat, wherein the primer, the intermediate paint and the topcoat are composite coatings loaded with an anti-corrosion factor and a bactericidal factor for preventing biological attachment, wherein the anti-corrosion factor comes from graphene; and the bactericidal factor comes from cuprous oxide, a corrosion inhibitor or a bactericide.

[0010] Preferably, the primer is a graphene-zinc-epoxy primer or a graphene-iron red-epoxy primer, and a hot-sprayed zinc, aluminum or zinc-aluminum composite coating is used as the base layer of the organic coating or as the overall protective coating of the steel structure alone. The primer contains fillers for providing shielding and cathodic protection.

[0011] Preferably, the intermediate paint is graphene-glass flake-epoxy intermediate paint or graphene-mica iron-epoxy intermediate paint.

[0012] Preferably, the topcoat is made of polyurethane, acrylic resin or vinyl resin coating, and the topcoat is graphene polyurethane topcoat or graphene fluorocarbon topcoat.

[0013] Preferably, the anti-corrosion coating further comprises: solvent-free barrier paint; the solvent-free barrier paint is solvent-free graphene barrier paint or graphene aluminum alloy barrier paint.

[0014] The second aspect of the present invention provides a coating method of an anticorrosive coating for a marine environment according to the first aspect, comprising:

[0015] S1, manual rust removal;

[0016] S2, painting primer;

[0017] S3, application of intermediate paint;

[0018] S4, topcoat.

[0019] Preferably, S2 includes:

[0020] S21, determine the properties of the primer material to be coated; the properties of the primer material in this embodiment include: volume solid content of 72% ± 2; dry film thickness of 80-100 μm; wet film thickness of 180-200 μm; theoretical coating rate of 3m 2 / kg and the dry film thickness is 80μ, the color is red and the paint surface is matte;

[0021] S22, primer is applied by air spray or airless spray, the distance of air spray is 0.38-0.48mm, the pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes;

[0022] S23, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

[0023] Preferably, S3 includes:

[0024] S31, determine the properties of the intermediate paint material for coating; the properties of the intermediate paint material in this embodiment include: volume solid content of 72% ± 2; dry film thickness of 80-100μm; wet film thickness of 180-200μm; theoretical coating rate of 3m 2 / kg and the dry film thickness is 80μm, the color is metallic gray and the paint surface is matte;

[0025] S32, intermediate coating based on air spray or airless spray method, air spray distance is 0.38-0.48mm, pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes;

[0026] S33, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

[0027] Preferably, S4 includes:

[0028] S41, determine the properties of the topcoat material to be coated; the properties of the topcoat material in this embodiment include: volume solid content of 60% ± 2; dry film thickness of 60-80 μm; wet film thickness of 120-150 μm; theoretical coating rate of 3m 2 / kg and the dry film thickness is 80μm, the color is silvery white and the paint surface is matte;

[0029] S42, intermediate coating based on air spray or airless spray method, air spray distance is 0.38-0.48mm, pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes;

[0030] S43, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

[0031] Preferably, in the case where the anti-corrosion coating further includes a solvent-free barrier paint, the coating method further includes: S5, coating the solvent-free barrier paint;

[0032] Wherein, the S5 includes:

[0033] S51, determine the properties of the solvent-free barrier paint material to be applied; the properties of the solvent-free barrier paint material in this embodiment include: volume solid content> 97%; dry film thickness is 250-300μm; wet film thickness is 300-320μm; theoretical coating rate is 4m 2 / kg and the dry film thickness is 80μm, the color is metallic gray and the paint surface is matte;

[0034] S42, intermediate coating based on air spray or airless spray method, air spray distance is 0.38-0.48mm, pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes;

[0035] S43, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

[0036] Beneficial effects of the present invention:

[0037] (1) Graphene is used as a diffusion barrier. The anti-corrosion factor provided by graphene is used. Graphene is a two-dimensional carbon nanomaterial that is chemically inert, has antioxidant ability, has anti-diffusion properties for oxygen, and has a special lamellar structure. It can be used as a filler in anti-corrosion coatings, thereby having a physical barrier effect, hindering the penetration of oxygen and corrosive media, reducing the permeability of the anti-corrosion coating, improving the corrosion resistance of the coating, and achieving corrosion inhibition and passivation of metal materials, thereby providing efficient corrosion protection.

[0038] (2) The fungicide factor comes from cuprous oxide, corrosion inhibitors or other dedicated fungicides. Cuprous oxide is mainly used for antifouling of ship bottoms (to kill low-level marine animals) and insecticides; corrosion inhibitors or other dedicated fungicides can effectively inhibit the attachment and growth of marine organisms on the coating surface, thereby providing efficient protection against biofouling.

