Yellowing-resistant transparent TPU color-changing film and preparation method thereof

By combining the design of PET gloss protective film, vinyl protective film, cast-grade polyurethane color film and polyvinyl chloride film, the problem of existing color change films being prone to yellowing is solved, and the yellowing resistance and transparency are improved. It is suitable for Invisible car clothing market in the automotive beauty industry.

CN119039895AInactive Publication Date: 2024-11-29JIANGSU YAOSHENG NEW MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411011373.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing cast-grade PVC color-changing films are prone to yellowing and aging during use, resulting in poor yellowing resistance and cannot meet the demand for transparent color-changing films in the automotive beauty industry.

Method used

The yellow-resistant transparent TPU color-changing film consisting of PET gloss protective film, vinyl protective film, cast-grade polyurethane color film, polyvinyl chloride film and high-performance low-primary viscosity acrylic backing glue is adopted. Through specific raw material ratios and process steps, Including coating, baking, fusion stacking and composite treatment, a color-changing film with excellent yellowing resistance and transparency characteristics were prepared.

Benefits of technology

It achieves excellent yellowing resistance and transparency of the TPU color change film, extends the service life, avoids photooxidation reaction, improves UV resistance and transparency, and significantly improves the yellowing resistance of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039895A_ABST
    Figure CN119039895A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of color changing films, and provides an anti-yellowing transparent TPU color changing film and a preparation method thereof. The TPU color changing film is formed by polymerizing a PET (Polyethylene Terephthalate) gloss protective film, a vinyl protective film, a casting-grade polyurethane color film, a polyvinyl chloride film, a high-performance low-initial-viscosity acrylic acid back adhesive and a release bottom film in sequence from top to bottom, wherein the casting-grade polyurethane color film is prepared from the following raw materials in parts by weight: 50-70 parts of TPU thermoplastic polyurethane resin, 15-40 parts of PC plastic polycarbonate, 5-10 parts of pigment, 2-5 parts of ultraviolet light absorber, 1-5 parts of antioxidant stabilizer, 1-8 parts of bi-component epoxy adhesive and 3-10 parts of filler. PC plastic is added in the preparation of the yellowing-resistant transparent TPU color-changing film, so that the yellowing-resistant transparent TPU color-changing film has excellent ultraviolet resistance and transparency, and TPU thermoplastic polyurethane resin is prevented from being subjected to photooxidation reaction; the ultraviolet light absorber is added, so that the ultraviolet resistance can be further improved, and a dual-protection effect is achieved; the TPU color-changing film has the advantages of excellent yellowing resistance and transparency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of color-changing films, and in particular relates to a yellowing-resistant transparent TPU color-changing film and a preparation method thereof. Background Art

[0002] With the continuous development of my country's economy and the continuous improvement of people's living standards, people's consumption concepts and consumption levels have also changed and improved greatly. With this opportunity, my country's automotive aftermarket has entered a period of rapid development. As the new favorite of the automotive beauty industry, invisible car cover has been recognized by many domestic consumers. The number of cars in use and the number of new cars have brought huge potential market space for invisible car cover.

[0003] In the related prior art, for example, the Chinese invention patent application is entitled "A casting-grade PVC color-changing film and its preparation method", with the publication number CN113736190A, and the specific disclosure scheme is "The PVC color-changing film includes 100 parts of PVC resin, 40-150 parts of TPU resin, 3-15 parts of pigment, 0.2-1 parts of ultraviolet absorber, 0.4-2 parts of antioxidant stabilizer, 0.5-2 parts of dispersant, and 0-10 parts of filler according to the weight ratio." Although this color-changing film can have better physical and mechanical properties, better wear resistance and scratch resistance, and longer service life to a certain extent, it is prone to yellowing and aging, resulting in poor yellowing resistance of the product. Summary of the invention

[0004] In view of the above problems existing in the prior art, the object of the present invention is to provide a yellowing-resistant transparent TPU color-changing film and a preparation method thereof, so that the TPU color-changing film has excellent yellowing resistance and transparency advantages.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A yellowing-resistant transparent TPU color-changing film, which is composed of a PET gloss protective film, a vinyl protective film, a casting-grade polyurethane color film, a polyvinyl chloride film, a high-performance low initial viscosity acrylic backing and a release base film from top to bottom; wherein the casting-grade polyurethane color film is made according to the following raw materials in parts by weight:

[0007] 50-70 parts of TPU thermoplastic polyurethane resin, 15-40 parts of PC plastic polycarbonate, 5-10 parts of pigment, 2-5 parts of ultraviolet absorber, 1-5 parts of antioxidant stabilizer, 1-8 parts of two-component epoxy adhesive, and 3-10 parts of filler.

