Iron oxide pigment dispersion as well as preparation method and application thereof
By modifying iron oxide pigments with polybasic acids, polyols, and substances containing both hydroxyl and carboxyl groups, a hyperbranched structure is formed, which solves the problems of dispersibility and stability of iron oxide pigments in acrylic coatings, and achieves good tinting strength and post-heat storage performance stability.
Patent Information
- Application Number
- CN202411155439.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
There are no reports in the existing technology on modifying iron oxide pigments with polybasic acids, polyols, or substances containing both hydroxyl and carboxyl groups and applying them to acrylic coatings. This results in iron oxide pigments being prone to agglomeration and poor dispersibility during storage, which affects tinting strength and coating performance.
Iron oxide pigments are modified by using polybasic acids, polyols, and substances containing both hydroxyl and carboxyl groups to form modified iron oxide pigments with hydrophilic hyperbranched structures. These pigments are stably dispersed through steric hindrance and electrostatic repulsion and can be applied to acrylic coatings.
Modified iron oxide pigments exhibit good dispersibility and compatibility in acrylic coatings, strong tinting strength, stable performance after heat storage, small color difference, and good compatibility with acrylic coatings.
Smart Images

Figure BDA0005004839300000111 
Figure BDA0005004839300000121 
Figure BDA0005004839300000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fine chemical industry, and in particular to an iron oxide pigment dispersion and a preparation method and application thereof. Background Art
[0002] Iron oxide pigments mainly refer to three kinds of coloring pigments, namely iron oxide red, iron yellow and iron black, which are based on iron oxide. By blending, composite pigments of a series of color spectra such as orange, brown and green can be obtained. Among them, iron oxide red is the main one, accounting for about 50% of iron oxide pigments. Iron oxide pigments are the second largest inorganic pigment after titanium dioxide and the largest colored inorganic pigment. Iron oxide pigments have good light resistance, weather resistance, alkali resistance and solvent resistance, and are also non-toxic. They are widely used in coatings, inks, plastics, ceramics, papermaking and other industries. Compared with organic pigments, iron oxide pigments have defects such as high density, difficult grinding of particles, and easy sedimentation of pigment particles during storage. In addition, the adsorption force of dispersants on the surface of iron oxide pigments is small and the desorption phenomenon is serious. After long-term storage, the coloring power is easily reduced due to dispersant desorption and pigment particle agglomeration.
[0003] In the prior art, suitable dispersants are used to improve the stability and dispersibility of pigments. For example, Chinese patent No. CN113913051A discloses a high-concentration, stable, water-based, environmentally friendly iron oxide color paste for a color mixing machine and a preparation method thereof. A polymerizable surface-activated polymer dispersant with specific configuration parameters is added to the formula. The effective parts of the dispersant include polyoxyethylene oleate, decyl glucoside and phosphate-type anionic surfactant, which can reduce the amount of cosolvent, improve the anti-drying property of the water-based iron oxide color paste, and reduce or do not use other dispersants to prepare a high-concentration, low-viscosity, stable, water-based environmentally friendly iron oxide color paste; Chinese patent No. CN105885658A discloses a water-based one-component automotive paint containing iron oxide pigment and a preparation method thereof, wherein the dispersant in the iron oxide color paste is a compound of an anionic high molecular weight dispersant and an anionic low molecular weight dispersant, and a color paste suitable for automotive paint is prepared in synergistic with a wetting agent and an anti-settling agent.
[0004] Surface modification of pigment particles can change the physical and chemical properties of the pigment particle surface, improve its dispersibility, weather resistance, acid and alkali resistance, and make it more in line with the application requirements of its downstream application fields. For example, US Patents No. US5865885 and US5922121 respectively introduce methods for hydrophilic and hydrophobic surface treatment of pigments to obtain pigment dispersions with smaller average particle size, narrower particle size distribution, and more stability in various solvents; US Patent No. US6524705 discloses a method for surface modification of metal oxides using silicon-containing compounds to improve their dispersibility in various organic solvents such as mineral oil and fluorine-containing solutions; Chinese Patent No. CN102604447A discloses a method for surface treatment of pigments using phosphorus-containing compounds to improve the stability and tinting power of the pigment in preparing water-based color pastes.
