Single-component recyclable solvent high-efficiency thermal transfer ribbon back coating glue and preparation process thereof
By using a combination of silicone resin with acrylic copolymer and toluene in the thermal transfer carbon tape back coating, the problems of static electricity and dust adsorption under friction are solved, and more efficient heat conduction and lubrication are achieved. Reduces cost and environmental impact and improves print quality.
Patent Information
- Application Number
- CN202411236026.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The glue on the back of the traditional thermal transfer carbon belt produces static electricity under the action of friction, adsorbing external dust, resulting in wear and unevenness of the print head, affecting the printing quality.
The high-efficiency thermal transfer carbon tape back coated with a single component recyclable solvent, including silicone resin, acrylic copolymer and toluene, is stirred by pretreatment of silicone resin, acrylic copolymer solution and solvent toluene. Form a heat-resistant coating material to reduce static electricity and enhance heat conduction.
Effectively reduces static electricity generation and printhead wear, reduces unit area usage, reduces VOC emissions and solvent usage by 99%, reduces production costs, and improves printing efficiency and quality.
Smart Images

Figure CN119039882A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal transfer carbon ribbon back coating adhesive, in particular to a single-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive and a preparation process thereof. Background Art
[0002] Back-coated adhesive is a material coated with an adhesive, which is usually composed of ingredients such as butyl rubber or silicone. Back-coated adhesive is widely used in printing, packaging and labeling. It can be used to make various labels, trademarks, posters, books, magazines and other products.
[0003] The back coating of thermal transfer ribbon mainly plays the following important roles: Reduce print head wear: The back coating can serve as a buffer layer between the print head and the ribbon to reduce direct friction, thereby extending the service life of the print head and reducing maintenance costs; Reduce static electricity generation: The ribbon is prone to static electricity during high-speed operation and heating. The back coating has certain anti-static properties, which can effectively reduce static electricity accumulation, avoid problems such as skipping and static electricity adsorption of dust during printing, and ensure print quality; Enhance heat conduction: Optimize heat transfer to ensure that the heat generated by the print head can be more evenly and effectively transferred to the ink layer of the ribbon, helping the ink to be more stable and Transfer to the print medium more quickly, thereby improving printing efficiency and quality; Improve ribbon stability: Enhance the overall structural stability of the ribbon to prevent twisting or deformation during printing, and ensure the continuity and accuracy of printing; Protect printing materials: The back coating can prevent the print head from directly contacting the print medium, reducing the damage that may be caused by high temperature directly acting on the medium, which is especially important for sensitive or fragile printing materials; Moisture-proof and dust-proof: Form a protective barrier to block moisture and particles from entering the interior of the ribbon, protect the ink layer from the external environment, maintain the ribbon in good condition, and ensure the long-term stability of the printing effect.
[0004] The preparation components of the back coating adhesive of thermal transfer carbon ribbon on the market are: silicone resin SP-6068N: 8.1%, silicone resin SP-8022T: 4.2%, solvent toluene: 28.6%, solvent butanone: 44.2% and solvent ethyl acetate: 14.9%
[0005] However, the traditional thermal transfer ribbon back coating has the following disadvantages:
[0006] During the printing process of traditional thermal transfer carbon ribbon with back coating, static electricity is generated under the action of friction. The static electricity absorbs dust in the external environment, increases the unevenness of the printed body itself, and the print head is prone to wear after continued friction. Summary of the invention
[0007] The purpose of the present invention is to provide a single-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive and a preparation process, so as to solve the problem raised in the above background technology that during the printing process of the traditional thermal transfer carbon ribbon back coating adhesive, static electricity is generated under the action of friction, and the static electricity absorbs dust in the external environment, thereby increasing the unevenness of the printed body itself, and the print head is prone to wear after continued friction.
[0008] To achieve the above purpose, the present invention provides the following technical solution: a single-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive, comprising the following components, by weight percentage: silicone resin and acrylic copolymer: 7%-10% and solvent toluene: 89%-93%.
[0009] As a preferred technical solution of the present invention, by weight percentage, the organic silicon resin and acrylic acid copolymer: 9.6% and the solvent toluene: 90.4%.
[0010] As a preferred technical solution of the present invention, by weight percentage, the organic silicon resin and acrylic acid copolymer: 8% and the solvent toluene: 92%.
[0011] As a preferred technical solution of the present invention, by weight percentage, the organic silicon resin and acrylic acid copolymer: 9% and the solvent toluene: 91%.
[0012] As a preferred technical solution of the present invention, by weight percentage, the organic silicon resin and acrylic acid copolymer: 8.5% and the solvent toluene: 91.5%.