[0008] As a preferred technical solution of the present invention, the TPU color-changing layer is calculated according to the weight parts of the following raw materials:

[0009] 56 parts of TPU thermoplastic polyurethane resin, 26 parts of PC plastic polycarbonate, 6.5 parts of pigment, 3.5 parts of ultraviolet absorber, 2 parts of antioxidant stabilizer, 2.5 parts of two-component epoxy adhesive, and 3.5 parts of filler.

[0010] As a preferred technical solution of the present invention, the hardness of the TPU thermoplastic polyurethane resin is 35A-80A.

[0011] As a preferred technical solution of the present invention, the ultraviolet absorber includes one of 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole, or monobenzoic acid resorcinol ester.

[0012] As a preferred technical solution of the present invention, the antioxidant stabilizer is a calcium zinc stabilizer or a phosphite.

[0013] As a preferred technical solution of the present invention, the filler is at least one of calcium carbonate, silicon dioxide or titanium dioxide.

[0014] The present invention also provides a method for preparing the yellowing-resistant transparent TPU color-changing film as described above, comprising the following steps:

[0015] S1. The high-performance, low-initial-viscosity acrylic adhesive is uniformly coated on the surface of the release film, wherein the coating adhesive thickness is set to 0.2-0.5 mm; then the coated release film is placed in an oven for heating time T of 1.5-3 h, and the oven heating temperature is set to 60-120° C., so as to obtain a coating layer A;

[0016] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the release base film, the casting-grade polyurethane color film, and the polyvinyl chloride film together to obtain a fused stacking layer B;

[0017] S3, compounding the vinyl protective film and the PET gloss protective film in sequence on the surface of the fused stacking layer B obtained in step S2 to obtain a composite film C;

[0018] S4. The composite film C of step S3 is allowed to stand at a temperature of 45-80° C. for 48-96 hours, then placed in a cooling machine for cooling, and wound up using a winding device to obtain a yellowing-resistant transparent TPU color-changing film.

[0019] As a preferred technical solution of the present invention, the thickness of the coated adhesive is set to 0.3 mm, the heating time T in the oven is 2 h, and the heating temperature of the oven is set to 110°C.

[0020] The present invention relates to a yellowing-resistant transparent TPU color-changing film and a preparation method thereof, which have the following beneficial effects: the yellowing-resistant transparent TPU color-changing film of the present invention contains a casting-grade polyurethane color film and has a TPU thermoplastic polyurethane resin, which has certain yellowing-resistant properties; PC plastic polycarbonate is added during the preparation, which has excellent UV resistance and transparency, and avoids the TPU thermoplastic polyurethane resin from photo-oxidation reaction; while adding an ultraviolet absorber, the UV resistance can be further improved, and the film has a dual protective effect; in addition, the addition of a two-component epoxy adhesive can improve the transparency and also has certain yellowing resistance, thereby making the TPU color-changing film of the present invention have the advantages of excellent yellowing resistance and transparency.

[0021] The present invention will be further described below in conjunction with specific implementation modes. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic diagram of the structure of the yellowing-resistant transparent TPU color-changing film applied for by the present invention;

[0023] Figure 2 Yellowing resistance test diagram of the TPU color-changing film made in Example 3 of the present invention and comparative examples 1-3.

[0024] Reference numerals - In the drawings:

[0025] a-PET glossy protective film; b-vinyl protective film; c-casting grade polyurethane color film; d-polyvinyl chloride film; e-high performance low initial viscosity acrylic adhesive; f-release base film layer. DETAILED DESCRIPTION

[0026] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0027] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.