[0005] However, there is no report in the prior art about modifying iron oxide pigments with polyacids, polyols, and substances containing both hydroxyl groups and carboxyl groups in sequence and applying them to acrylic paints. Summary of the invention
[0006] In order to solve the above technical problems, the purpose of the present invention is to provide an iron oxide pigment dispersion and a preparation method and application thereof; the modified iron oxide pigment in the iron oxide pigment dispersion of the present invention can be stably dispersed through steric hindrance and electrostatic repulsion, has a small fineness, a strong relative tinting strength, a small color difference ΔE, and the fineness, relative tinting strength and color difference ΔE do not change significantly after heat storage, and has good compatibility with acrylic paint, and the relative tinting strength and color difference ΔE of the paint prepared by using the same do not change significantly after oscillation and heat storage.
[0007] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0008] On the one hand, the present invention provides an iron oxide pigment dispersion, which comprises, by weight, 40 to 55 parts of modified iron oxide pigment, 2 to 5 parts of humectant, 0.1 to 0.5 parts of defoamer, 0.01 to 0.05 parts of mildew and fungicide per 100 parts of the iron oxide pigment dispersion, and the balance is water; wherein the modified iron oxide pigment is obtained by reacting the iron oxide pigment with a polyacid, a polyol, and a substance containing both hydroxyl and carboxyl groups in sequence.
[0009] Further, the polyacid is one of polyacrylic acid, polymethacrylic acid, terephthalic acid, isophthalic acid, succinic acid, glutaric acid, adipic acid, etc., preferably polyacrylic acid, more preferably polyacrylic acid with an average molecular weight of 5000; the polyol is one of pentaerythritol, glycerol, ethylene glycol, propylene glycol, butanediol, pentanediol and hexanediol, etc., preferably pentaerythritol; the substance containing both hydroxyl and carboxyl groups is one of 2,2-dihydroxymethylpropionic acid, 2-hydroxyhexanoic acid, 3-hydroxyhexanoic acid, 9-hydroxynonanoic acid, p-hydroxybenzoic acid, o-hydroxybenzoic acid, m-hydroxybenzoic acid, 2,3-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4,5-trihydroxybenzoic acid, 2,4,6-trihydroxybenzoic acid, etc., preferably 2,2-dihydroxymethylpropionic acid.
[0010] Furthermore, the modified iron oxide pigment is obtained by reacting 10 parts of iron oxide pigment with 0.1-0.3 parts of polyacid, 0.2-0.6 parts of polyol, and 2.0-5.0 parts of a substance containing both hydroxyl and carboxyl groups.
[0011] Furthermore, the preparation steps of the modified iron oxide pigment are:
[0012] a) dispersing 10 parts of iron oxide pigment into 50 parts of water, adding 100 parts of DMF to disperse evenly, and then adding 10 parts of DMF solution containing 0.1-0.3 parts of polyacid to mix and disperse; reacting at 120-140° C. for 8-10 hours, cooling, filtering, washing and drying to obtain iron oxide pigment containing polyacid;
[0013] b) 10 parts of iron oxide pigment containing polyacid, 0.2-0.6 parts of polyol, 0.1-0.2 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 70-90° C. and reacted for 2-4 hours; then 2.0-5.0 parts of a substance containing both hydroxyl and carboxyl groups are added, the reaction is continued for 2-4 hours, cooled, filtered, washed and dried to obtain a modified iron oxide pigment.
[0014] Furthermore, the iron oxide pigment is at least one of iron oxide red pigment, iron oxide yellow pigment and iron oxide black pigment.
[0015] Furthermore, the moisturizing agent is at least one of polyethylene glycol, glycerol, ethylene glycol, propylene glycol, n-propanol, n-butanol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, triethylene glycol, and tetraethylene glycol, preferably polyethylene glycol 300.
[0016] Furthermore, the defoaming agent is at least one of polyethers, polysiloxanes, and polyether-modified silicones, and is preferably a polyether-modified silicone defoaming agent.
[0017] During the storage and use of the product, due to the growth of bacteria, the product performance is destroyed, the quality is reduced, and corruption phenomena such as bloating, barrel swelling, viscosity reduction, pigment precipitation, pH drift, etc. occur, which eventually lead to the abandonment of the product material and cause losses to users and producers. When producing the product, mildew-proof fungicides must be added to prevent and inhibit the survival of microorganisms to ensure the quality of the product. In the present invention, as long as it can ensure that the above phenomenon will not occur during the storage and use of the color paste and the mildew-proof fungicides comply with the relevant regulations of the coatings industry, they can be used, preferably 1,2-benzisothiazolin-3-one.