[0013] The preparation process of the single-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive of the present invention comprises the following steps:
[0014] Step 1, preparing a solution: preparing a solution of a silicone resin and an acrylic acid copolymer;
[0015] Step 2, solution pretreatment: pretreating the solvent toluene;
[0016] Step 3, solution mixing: 7%-10% of the prepared silicone resin and acrylic copolymer solution and 89%-93% of the pre-treated solvent toluene are stirred for 4-6 hours to obtain a finished product of the heat-resistant coating material of the thermal transfer carbon ribbon.
[0017] As a preferred technical solution of the present invention, the preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically as follows: S1, preparing the silicone resin: preparing a silicone resin with hydroxyl, amino, alkoxy or epoxy groups; S2, preparing the solution: utilizing these active groups to react with the functional groups on the acrylate, thereby bonding the silicone component to the acrylic resin molecule.
[0018] As a preferred technical solution of the present invention, the preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically carried out by copolymerizing the unsaturated group or the active group of hydrogen-containing siloxane with the acrylate monomer.
[0019] As a preferred technical solution of the present invention, the pretreatment in step 2 is specifically to use an ultrasonic instrument to perform ultrasonic treatment for 1-3 hours.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The back coating of the thermal transfer ribbon reduces static electricity generation and enhances heat conduction and lubrication during printing, reducing print head wear;
[0022] 2. A new type of silicone resin and acrylic copolymer was used to replace the original silicone resin mixture;
[0023] 3. Use single-component solvent toluene to replace the original multi-component mixed solvent, so that the solvent can be safely recycled;
[0024] 4. Under the same function as the back coating of carbon ribbon, the patented formula product reduces the usage per unit area by 1 / 3 compared with the existing products, thus reducing the cost;
[0025] 5. Use single-component solvent toluene to replace multi-component mixed solvents, so that the solvent can be safely recycled, reducing 99% of VOC emissions during product production and protecting the environment;
[0026] 6. The safe recycling of the single-component solvent toluene reduces the use of solvent by 99% and reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the structure of the back-coated adhesive of the thermal transfer carbon ribbon of the present invention;
[0028] Figure 2 is a flow chart of the present invention;
[0029] Figure 3 The present invention is a flow chart for preparing a solution of a silicone resin and an acrylic acid copolymer. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Embodiment 1:
[0032] See also Figure 1-3 The invention provides a single-component solvent-recyclable high-efficiency thermal transfer carbon belt back coating adhesive, which comprises the following components, calculated by weight percentage: organic silicon resin and acrylic copolymer: 7%-10% and solvent toluene: 89%-93%.
[0033] The preparation process of the single-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive of the present invention comprises the following steps:
[0034] Step 1, preparing a solution: preparing a solution of a silicone resin and an acrylic acid copolymer;
[0035] Step 2, solution pretreatment: pretreating the solvent toluene;
[0036] Step 3, solution mixing: 7%-10% of the prepared silicone resin and acrylic copolymer solution and 89%-93% of the pre-treated solvent toluene are stirred for 4-6 hours to obtain a finished product of the heat-resistant coating material of the thermal transfer carbon ribbon.
[0037] The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically as follows: S1, preparing silicone resin: preparing silicone resin with hydroxyl, amino, alkoxy or epoxy groups; S2, preparing solution: using these active groups to react with the functional groups on the acrylate, thereby bonding the silicone component to the acrylic resin molecule.
[0038] The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically carried out by copolymerizing the unsaturated group or the active group of hydrogen-containing siloxane with the acrylate monomer.
[0039] The pretreatment in step 2 specifically includes using an ultrasonic instrument to perform ultrasonic treatment for 1-3 hours.
[0040] Embodiment 2:
[0041] See also Figure 1-3 The invention provides a single-component solvent-recyclable high-efficiency thermal transfer carbon belt back coating adhesive, which comprises the following components, calculated by weight percentage: 9.6% of organic silicon resin and acrylic copolymer and 90.4% of solvent toluene.
[0042] The preparation process of the single-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive of the present invention comprises the following steps:
[0043] Step 1, preparing a solution: preparing a solution of a silicone resin and an acrylic acid copolymer;
[0044] Step 2, solution pretreatment: pretreating the solvent toluene;
[0045] Step 3, solution mixing: 9.6% of the prepared silicone resin and acrylic copolymer solution and 90.4% of the pre-treated solvent toluene are stirred for 4-6 hours to obtain a finished product of the heat-resistant coating material of the thermal transfer carbon ribbon.