[0039] Based on the following detailed description of specific embodiments of the present invention in conjunction with the accompanying drawings, those skilled in the art will become more aware of the above and other objects, advantages and features of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Hereinafter, some specific embodiments of the present invention will be described in detail in an exemplary and non-limiting manner with reference to the accompanying drawings. The same reference numerals in the accompanying drawings indicate the same or similar components or parts. It should be understood by those skilled in the art that these drawings are not necessarily drawn to scale. The objects and features of the present invention will become more apparent in view of the following description in conjunction with the accompanying drawings, in which:

[0041] Figure 1 Schematic diagram of the principle of using graphene as a diffusion barrier according to an embodiment of the present invention. DETAILED DESCRIPTION

[0042] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0043] This embodiment provides an anti-corrosion coating for marine environment, including a primer, an intermediate paint and a topcoat, wherein the primer, the intermediate paint and the topcoat are composite coatings loaded with an anti-corrosion factor and a bactericidal factor for preventing biological attachment, wherein the anti-corrosion factor is derived from graphene;

[0044] like Figure 1 The figure shows the principle diagram of graphene as a diffusion barrier. The anti-corrosion factor provided by graphene is that graphene is a two-dimensional carbon nanomaterial, which is chemically inert, has antioxidant ability, has anti-diffusion properties to oxygen, and has a special lamellar structure. It can be used as a filler in anti-corrosion coatings, thereby having a physical barrier effect, hindering the penetration of oxygen and corrosive media, reducing the permeability of the anti-corrosion coating, improving the corrosion resistance of the coating, and achieving corrosion inhibition and passivation of metal materials.

[0045] As a preferred embodiment, the bactericidal factor comes from cuprous oxide, corrosion inhibitor or other exclusive bactericide. Cuprous oxide is mainly used for antifouling of ship bottom (to kill low-level marine animals) and insecticide; corrosion inhibitor or other exclusive bactericide can effectively inhibit the attachment and growth of marine organisms on the coating surface.

[0046] As a preferred embodiment, the primer is graphene-zinc-epoxy primer or graphene-iron red-epoxy primer.

[0047] When graphene-zinc-epoxy primer is used, it has good adhesion to the substrate, strong salt spray resistance, good flexibility and impact resistance; it is often used in the field of heavy anti-corrosion technology;

[0048] When using graphene-iron red-epoxy primer, it has good adhesion to the substrate, excellent flexibility and impact resistance, and high cost performance; it is often used in oil tank corrosion protection, oil pipeline corrosion protection, ship corrosion protection or chemical corrosion protection and other fields.

[0049] In this embodiment, the primer is generally an organic or inorganic epoxy primer. The hot-sprayed zinc, aluminum or zinc-aluminum composite coating can be used as the bottom layer of the organic coating, or can be used alone as the overall protective coating of the steel structure. The filler in the primer, such as Zn powder, can provide a shielding effect and a cathodic protection effect.

[0050] As a preferred embodiment, the intermediate paint is graphene-glass flake-epoxy intermediate paint or graphene-mica iron-epoxy intermediate paint.

[0051] When graphene-glass flake-epoxy intermediate paint is used, it has good adhesion to the primer layer, good water vapor barrier and shielding performance, and good construction performance; it is often used in the fields of ship corrosion protection or chemical corrosion protection;

[0052] When using graphene-mica iron-epoxy intermediate paint, it has good adhesion with the primer layer, good water vapor barrier and shielding properties, and good construction performance; it is often used in fields such as chemical equipment corrosion protection or engineering machinery corrosion protection.

[0053] In this embodiment, the intermediate paint is mainly epoxy paint, which needs to have sufficient anti-penetration ability, such as epoxy micaceous iron, epoxy glass flake, etc.

[0054] As a preferred embodiment, the topcoat is a graphene polyurethane topcoat or a graphene fluorocarbon topcoat.

[0055] When graphene polyurethane topcoat is used, it has good weather resistance and resistance to ultraviolet radiation, can be mixed with various colors, and has decorative and aesthetic functions; it is often used in fields such as ship corrosion protection or chemical corrosion protection.

[0056] When graphene fluorocarbon topcoat is used, it has good weather resistance, resistance to UV radiation, can be mixed with various colors, and has decorative and aesthetic functions; it is often used in the field of oil tank anti-corrosion or oil pipeline anti-corrosion technology.

[0057] In this embodiment, the topcoat is generally made of polyurethane, acrylic resin or vinyl resin coating, and the topcoat is required to have high weather resistance.