[0018] Another aspect of the present invention provides a method for preparing an iron oxide pigment dispersion, wherein a moisturizer, a defoamer, and an antifungal bactericide are added to water and dispersed evenly, and then a modified iron oxide pigment is added and dispersed evenly, and an alkali solution is used to adjust the pH value to 8 to 9, and then the alkali solution is ground and filtered to obtain an iron oxide pigment dispersion. The alkali solution is at least one of sodium hydroxide, potassium hydroxide, and ammonia water, preferably a sodium hydroxide solution.
[0019] The present invention also provides an application of the above iron oxide pigment dispersion in acrylic paint, such as in architectural paint.
[0020] The beneficial effects of the present invention are:
[0021] Part of the carboxyl groups in the polyacid of the present invention undergoes an esterification reaction with the hydroxyl groups on the surface of the iron oxide pigment, so that the polyacid can be partially coated on the surface of the iron oxide pigment, and then the remaining carboxyl groups in the polyacid undergo an esterification reaction with part of the hydroxyl groups in the polyol; the remaining hydroxyl groups in the polyol undergo an esterification reaction with the carboxyl groups in the substance containing both hydroxyl groups and carboxyl groups, and the hydroxyl groups in the substance containing both hydroxyl groups and carboxyl groups can continue to undergo an esterification reaction with the carboxyl groups contained therein, thereby forming a hydrophilic hyperbranched structure polymer on the surface of the iron oxide pigment. The modified iron oxide pigment can be stably dispersed through steric hindrance and electrostatic repulsion, has a small fineness, a strong relative tinting strength, a small color difference ΔE, and the fineness, relative tinting strength and color difference ΔE do not change significantly after heat storage; and it has good compatibility with acrylic paint, and the paint prepared by using it does not change significantly in relative tinting strength and color difference ΔE after oscillation and heat storage. DETAILED DESCRIPTION
[0022] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] The invention provides an iron oxide pigment dispersion, which comprises, by weight, 40 to 55 parts of modified iron oxide pigments, 2 to 5 parts of moisturizers, 0.1 to 0.5 parts of defoamers, 0.01 to 0.05 parts of mildew and fungicide per 100 parts of the iron oxide pigment dispersion, and the balance is water; wherein the modified iron oxide pigment is obtained by reacting the iron oxide pigment with polyacids, polyols, and substances containing both hydroxyl groups and carboxyl groups in sequence.
[0024] Among them, the polyacid is one of polyacrylic acid, polymethacrylic acid, terephthalic acid, isophthalic acid, succinic acid, glutaric acid, adipic acid, etc., preferably polyacrylic acid, more preferably polyacrylic acid with an average molecular weight of 5000; the polyol is one of pentaerythritol, glycerol, ethylene glycol, propylene glycol, butanediol, pentanediol and hexanediol, etc., preferably pentaerythritol; the substance containing both hydroxyl and carboxyl groups is one of 2,2-dihydroxymethylpropionic acid, 2-hydroxyhexanoic acid, 3-hydroxyhexanoic acid, 9-hydroxynonanoic acid, p-hydroxybenzoic acid, o-hydroxybenzoic acid, m-hydroxybenzoic acid, 2,3-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4,5-trihydroxybenzoic acid, 2,4,6-trihydroxybenzoic acid, etc., preferably 2,2-dihydroxymethylpropionic acid.
[0025] Furthermore, the modified iron oxide pigment is obtained by reacting 10 parts of iron oxide pigment with 0.1-0.3 parts of polyacid, 0.2-0.6 parts of polyol, and 2.0-5.0 parts of a substance containing both hydroxyl and carboxyl groups.
[0026] The specific preparation steps of the modified iron oxide pigment are:
[0027] a) dispersing 10 parts of iron oxide pigment into 50 parts of water, adding 100 parts of DMF to disperse evenly, and then adding 10 parts of DMF solution containing 0.1-0.3 parts of polyacid to mix and disperse; reacting at 120-140° C. for 8-10 hours, cooling, filtering, washing and drying to obtain iron oxide pigment containing polyacid;
[0028] b) 10 parts of iron oxide pigment containing polyacid, 0.2-0.6 parts of polyol, 0.1-0.2 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 70-90° C. and reacted for 2-4 hours; then 2.0-5.0 parts of a substance containing both hydroxyl and carboxyl groups are added, the reaction is continued for 2-4 hours, cooled, filtered, washed and dried to obtain a modified iron oxide pigment.