[0028] A yellowing-resistant transparent TPU color-changing film, which is composed of a PET gloss protective film a, a vinyl protective film b, a casting-grade polyurethane color film c, a polyvinyl chloride film d, a high-performance low initial viscosity acrylic adhesive e and a release bottom film f from top to bottom;

[0029] The casting grade polyurethane color film C is made according to the weight parts of the following raw materials:

[0030] 50-70 parts of TPU thermoplastic polyurethane resin, 15-40 parts of PC plastic polycarbonate, 5-10 parts of pigment, 2-5 parts of ultraviolet absorber, 1-5 parts of antioxidant stabilizer, 1-8 parts of two-component epoxy adhesive, 3-10 parts of filler; wherein the preparation method of casting grade polyurethane color film is batching, solvent dissolving, mixing, filtering, coating and scraping, baking, cooling and rolling; specifically: the proportion of each raw material component is as shown in the range recorded above;

[0031] Solvent dissolution: the raw materials measured according to the formula and the polyurethane solution are added into the polyurethane solution at a mass ratio of 1: (0.5-3) to dissolve;

[0032] Mixing: The above dissolved solution is stirred and mixed by a stirrer, the stirring temperature is 10-15°C, the stirring time is 30-90min, and the stirring speed is 800-1200r / min;

[0033] Filtration: The stirred and mixed solution is filtered under pressure, the filter mesh number is set at 600-1000 mesh, and the pressure is 0.5-1.8MPa;

[0034] Coating and scraping: The filtered solution is coated on the coating paper through a coating machine;

[0035] Baking: Send the coated paper into the baking room through the rubber roller, the baking temperature is 120-220℃, and the baking time is 1.5-3min.

[0036] Example 1

[0037] A yellowing-resistant transparent TPU color-changing film, which is composed of a PET gloss protective film a, a vinyl protective film b, a casting-grade polyurethane color film c, a polyvinyl chloride film d, a high-performance low initial viscosity acrylic adhesive e and a release bottom film f from top to bottom;

[0038] The casting grade polyurethane color film is made according to the following raw materials in parts by weight:

[0039] 50 parts of TPU thermoplastic polyurethane resin with a hardness of 35A, 25 parts of PC plastic polycarbonate, 5 parts of pigment, 5 parts of ultraviolet absorber, 5 parts of antioxidant stabilizer, 1 part of two-component epoxy adhesive, and 9 parts of filler; the preparation of casting-grade polyurethane color film is implemented according to the above content, which is not repeated here; wherein the ultraviolet absorber is 2,4-dihydroxybenzophenone, which is light-colored needle-shaped crystals or white powder, and the water content is 2.5-3.0.

[0040] <0.5%, ash 100 ml solvent, 25℃ acetone 50, benzene 1, ethanol>50, water <0.5, n-heptane <0.5.

[0041] The method for preparing a yellowing-resistant transparent TPU color-changing film comprises the following steps

[0042] S1, uniformly coating the high-performance, low-initial-viscosity acrylic adhesive e on the surface of the release film f, wherein the coating adhesive thickness is set to 0.2 mm; then placing the coated release film f in an oven for a heating time T of 1.5 h, and the oven heating temperature is set to 100° C., so as to obtain a coating layer A;

[0043] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the release base film f, the casting grade polyurethane color film c, and the polyvinyl chloride film d together to obtain a fused stacking layer B;

[0044] S3, compounding the vinyl protective film b and the PET gloss protective film a in sequence on the surface of the fused stacking layer B obtained in step S2 to obtain a composite film C;

[0045] S4. The composite film C of step S3 is allowed to stand at 60° C. for 48 hours, then placed in a cooling machine for cooling, and rolled up using a rolling device to obtain a yellowing-resistant transparent TPU color-changing film.

[0046] Example 2

[0047] A yellowing-resistant transparent TPU color-changing film, which is composed of a PET gloss protective film a, a vinyl protective film b, a casting-grade polyurethane color film c, a polyvinyl chloride film d, a high-performance low initial viscosity acrylic adhesive e and a release bottom film f from top to bottom;

[0048] The casting grade polyurethane color film is made according to the following raw materials in parts by weight:

[0049] 60 parts of TPU thermoplastic polyurethane resin with a hardness of 40A, 15 parts of PC plastic polycarbonate, 5 parts of pigment, 2 parts of ultraviolet absorber, 5 parts of antioxidant stabilizer, 8 parts of two-component epoxy adhesive, and 5 parts of filler; the preparation of the casting-grade polyurethane color film is implemented according to the above content, which is not repeated here; wherein the ultraviolet absorber is 2-hydroxy-4-methoxybenzophenone, which is a light yellow or white crystalline powder with a density of 1.324g / cm3 (2℃5), a melting point of 62-66℃, and a boiling point of 150-160℃

[0050] (0.67kPa), 220℃(2.4kPa), soluble in most organic solvents such as acetone, ketone, benzene, methanol, ethyl acetate, methyl ethyl ketone and ethanol, but insoluble in water; the solubility of the ultraviolet absorber in some solvents (g / 100g solvent, 25) is 56.2 in solvent benzene, 4.3 in n-hexane, 5.8 in ethanol (95%), 34.5 in carbon tetrachloride, 51.2 in styrene, and 18.7 in DOP.