[0058] As a preferred embodiment, the anti-corrosion coating further comprises: solvent-free barrier paint.

[0059] As a preferred embodiment, the solvent-free barrier paint is solvent-free graphene barrier paint or graphene aluminum alloy barrier paint.

[0060] When solvent-free graphene barrier paint is used, there is no VOC emission, good permeability, strong adhesion, it can be constructed with water vapor, and the coating has strong density; it is often used in the field of reinforced concrete anti-corrosion or cement pier anti-corrosion;

[0061] When using graphene aluminum alloy barrier paint, it has good permeability, strong adhesion, can be constructed with rust, and has a strong coating density. It is often used in the field of magnesium alloy or aluminum alloy anti-corrosion technology.

[0062] The second aspect of the present invention provides a coating method of an anticorrosive coating for a marine environment according to the first aspect, comprising:

[0063] S1, manual rust removal;

[0064] S2, painting primer;

[0065] S3, application of intermediate paint;

[0066] S4, topcoat.

[0067] As shown in Table 1, the graphene primer coating instructions, as a preferred embodiment, the S2 includes:

[0068] S21, determine the properties of the primer material to be coated; the properties of the primer material in this embodiment include: volume solid content of 72% ± 2; dry film thickness of 80-100 μm; wet film thickness of 180-200 μm; theoretical coating rate of 3m 2 / kg and the dry film thickness is 80μ, the color is red and the paint surface is matte;

[0069] S22, primer is applied by air spray or airless spray, the distance of air spray is 0.38-0.48mm, the pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes;

[0070] S23, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

[0071] Table 1

[0072]

[0073] As shown in Table 2, the graphene intermediate paint coating instructions, as a preferred embodiment, the S3 includes:

[0074] S31, determine the properties of the intermediate paint material for coating; the properties of the intermediate paint material in this embodiment include: volume solid content of 72% ± 2; dry film thickness of 80-100μm; wet film thickness of 180-200μm; theoretical coating rate of 3m 2 / kg and the dry film thickness is 80μm, the color is metallic gray and the paint surface is matte;

[0075] S32, intermediate coating based on air spray or airless spray method, air spray distance is 0.38-0.48mm, pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes;

[0076] S33, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

[0077] Table 2

[0078]

[0079] As shown in Table 3, the surface coating description, as a preferred embodiment, the S4 includes:

[0080] S41, determine the properties of the topcoat material to be coated; the properties of the topcoat material in this embodiment include: volume solid content of 60% ± 2; dry film thickness of 60-80 μm; wet film thickness of 120-150 μm; theoretical coating rate of 3m 2 / kg and the dry film thickness is 80μm, the color is silvery white and the paint surface is matte;

[0081] S42, intermediate coating based on air spray or airless spray method, air spray distance is 0.38-0.48mm, pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes;

[0082] S43, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

[0083] Table 3

[0084]

[0085] As a preferred embodiment, in the case where the anti-corrosion coating further includes solvent-free barrier paint, the coating method further includes:

[0086] S5, applying the solvent-free barrier paint.

[0087] As shown in Table 4, the solvent-free barrier paint coating instructions, as a preferred embodiment, the S5 includes:

[0088] S51, determine the properties of the solvent-free barrier paint material to be applied; the properties of the solvent-free barrier paint material in this embodiment include: volume solid content> 97%; dry film thickness is 250-300μm; wet film thickness is 300-320μm; theoretical coating rate is 4m 2 / kg and the dry film thickness is 80μm, the color is metallic gray and the paint surface is matte;

[0089] S42, intermediate coating based on air spray or airless spray method, air spray distance is 0.38-0.48mm, pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes;

[0090] S43, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

[0091] Table 4

[0092]

[0093] Application examples:

[0094] The anti-corrosion coating and Hempel anti-fouling coating were applied on the same wall and cabin surface for comparative testing, and biological attachment and corrosion parameters were measured to determine that the anti-fouling effects of the test anti-corrosion coating and Hempel anti-fouling coating were basically equivalent.

[0095] Anti-corrosion coatings are widely used in a special marine atmosphere experimental station in the South China Sea, a substation coating project in Haiyan, Jiaxing, and a test field for atmospheric and soil corrosion of power grid materials. At the same time, after overall coating of fixed steel equipment in a certain offshore project, it was found that the anti-fouling coating below the waterline area had good anti-fouling performance after one year of operation at sea.

[0096] Although preferred embodiments of the present invention have been described, additional changes and modifications may be made to these embodiments by those skilled in the art once the basic inventive concepts are known. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention. Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. An anticorrosive coating for use in a marine environment, characterized in that: The invention comprises a primer, an intermediate paint and a topcoat, wherein the primer, the intermediate paint and the topcoat are composite coatings loaded with anticorrosive factors and bactericidal factors for preventing biological attachment, wherein the anticorrosive factors are from graphene, and the bactericidal factors are from cuprous oxide, corrosion inhibitor or bactericide.