[0029] Wherein, the iron oxide pigment is at least one of iron oxide red pigment, iron oxide yellow pigment and iron oxide black pigment.
[0030] Wherein, the moisturizing agent is at least one of polyethylene glycol, glycerol, ethylene glycol, propylene glycol, n-propanol, n-butanol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, triethylene glycol, and tetraethylene glycol.
[0031] The defoaming agent is at least one of polyether, polysiloxane and polyether-modified silicone, and is preferably a polyether-modified silicone defoaming agent.
[0032] Wherein, the mildew-proofing and fungicide is 1,2-benzisothiazolin-3-one.
[0033] Another aspect of the present invention provides a method for preparing an iron oxide pigment dispersion, wherein a moisturizer, a defoamer, and an antifungal bactericide are added to water and dispersed evenly, and then a modified iron oxide pigment is added and dispersed evenly, and an alkali solution is used to adjust the pH value to 8 to 9, and then the alkali solution is ground and filtered to obtain an iron oxide pigment dispersion. The alkali solution is at least one of sodium hydroxide, potassium hydroxide, and ammonia water, preferably a sodium hydroxide solution.
[0034] The iron oxide pigment dispersion can be applied in acrylic paints.
[0035] The present invention is further described in detail below through specific examples.
[0036] Preparation of modified iron oxide pigments
[0037] Example 1
[0038] a) Iron oxide red pigment containing polyacrylic acid: 10 parts of iron oxide red pigment are dispersed in 50 parts of water, 100 parts of DMF are added to disperse evenly, and then 10 parts of DMF solution containing 0.2 parts of polyacrylic acid are added to mix and disperse; react at 130° C. for 9 hours, cool, filter, wash and dry to obtain iron oxide red pigment containing polyacrylic acid;
[0039] b) Modified iron oxide red pigment: 10 parts of iron oxide red pigment containing polyacrylic acid, 0.4 parts of pentaerythritol, and 0.2 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 80° C. and reacted for 3 hours; then 4.0 parts of 2,2-dihydroxymethylpropionic acid are added, and the reaction is continued for 4 hours, cooled, filtered, washed, and dried to obtain modified iron oxide red pigment A1.
[0040] Example 2
[0041] a) Iron oxide red pigment containing polyacrylic acid: 10 parts of iron oxide red pigment are dispersed in 50 parts of water, 100 parts of DMF are added to disperse evenly, and then 10 parts of DMF solution containing 0.1 parts of polyacrylic acid are added to mix and disperse; react at 140° C. for 8 hours, cool, filter, wash and dry to obtain iron oxide red pigment containing polyacrylic acid;
[0042] b) Modified iron oxide red pigment: 10 parts of iron oxide red pigment containing polyacrylic acid, 0.2 parts of pentaerythritol, and 0.1 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 90°C and reacted for 2 hours; then 2.0 parts of 2,2-dihydroxymethylpropionic acid are added, and the reaction is continued for 2 hours, cooled, filtered, washed, and dried to obtain modified iron oxide red pigment A2.
[0043] Example 3
[0044] a) Iron oxide red pigment containing polyacrylic acid: 10 parts of iron oxide red pigment are dispersed in 50 parts of water, 100 parts of DMF are added to disperse evenly, and then 10 parts of DMF solution containing 0.3 parts of polyacrylic acid are added to mix and disperse; react at 120° C. for 10 hours, cool, filter, wash and dry to obtain iron oxide red pigment containing polyacrylic acid;
[0045] b) Modified iron oxide red pigment: 10 parts of iron oxide red pigment containing polyacrylic acid, 0.6 parts of pentaerythritol, and 0.2 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 70° C. and reacted for 4 hours; then 5.0 parts of 2,2-dihydroxymethylpropionic acid are added, and the reaction is continued for 4 hours, cooled, filtered, washed, and dried to obtain modified iron oxide red pigment A3.