[0051] The method for preparing a yellowing-resistant transparent TPU color-changing film comprises the following steps

[0052] S1, uniformly coating the high-performance, low-initial-viscosity acrylic adhesive e on the surface of the release film f, wherein the coating adhesive thickness is set to 0.25 mm; then placing the coated release film in an oven for heating time T of 1.8 h, and the oven heating temperature is set to 80° C., so as to obtain a coating layer A;

[0053] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the release base film f, the casting grade polyurethane color film c, and the polyvinyl chloride film d together to obtain a fused stacking layer B;

[0054] S3, compounding the vinyl protective film b and the PET gloss protective film a in sequence on the surface of the fused stacking layer B obtained in step S2 to obtain a composite film C;

[0055] S4. The composite film C of step S3 is allowed to stand at 50° C. for 60 hours, then placed in a cooling machine for cooling, and rolled up using a rolling device to obtain a yellowing-resistant transparent TPU color-changing film.

[0056] Example 3

[0057] A yellowing-resistant transparent TPU color-changing film, which is composed of a PET gloss protective film a, a vinyl protective film b, a casting-grade polyurethane color film c, a polyvinyl chloride film d, a high-performance low initial viscosity acrylic adhesive e and a release bottom film f from top to bottom;

[0058] The casting grade polyurethane color film is made according to the following raw materials in parts by weight:

[0059] 56 parts of TPU thermoplastic polyurethane resin with a hardness of 75A, 26 parts of PC plastic polycarbonate, 6.5 parts of pigment, 3.5 parts of ultraviolet absorber, 2 parts of antioxidant stabilizer, 2.5 parts of two-component epoxy adhesive, and 3.5 parts of filler; the preparation of casting-grade polyurethane color film is implemented according to the above content, which is not repeated here; wherein the 2-hydroxy-4-n-octyloxybenzophenone, the product is light yellow or white crystalline powder, density 1.160g / cm3 (25°C), melting point 48-49°C, soluble in acetone, benzene, ethanol, isopropanol, slightly soluble in dichloroethane, insoluble in water; the solubility of the product in some solvents (g / 100 solvent, 25°C) is 74 in solvent acetone, 72 in benzene, 2 in methanol, 2.6 in ethanol (95%), 40 in n-heptane, 40.1 in n-hexane, and 0.5 in water.

[0060] The method for preparing a yellowing-resistant transparent TPU color-changing film comprises the following steps

[0061] S1, uniformly coating the high-performance, low-initial-viscosity acrylic adhesive e on the surface of the release film f, wherein the coating adhesive thickness is set to 0.3 mm; then placing the coated release film in an oven for heating time T for 2 hours, and the oven heating temperature is set to 110° C., so as to obtain a coating layer A;

[0062] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the release base film f, the casting grade polyurethane color film c, and the polyvinyl chloride film d together to obtain a fused stacking layer B;

[0063] S3, compounding the vinyl protective film b and the PET gloss protective film a in sequence on the surface of the fused stacking layer B obtained in step S2 to obtain a composite film C;

[0064] S4. The composite film C of step S3 is allowed to stand at 70° C. for 72 hours, then placed in a cooling machine for cooling, and rolled up using a rolling device to obtain a yellowing-resistant transparent TPU color-changing film.

[0065] Example 4

[0066] A yellowing-resistant transparent TPU color-changing film, which is composed of a PET gloss protective film a, a vinyl protective film b, a casting-grade polyurethane color film c, a polyvinyl chloride film d, a high-performance low initial viscosity acrylic adhesive e and a release bottom film f from top to bottom;

[0067] The casting grade polyurethane color film is made according to the following raw materials in parts by weight:

[0068] 65 parts of TPU thermoplastic polyurethane resin with a hardness of 80A, 15 parts of PC plastic polycarbonate, 8 parts of pigment, 2 parts of ultraviolet absorber, 2 parts of antioxidant stabilizer, 5 parts of two-component epoxy adhesive, and 3 parts of filler; the preparation of casting-grade polyurethane color film is implemented according to the above content, which is not repeated here; wherein the ultraviolet absorber is selected from 2-(2'-hydroxy-3', 5'-di-tert-phenyl)-5-chlorobenzotriazole or monobenzoic acid resorcinol ester; wherein the ultraviolet absorber is selected from 2-(2'-hydroxy-3', 5'-di-tert-phenyl)-5-chlorobenzotriazole The performance parameters are that it can strongly absorb ultraviolet rays with a wavelength of 270-380nm, has good chemical stability and extremely low volatility; it has good compatibility with polyolefins, and is particularly suitable for polyethylene and polypropylene; in addition, it can also be used for polyvinyl chloride, polymethyl methacrylate, polyoxymethylene, polyurethane, unsaturated polyester, ABS resin, epoxy resin and cellulose resin, etc.; the product has excellent resistance to heat sublimation, washing resistance, gas fading resistance and mechanical property retention; it has a significant synergistic effect when used in combination with antioxidants. To improve the thermal oxygen stability of the product, the general dosage of this product in plastics is 1% to 3%.

[0069] The method for preparing a yellowing-resistant transparent TPU color-changing film comprises the following steps

[0070] S1, uniformly coating the high-performance, low-initial-viscosity acrylic adhesive e on the surface of the release film f, wherein the coating adhesive thickness is set to 0.5 mm; then placing the coated release film in an oven for heating time T for 3 hours, and the oven heating temperature is set to 120° C., so as to obtain a coating layer A;

[0071] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the release base film f, the casting grade polyurethane color film c, and the polyvinyl chloride film d together to obtain a fused stacking layer B;

[0072] S3, compounding the vinyl protective film b and the PET gloss protective film a in sequence on the surface of the fused stacking layer B obtained in step S2 to obtain a composite film C;

[0073] S4. The composite film C of step S3 is allowed to stand at 80° C. for 96 hours, then placed in a cooling machine for cooling, and rolled up using a rolling device to obtain a yellowing-resistant transparent TPU color-changing film.

[0074] It should be noted that: the antioxidant stabilizer in Examples 1-4 is a calcium zinc stabilizer or one of the phosphites; the filler is at least one of calcium carbonate, silicon dioxide or titanium dioxide.

[0075] Comparative Example 1

[0076] Different from Example 1, no TPU thermoplastic polyurethane resin is added during the preparation.

[0077] Comparative Example 2

[0078] The difference from Example 1 is that no PC plastic polycarbonate is added during the preparation.

[0079] Comparative Example 3

[0080] Different from Example 1, no two-component epoxy adhesive was added during the preparation.

[0081] Test example

[0082] Different from Example 1, no TPU thermoplastic polyurethane resin, PC plastic polycarbonate, or two-component epoxy adhesive is added during the preparation.

[0083] The PC plastic polycarbonate used in Examples 1-4 and Comparative Examples 1-3 is a transparent PC product produced by Dongguan Zhangmutou Renhong Plastic Raw Materials Business Department, which has the characteristics of transparency, UV resistance, and wear resistance; and the two-component epoxy adhesive used in Examples 1-4 and Comparative Examples 1-3 is a model YG-308AB-3 product produced by Dongguan Youguang Industrial Co., Ltd., and the performance parameters are shown in Table 1:

[0084] project parameter Viscosity(cps) 250 Mixing ratio 50(g) Curing time 55℃1.5H(2g) Available time 15min(100g) Appearance Colorless and transparent Shelf life 6 months

[0085] According to the HG / T5659-2019 standard, the standard specifies in detail the yellowing measurement method of optical functional films under simulated sunlight or ultraviolet light; Examples 1-4, Comparative Examples 1-3 and Test Examples were subjected to corresponding performance tests, in which 8 Toyota Vezel vehicles were used as examples for the test; QUV yellowing resistance test: UVA bulbs were used in the same room and Under the same conditions, the color change data was recorded after irradiation with ultraviolet light for 4 hours, and at 90 hours, 300 hours, 800 hours and 3000 hours respectively. See Table 2 for color change data:

[0086] 4h 90h 300h 800h 3000h Test example Yellowing Yellowing Yellowing Yellowing Yellowing Comparative Example 1 none Yellowing Yellowing Yellowing Yellowing Comparative Example 2 none none Yellowing Yellowing Yellowing Comparative Example 3 none none none Yellowing Yellowing Example 1 none none none none none Example 2 none none none none none Example 3 none none none none none Example 4 none none none none none