[0046] The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically as follows: S1, preparing silicone resin: preparing silicone resin with hydroxyl, amino, alkoxy or epoxy groups; S2, preparing solution: using these active groups to react with the functional groups on the acrylate, thereby bonding the silicone component to the acrylic resin molecule.
[0047] The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically carried out by copolymerizing the unsaturated group or the active group of hydrogen-containing siloxane with the acrylate monomer.
[0048] The pretreatment in step 2 specifically includes using an ultrasonic instrument to perform ultrasonic treatment for 1-3 hours.
[0049] Embodiment 3:
[0050] See also Figure 1-3 The invention provides a single-component solvent-recyclable high-efficiency thermal transfer carbon belt back coating adhesive, which comprises the following components, calculated by weight percentage: 8% of organic silicon resin and acrylic acid copolymer and 92% of solvent toluene.
[0051] The preparation process of the single-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive of the present invention comprises the following steps:
[0052] Step 1, preparing a solution: preparing a solution of a silicone resin and an acrylic acid copolymer;
[0053] Step 2, solution pretreatment: pretreating the solvent toluene;
[0054] Step 3, solution mixing: 8% of the prepared silicone resin and acrylic copolymer solution and 92% of the pre-treated solvent toluene are stirred for 4-6 hours to obtain a finished product of the heat-resistant coating material of the thermal transfer carbon ribbon.
[0055] The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically as follows: S1, preparing silicone resin: preparing silicone resin with hydroxyl, amino, alkoxy or epoxy groups; S2, preparing solution: using these active groups to react with the functional groups on the acrylate, thereby bonding the silicone component to the acrylic resin molecule.
[0056] The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically carried out by copolymerizing the unsaturated group or the active group of hydrogen-containing siloxane with the acrylate monomer.
[0057] The pretreatment in step 2 specifically includes using an ultrasonic instrument to perform ultrasonic treatment for 1-3 hours.
[0058] Embodiment 4:
[0059] See also Figure 1-3 The invention provides a single-component recyclable solvent high-efficiency thermal transfer carbon belt back coating adhesive, which comprises the following components, calculated by weight percentage, 9% of organic silicon resin and acrylic acid copolymer and 91% of solvent toluene.
[0060] The preparation process of the single-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive of the present invention comprises the following steps:
[0061] Step 1, preparing a solution: preparing a solution of a silicone resin and an acrylic acid copolymer;
[0062] Step 2, solution pretreatment: pretreating the solvent toluene;
[0063] Step 3, solution mixing: 9% of the prepared silicone resin and acrylic copolymer solution and 91% of the pre-treated solvent toluene are stirred for 4-6 hours to obtain a finished product of the heat-resistant coating material of the thermal transfer carbon ribbon.
[0064] The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically as follows: S1, preparing silicone resin: preparing silicone resin with hydroxyl, amino, alkoxy or epoxy groups; S2, preparing solution: using these active groups to react with the functional groups on the acrylate, thereby bonding the silicone component to the acrylic resin molecule.
[0065] The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically carried out by copolymerizing the unsaturated group or the active group of hydrogen-containing siloxane with the acrylate monomer.
[0066] The pretreatment in step 2 specifically includes using an ultrasonic instrument to perform ultrasonic treatment for 1-3 hours.
[0067] Embodiment 5:
[0068] See also Figure 1-3 The invention provides a single-component recyclable solvent high-efficiency thermal transfer carbon belt back coating adhesive, which comprises the following components, calculated by weight percentage, 8.5% of organic silicon resin and acrylic acid copolymer and 91.5% of solvent toluene.
[0069] The preparation process of the single-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive of the present invention comprises the following steps:
[0070] Step 1, preparing a solution: preparing a solution of a silicone resin and an acrylic acid copolymer;
[0071] Step 2, solution pretreatment: pretreating the solvent toluene;
[0072] Step 3, solution mixing: 8.5% of the prepared silicone resin and acrylic copolymer solution and 91.5% of the pre-treated solvent toluene are stirred for 4-6 hours to obtain a finished product of the heat-resistant coating material of the thermal transfer carbon ribbon.
[0073] The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically as follows: S1, preparing silicone resin: preparing silicone resin with hydroxyl, amino, alkoxy or epoxy groups; S2, preparing solution: using these active groups to react with the functional groups on the acrylate, thereby bonding the silicone component to the acrylic resin molecule.
[0074] The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically carried out by copolymerizing the unsaturated group or the active group of hydrogen-containing siloxane with the acrylate monomer.