[0046] Example 4
[0047] a) Iron oxide red pigment containing polyacrylic acid: 10 parts of iron oxide red pigment are dispersed in 50 parts of water, 100 parts of DMF are added to disperse evenly, and then 10 parts of DMF solution containing 0.2 parts of polyacrylic acid are added to mix and disperse; react at 140° C. for 9 hours, cool, filter, wash and dry to obtain iron oxide red pigment containing polyacrylic acid;
[0048] b) Modified iron oxide red pigment: 10 parts of iron oxide red pigment containing polyacrylic acid, 0.4 parts of pentaerythritol, and 0.15 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 85° C. and reacted for 3 hours; then 3.5 parts of 2,2-dihydroxymethylpropionic acid are added, and the reaction is continued for 3 hours, cooled, filtered, washed, and dried to obtain modified iron oxide red pigment A4.
[0049] Comparative Example 1
[0050] Iron oxide red pigment containing polyacrylic acid: 10 parts of iron oxide red pigment are dispersed in 50 parts of water, 100 parts of DMF are added to disperse evenly, and then 10 parts of DMF solution containing 0.2 parts of polyacrylic acid are added to mix and disperse; react at 130° C. for 9 hours, cool, filter, wash and dry to obtain iron oxide red pigment B1 containing polyacrylic acid.
[0051] Comparative Example 2
[0052] a) Red iron oxide pigment containing polyacrylic acid: 10 parts of red iron oxide pigment are dispersed in 50 parts of water, 100 parts of DMF are added to disperse evenly, and then 10 parts of DMF solution containing 0.2 parts of polyacrylic acid are added to mix and disperse; react at 130° C. for 9 hours, cool, filter, wash and dry to obtain red iron oxide pigment containing polyacrylic acid;
[0053] b) Modified iron oxide red pigment: 10 parts of iron oxide red pigment containing polyacrylic acid, 0.4 parts of pentaerythritol, and 0.2 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 80° C. for reaction for 3 hours, cooled, filtered, washed, and dried to obtain modified iron oxide red pigment B2.
[0054] Comparative Example 3
[0055] a) Iron oxide red pigment containing polyacrylic acid: 10 parts of iron oxide red pigment are dispersed in 50 parts of water, 100 parts of DMF are added to disperse evenly, and then 10 parts of DMF solution containing 0.05 parts of polyacrylic acid are added to mix and disperse; react at 130° C. for 9 hours, cool, filter, wash and dry to obtain iron oxide red pigment containing polyacrylic acid;
[0056] b) Modified iron oxide red pigment: 10 parts of iron oxide red pigment containing polyacrylic acid, 0.4 parts of pentaerythritol, and 0.2 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 80°C and reacted for 3 hours; then 4.0 parts of 2,2-dihydroxymethylpropionic acid are added, and the reaction is continued for 4 hours, cooled, filtered, washed, and dried to obtain modified iron oxide red pigment B3.
[0057] Comparative Example 4
[0058] a) Iron oxide red pigment containing polyacrylic acid: 10 parts of iron oxide red pigment are dispersed in 50 parts of water, 100 parts of DMF are added to disperse evenly, and then 10 parts of DMF solution containing 0.2 parts of polyacrylic acid are added to mix and disperse; react at 130° C. for 9 hours, cool, filter, wash and dry to obtain iron oxide red pigment containing polyacrylic acid;
[0059] b) Modified iron oxide red pigment: 10 parts of iron oxide red pigment containing polyacrylic acid, 0.1 parts of pentaerythritol, and 0.2 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 80°C and reacted for 3 hours; then 4.0 parts of 2,2-dihydroxymethylpropionic acid are added, and the reaction is continued for 4 hours, cooled, filtered, washed, and dried to obtain modified iron oxide red pigment B4.
[0060] Comparative Example 5
[0061] a) Iron oxide red pigment containing polyacrylic acid: 10 parts of iron oxide red pigment are dispersed in 50 parts of water, 100 parts of DMF are added to disperse evenly, and then 10 parts of DMF solution containing 0.2 parts of polyacrylic acid are added to mix and disperse; react at 130° C. for 9 hours, cool, filter, wash and dry to obtain iron oxide red pigment containing polyacrylic acid;
[0062] b) Modified iron oxide red pigment: 10 parts of iron oxide red pigment containing polyacrylic acid, 0.4 parts of pentaerythritol, and 0.2 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 80°C and reacted for 3 hours; then 1.0 parts of 2,2-dihydroxymethylpropionic acid are added, and the reaction is continued for 4 hours, cooled, filtered, washed, and dried to obtain modified iron oxide red pigment B5.