2. The anticorrosive coating for marine environment according to claim 1, characterized in that: The primer is a graphene-zinc-epoxy primer or a graphene-iron red-epoxy primer, and a hot-sprayed zinc, aluminum or zinc-aluminum composite coating is used as the bottom layer of the organic coating or as the overall protective coating of the steel structure alone. The primer contains fillers for providing shielding and cathodic protection effects.

3. The anti-corrosion coating for marine environment according to claim 1, characterized in that: The intermediate paint is graphene-glass flake-epoxy intermediate paint or graphene-micaceous iron-epoxy intermediate paint.

4. The anticorrosive coating for marine environment according to claim 1, characterized in that: The topcoat is made of polyurethane, acrylic resin or vinyl resin coating, and the topcoat is graphene polyurethane topcoat or graphene fluorocarbon topcoat.

5. The anticorrosive coating for marine environment according to claim 1, characterized in that: The anti-corrosion coating also includes: solvent-free barrier paint; the solvent-free barrier paint is solvent-free graphene barrier paint or graphene aluminum alloy barrier paint.

6. A coating method for an anticorrosive coating for a marine environment according to any one of claims 1 to 5, characterized in that: include: S1, manual rust removal; S2, painting primer; S3, application of intermediate paint; S4, topcoat.

7. The coating method according to claim 6, characterized in that: The S2 includes: S21, determine the properties of the primer material to be coated; the properties of the primer material in this embodiment include: volume solid content of 72% ± 2; dry film thickness of 80-100 μm; wet film thickness of 180-200 μm; theoretical coating rate of 3m 2 / kg and the dry film thickness is 80μ, the color is red and the paint surface is matte; S22, primer is applied by air spray or airless spray, the distance of air spray is 0.38-0.48mm, the pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes; S23, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

8. The coating method according to claim 7, characterized in that: The S3 includes: S31, determine the properties of the intermediate paint material for coating; the properties of the intermediate paint material in this embodiment include: volume solid content of 72% ± 2; dry film thickness of 80-100μm; wet film thickness of 180-200μm; theoretical coating rate of 3m 2 / kg and the dry film thickness is 80μm, the color is metallic gray and the paint surface is matte; S32, intermediate coating based on air spray or airless spray method, air spray distance is 0.38-0.48mm, pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes; S33, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

9. The coating method according to claim 8, characterized in that: The S4 includes: S41, determine the properties of the topcoat material to be coated; the properties of the topcoat material in this embodiment include: volume solid content of 60% ± 2; dry film thickness of 60-80 μm; wet film thickness of 120-150 μm; theoretical coating rate of 3m 2 / kg and the dry film thickness is 80μm, the color is silvery white and the paint surface is matte; S42, intermediate coating based on air spray or airless spray method, air spray distance is 0.38-0.48mm, pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes; S43, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

10. The coating method according to claim 9, characterized in that: In the case where the anti-corrosion coating also includes solvent-free barrier paint, the coating method further includes: S5, coating the solvent-free barrier paint; Wherein, the S5 includes: S51, determine the properties of the solvent-free barrier paint material to be applied; the properties of the solvent-free barrier paint material in this embodiment include: volume solid content> 97%; dry film thickness is 250-300μm; wet film thickness is 300-320μm; theoretical coating rate is 4m 2 / kg and the dry film thickness is 80μm, the color is metallic gray and the paint surface is matte; S42, intermediate coating based on air spray or airless spray method, air spray distance is 0.38-0.48mm, pressure is 110-1600kg / cm 2 , brushing or rolling process is used for corners of different shapes; S43, drying after painting, wherein the surface temperature corresponding to drying is 15-35 degrees Celsius, the surface drying time is 2-4 hours, the actual drying time is 28-48 hours, the lightest recoating time is 6-8 hours, the longest recoating time is 1 month, and the service life is 2-4 hours.

Citation Information

Patent Citations

  • Supporting anti-corrosive coating modified by graphene, preparation and application thereof

    CN105419437A

  • Anti-corrosion coating system for outer wall of tower drum of marine wind turbine generator and coating method

    CN113150642A

  • Functionalised graphene and coatings comprising the same

    US20230044239A1

Cited By

  • Marine photovoltaic anticorrosive coating composition and preparation method thereof

    CN122405142A

  • A marine photovoltaic anticorrosive coating composition and a preparation method thereof

    CN122405142B