[0075] The pretreatment in step 2 specifically includes using an ultrasonic instrument to perform ultrasonic treatment for 1-3 hours.
[0076] In the present invention, a silicone resin with a hydroxyl group, an amino group, an alkoxy group or an epoxy group is prepared; these active groups are used to react with functional groups on acrylates, thereby bonding the silicone component to acrylic resin molecules to prepare a silicone resin and acrylic copolymer solution, pre-treating the solvent toluene, performing ultrasonic treatment for 1-3 hours using an ultrasonic instrument, stirring 9.6% of the prepared silicone resin and acrylic copolymer solution with 90.4% of the pre-treated solvent toluene for 4-6 hours, and obtaining a finished product of a heat-resistant coating material for a thermal transfer carbon ribbon.
[0077] In the present invention, an organic silicone resin and acrylic copolymer solution is prepared by copolymerizing an unsaturated group or an active group of hydrogenated siloxane with an acrylate monomer, the solvent toluene is pretreated, and an ultrasonic instrument is used to perform ultrasonic treatment for 1-3 hours, and 9.6% of the prepared organic silicone resin and acrylic copolymer solution and 90.4% of the pretreated solvent toluene are stirred for 4-6 hours to obtain a finished product of a heat-resistant coating material for a thermal transfer carbon ribbon.
[0078] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. The single-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive comprises the following components, calculated by weight percentage: organic silicon resin and acrylic copolymer: 7%-10% and solvent toluene: 89%-93%.
2. The one-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive according to claim 1, characterized in that: By weight percentage, the silicone resin and acrylic acid copolymer: 9.6% and the solvent toluene: 90.4%.
3. The one-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive according to claim 1, characterized in that: By weight percentage, organic silicon resin and acrylic acid copolymer: 8% and solvent toluene: 92%.
4. The one-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive according to claim 1, characterized in that: By weight percentage, silicone resin and acrylic acid copolymer: 9% and solvent toluene: 91%.
5. The one-component recyclable solvent high-efficiency thermal transfer carbon ribbon back coating adhesive according to claim 1, characterized in that: By weight percentage, organic silicon resin and acrylic acid copolymer: 8.5% and solvent toluene: 91.5%.
6. The process for preparing the one-component recyclable solvent efficient thermal transfer carbon ribbon back coating adhesive according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1, preparing a solution: preparing a solution of a silicone resin and an acrylic acid copolymer; Step 2, solution pretreatment: pretreating the solvent toluene; Step 3, solution mixing: 7%-10% of the prepared silicone resin and acrylic copolymer solution and 89%-93% of the pre-treated solvent toluene are stirred for 4-6 hours to obtain a finished product of the heat-resistant coating material of the thermal transfer carbon ribbon.
7. The process for preparing the one-component recyclable solvent efficient thermal transfer carbon ribbon back coating adhesive according to claim 6, characterized in that: The step 1 of preparing the organic silicone resin and acrylic copolymer solution specifically comprises S1, preparing an organic silicone resin: preparing an organic silicone resin with hydroxyl, amino, alkoxy or epoxy groups; S2, preparing a solution: utilizing these active groups to react with the functional groups on the acrylate, thereby bonding the organic silicone component to the acrylic resin molecule.
8. The process for preparing the one-component recyclable solvent efficient thermal transfer carbon ribbon back coating adhesive according to claim 6, characterized in that: The preparation of the silicone resin and acrylic copolymer solution in step 1 is specifically carried out by copolymerizing the unsaturated group or the active group of hydrogen-containing siloxane with the acrylate monomer.
9. The process for preparing the one-component recyclable solvent efficient thermal transfer carbon ribbon back coating adhesive according to claim 6, characterized in that: The pretreatment in step 2 specifically includes using an ultrasonic instrument to perform ultrasonic treatment for 1-3 hours.
Citation Information
Patent Citations
Resin for bar code thermal transfer ribbon back coating and preparation method thereof as well as bar code thermal transfer ribbon back coating liquid and application thereof
CN107903364A
Organosilicon-modified acrylate emulsion and preparation method thereof, heat transfer printing back coating liquid, heat transfer printing carbon ribbon back coating and carbon ribbon
CN110294817A
Back coating material for heat transfer printing bar code thermal transfer ribbon and preparation method and application thereof
CN111253524A
Heat-resistant back coating material for thermal transfer ribbon as well as preparation method and application of heat-resistant back coating material
CN113199884A
Preparation method of acrylate modified organosilicon polymer and application of acrylate modified organosilicon polymer in thermal transfer ribbon
CN114656601A