[0063] Preparation and testing of iron oxide pigment dispersions
[0064] According to the mass parts of each component in Table 1, polyethylene glycol 300, polyether modified silicone defoamer, and 1,2-benzisothiazolin-3-one were added to water and dispersed evenly, and then iron oxide pigment was added and dispersed evenly, and the pH value was adjusted to 8-9 with sodium hydroxide, and then ground and filtered to obtain an iron oxide pigment dispersion. Among them, the iron oxide pigment B6 is a commercially available iron oxide pigment red, which is untreated.
[0065] Table 1. Composition of iron oxide pigment dispersions No. 1 to 10
[0066]
[0067] Test method:
[0068] Fineness: Refer to standard GB / T1724-2019 "Determination of grinding fineness of paints, varnishes and printing inks" to test the fineness of iron oxide pigment dispersion.
[0069] Relative tinting strength: refer to the instrumental method in Appendix B of standard HG / T3951-2007 "Water-based colorants for architectural coatings" to test relative tinting strength.
[0070] Color difference ΔE: Refer to the instrumental method in Appendix A of standard HG / T3951-2007 "Water-based color paste for architectural coatings" to test the color ΔE of the dry film.
[0071] The prepared iron oxide pigment dispersions No. 1 to No. 10 were tested for fineness, relative tinting strength and color difference ΔE; the color paste was tested for fineness, relative tinting strength and color difference ΔE after 7 days of heat storage at 50°C. When testing the relative tinting strength and color difference ΔE, the No. 1 iron oxide pigment dispersion was used as the standard dispersion, and the mass ratio of transparent iron oxide pigment to acrylic paint in the transparent iron oxide pigment dispersion was 0.5:25. The test results are shown in Table 2.
[0072] Table 2. Iron oxide pigment dispersion performance test results
[0073]
[0074] It can be seen from Table 2 that the fineness of the iron oxide pigment dispersions No. 1 to 4 is relatively small, all of which are 5 μm, and the relative tinting strength is relatively high, at 99% to 103%, and the color difference ΔE ≤ 0.12; the fineness, relative tinting strength and color difference ΔE after heat storage at 50°C for 7 days do not change much, indicating that the iron oxide pigment dispersion prepared by the present invention has good stability.
[0075] Iron oxide pigment dispersion No. 5 did not use pentaerythritol and 2,2-dimethylolpropionic acid to modify the iron oxide pigment. Only polyacrylic acid was grafted on the surface. There was no large steric hindrance on the surface and it could not be stably dispersed in water. Iron oxide pigment dispersion No. 6 did not use 2,2-dimethylolpropionic acid to modify the iron oxide pigment. There was no large steric hindrance on the surface and it could not be stably dispersed in water. The amount of polyacrylic acid added to iron oxide pigment dispersion No. 7 was too small. The carboxyl groups mostly reacted with the hydroxyl groups on the surface of the iron oxide pigment and rarely reacted with pentaerythritol. The amount of pentaerythritol grafted was too small, and the steric hindrance effect was not obvious. The amount of pentaerythritol added to iron oxide pigment dispersion No. 8 was too small. The hydroxyl groups of pentaerythritol mostly reacted with the carboxyl groups of polypropionic acid and rarely reacted with 2,2-dimethylolpropionic acid. The steric hindrance effect was not obvious. The amount of 2,2-dimethylolpropionic acid added to iron oxide pigment dispersion No. 9 was too small. The hyperbranching reaction did not occur sufficiently, and the steric hindrance effect was not obvious. The iron oxide pigments No. 5 to 9 have a larger fineness of dispersion, a lower relative tinting strength, and a larger color difference ΔE; especially the performance is worse after hot storage.
[0076] The No. 10 iron oxide pigment dispersion is a commercially available iron oxide pigment that has not been modified. After hot storage, the iron oxide pigment dispersion exhibits phenomena such as stratification, sedimentation, and flocculation.
[0077] Evaluation of the application performance of iron oxide pigment dispersion
[0078] The iron oxide pigment dispersions No. 1 to No. 10 were mixed with acrylic paint to obtain a paint, wherein the mass ratio of the iron oxide pigment to the acrylic paint in the iron oxide pigment dispersion was 0.5:25. The paint was shaken at 680 times / min for 8 minutes, and the relative tinting strength and color difference ΔE were tested; the paint was heat stored at 50°C for 7 days, and the relative tinting strength and color difference ΔE were tested. The test results are shown in Table 3.