[0087] In addition, please combine Figure 1 and Figure 2 As shown, Figure 2 The yellowing test graph (TPU in Example 3, i.e., the graph, is selected, and comparative examples 1-3 are prepared). In this graph, the smaller the yellowing resistance value, the stronger the yellowing resistance performance. From the above Table 2, and Figure 1 and Figure 2It can be seen that: the TPU color-changing film embodiments 1-4 of the present invention can still remain unchanged yellow after testing for 3000 hours, and have excellent yellowing resistance. The color-changing film made using the raw material ratio of Example 3 has the best yellowing resistance effect; and each has good transparency; therefore, it has TPU thermoplastic polyurethane resin, which has certain yellowing resistance; PC plastic polycarbonate is added in the preparation, which has excellent UV resistance and transparency, and avoids photo-oxidation reaction of TPU thermoplastic polyurethane resin; at the same time, adding ultraviolet absorber can further enhance UV resistance and has dual protection; in addition, adding two-component epoxy adhesive can enhance transparency and also has certain yellowing resistance, thereby making the TPU color-changing film of the present invention have excellent yellowing resistance and transparency.

[0088] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0089] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A yellowing-resistant transparent TPU color-changing film, characterized in that: The TPU color-changing film is composed of a PET gloss protective film, a vinyl protective film, a casting-grade polyurethane color film, a polyvinyl chloride film, a high-performance low-initial viscosity acrylic adhesive and a release base film from top to bottom; wherein the casting-grade polyurethane color film is made according to the following raw materials in parts by weight: 50-70 parts of TPU thermoplastic polyurethane resin, 15-40 parts of PC plastic polycarbonate, 5-10 parts of pigment, 2-5 parts of ultraviolet absorber, 1-5 parts of antioxidant stabilizer, 1-8 parts of two-component epoxy adhesive, and 3-10 parts of filler.

2. The yellowing-resistant transparent TPU color-changing film according to claim 1, characterized in that: The TPU color-changing layer is calculated based on the weight parts of the following raw materials: 56 parts of TPU thermoplastic polyurethane resin, 26 parts of PC plastic polycarbonate, 6.5 parts of pigment, 3.5 parts of ultraviolet absorber, 2 parts of antioxidant stabilizer, 2.5 parts of two-component epoxy adhesive, and 3.5 parts of filler.

3. The yellowing-resistant transparent TPU color-changing film according to claim 2, characterized in that: The hardness of the TPU thermoplastic polyurethane resin is 35A-80A.

4. The yellowing-resistant transparent TPU color-changing film according to claim 2, characterized in that: The ultraviolet absorber includes one of 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2-(2'-hydroxy-3',5'-di-tert-phenyl)-5-chlorobenzotriazole, and monobenzoic acid resorcinol ester.

5. The yellowing-resistant transparent TPU color-changing film according to claim 2, characterized in that: The antioxidant stabilizer is a calcium zinc stabilizer or a phosphite.

6. A yellowing-resistant transparent TPU color-changing film according to any one of claims 2 to 5, characterized in that: The filler is at least one of calcium carbonate, silicon dioxide or titanium dioxide.

7. A method for preparing a yellowing-resistant transparent TPU color-changing film according to any one of claims 1 to 6, characterized in that: The following steps are included S1. The high-performance, low-initial-viscosity acrylic adhesive is uniformly coated on the surface of the release film, wherein the coating adhesive thickness is set to 0.2-0.5 mm; then the coated release film is placed in an oven for heating time T of 1.5-3 h, and the oven heating temperature is set to 60-120° C., so as to obtain a coating layer A; S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the release base film, the casting-grade polyurethane color film, and the polyvinyl chloride film together to obtain a fused stacking layer B; S3, compounding the vinyl protective film and the PET gloss protective film in sequence on the surface of the fused stacking layer B obtained in step S2 to obtain a composite film C; S4. The composite film C of step S3 is allowed to stand at a temperature of 45-80° C. for 48-96 hours, then placed in a cooling machine for cooling, and wound up using a winding device to obtain a yellowing-resistant transparent TPU color-changing film.

8. The preparation method according to claim 7, characterized in that: The thickness of the coated adhesive was set to 0.3 mm, the heating time T in the oven was 2 h, and the heating temperature of the oven was set to 110° C.

Citation Information

Patent Citations