[0079] Table 3. Coating performance test results
[0080]
[0081] It can be seen from Table 3 that: by comparison, it can be seen that the iron oxide pigment dispersion prepared by the present invention has good compatibility with acrylic paint, the relative tinting strength of the paint after oscillation and heat storage is strong, and the color difference ΔE is low.
[0082] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0083] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An iron oxide pigment dispersion, characterized in that: Calculated by weight, every 100 parts of iron oxide pigment dispersion contains 40 to 55 parts of modified iron oxide pigment, 2 to 5 parts of moisturizer, 0.1 to 0.5 parts of defoamer, 0.01 to 0.05 parts of mildew and fungicide, and the balance is water; wherein the modified iron oxide pigment is obtained by reacting the iron oxide pigment with a polyacid, a polyol, and a substance containing both hydroxyl and carboxyl groups in sequence.
2. The iron oxide pigment dispersion according to claim 1, characterized in that The polyacid is one of polyacrylic acid, polymethacrylic acid, terephthalic acid, isophthalic acid, succinic acid, glutaric acid, and adipic acid; the polyol is one of pentaerythritol, glycerol, ethylene glycol, propylene glycol, butylene glycol, pentanediol, and hexanediol; the substance containing both hydroxyl and carboxyl groups is one of 2,2-dihydroxymethylpropionic acid, 2-hydroxyhexanoic acid, 3-hydroxyhexanoic acid, 9-hydroxynonanoic acid, p-hydroxybenzoic acid, o-hydroxybenzoic acid, m-hydroxybenzoic acid, 2,3-dihydroxybenzoic acid, 3,5-dihydroxybenzoic acid, 2,6-dihydroxybenzoic acid, 3,4,5-trihydroxybenzoic acid, and 2,4,6-trihydroxybenzoic acid.
3. The iron oxide pigment dispersion according to claim 1, characterized in that The modified iron oxide pigment is obtained by reacting 10 parts of iron oxide pigment with 0.1-0.3 parts of polyacid, 0.2-0.6 parts of polyol and 2.0-5.0 parts of a substance containing both hydroxyl and carboxyl groups.
4. The iron oxide pigment dispersion according to claim 3, characterized in that The preparation steps of the modified iron oxide pigment are: a) dispersing 10 parts of iron oxide pigment into 50 parts of water, adding 100 parts of DMF to disperse evenly, and then adding 10 parts of DMF solution containing 0.1-0.3 parts of polyacid to mix and disperse; reacting at 120-140° C. for 8-10 hours, cooling, filtering, washing and drying to obtain iron oxide pigment containing polyacid; b) 10 parts of iron oxide pigment containing polyacid, 0.2-0.6 parts of polyol, 0.1-0.2 parts of n-butyl titanate catalyst are added to 100 parts of xylene, heated to 70-90° C. and reacted for 2-4 hours; then 2.0-5.0 parts of a substance containing both hydroxyl and carboxyl groups are added, the reaction is continued for 2-4 hours, cooled, filtered, washed and dried to obtain a modified iron oxide pigment.
5. The iron oxide pigment dispersion according to claim 1 or 2, characterized in that The iron oxide pigment is at least one of iron oxide red pigment, iron oxide yellow pigment and iron oxide black pigment.
6. The iron oxide pigment dispersion according to claim 1, characterized in that The moisturizing agent is at least one of polyethylene glycol, glycerol, ethylene glycol, propylene glycol, n-propanol, n-butanol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, triethylene glycol, and tetraethylene glycol.
7. The iron oxide pigment dispersion according to claim 1, characterized in that The defoaming agent is at least one of polyethers, polysiloxanes and polyether-modified silicones.
8. The iron oxide pigment dispersion according to claim 1, characterized in that The mildew-proofing and fungicide is 1,2-benzisothiazolin-3-one.
9. A method for preparing the iron oxide pigment dispersion according to any one of claims 1 to 8, characterized in that: The moisturizer, defoamer and mildew and fungicide are added into water and dispersed evenly, and then the modified iron oxide pigment is added and dispersed evenly, and the pH value is adjusted to 8-9 with alkaline solution, and then ground and filtered to obtain the iron oxide pigment dispersion.
10. Use of the iron oxide pigment dispersion according to any one of claims 1 to 8 in acrylic paint.