Low-temperature plasma sintering method of calcium carbonate white fluorescent powder
By using low-temperature plasma sintering technology, argon and carbon dioxide plasma are used to bombard the powder surface to achieve uniform doping of rare earth elements, solving the problem of high-temperature sintering of calcium carbonate phosphor, improving fluorescence intensity and stability, and making it suitable for industrial production.
Patent Information
- Application Number
- CN202410974057.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The high-temperature sintering of existing calcium carbonate phosphors makes it difficult to dope rare earth elements, and they are prone to decomposition at high temperatures, affecting fluorescence intensity and stability. Traditional low-temperature methods require mechanical pressure devices, which limits the efficiency of batch preparation.
A tubular low-pressure vacuum chamber is used to bombard the powder surface with argon and carbon dioxide plasma to achieve low-temperature co-doping of rare earth ions. Low-pressure sintering is carried out through a radio frequency plasma chamber to avoid external pressure facilities. Europium, cerium and bismuth are used as activators and sensitizers to control the sintering temperature below 600℃.
Uniform doping of rare earth elements was achieved, which improved the yield and stability of phosphors, simplified the preparation process, made it suitable for industrial production, and reduced energy consumption and costs.
Smart Images

Figure CN119039980A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material preparation, and in particular relates to the preparation of white light fluorescent powder with calcium carbonate as a matrix, and a special low-temperature plasma sintering method thereof. Background Art
[0002] Fluorescent material is a material that can emit visible light of a certain color after absorbing visible light and ultraviolet light. Rare earth doped alkaline earth aluminates and silicates are the most mainstream fluorescent materials in the market. However, the luminescent color of this type of system is concentrated in the blue-green band, and mature red and white phosphors have not yet been developed. At the same time, aluminates and silicates are unstable when exposed to water, the raw materials are complex and the preparation energy consumption is high. Phosphors based on calcium carbonate provide a solution to the above problems.
[0003] Calcium carbonate has the advantages of low price, stable chemical properties, low hardness, and easy control of powder size. By doping calcium carbonate with suitable rare earth elements and replacing calcium ions with rare earth elements at high temperature using a solid phase sintering method, a three-primary color phosphor can be prepared (CN114989810A). The essence of traditional white phosphors is a mixture of these three-primary color phosphors, not a pure white light phosphor. This brings inconvenience to the practical application of such phosphors. Therefore, the preparation of monomer white light fluorescent powders by co-doping rare earth ions can promote the application of white light in the field of luminescence. According to the traditional sintering mechanism, high-temperature sintering helps the transition substitution of doped ions to form sufficient doping and luminescence centers, and co-doping with rare earth ions increases the difficulty of uniform doping. Increasing the sintering temperature helps to improve uniformity, but calcium carbonate is easy to decompose at high temperatures, so the luminescence intensity of calcium carbonate phosphors is generally not high at present. Although it is also possible to prepare a phosphor with calcium oxide as the matrix (Optics Communications, (2014) 311: 266-269.), the calcium oxide powder is easy to deliquesce and causes fluorescence decay, so the practical value is not high. For this reason, how to promote the doping of rare earth ions and keep the calcium carbonate matrix is a difficult problem in the preparation of calcium carbonate-based phosphors. In order to promote the doping of rare earth elements and suppress the decomposition of calcium carbonate, the team of Changchun Institute of Applied Chemistry used hot pressing plasma sintering technology to achieve stable phosphor preparation (CN103627399A). Hot pressing plasma sintering is to apply alternating current to the sintering object powder, break through the gas between the powder gaps to form plasma, enhance the activity of the powder, and promote the migration and doping of rare earth ions. However, this method requires a mechanical hot pressing device. In order to maintain the pressure at the MPa level, the cavity cannot be made too large, which affects the batch preparation efficiency of the powder. Summary of the invention
[0004] In order to solve the problem of existing high-efficiency sintering of calcium carbonate-based phosphors, the present invention uses a tubular low-pressure vacuum chamber to obtain plasma through argon and nitrogen glow discharge. The plasma bombards the powder surface to promote the migration doping of co-doped rare earth ions, thereby realizing low-temperature sintering of phosphors based on calcium carbonate.
[0005] The technical solution of the present invention is as follows:
[0006] A low-temperature plasma sintering method for calcium carbonate white light phosphor powder utilizes plasma atmosphere to solid-phase sinter calcium carbonate phosphor powder based on rare earth co-doping effect at low temperature without hot pressing and external pressure facilities.
[0007] Furthermore, the phosphor is sintered with calcium carbonate as a matrix, europium and cerium as activators and bismuth as a sensitizer, the molar percentage of europium doping is 1-4%, the molar percentage of cerium doping is 1-5%, and the rare earth elements are provided by rare earth oxides.
[0008] Furthermore, the white light powder includes a monomer phosphor having a cyan luminescence peak and a red luminescence powder, wherein europium doping results in a red fluorescence peak, cerium doping results in a cyan fluorescence peak, and the luminescence of the two rare earth elements is regulated by bismuth as an energy transfer center.
[0009] Powder excitation wavelength: 200-350nm, luminescence wavelength: two fluorescence peaks at 471nm cyan and 615nm red, powder particle size: 1-20μm, temperature resistance: above 400℃.
[0010] Low-pressure plasma atmosphere solid-phase sintering is used. During the sintering process, there is no need to apply external mechanical high pressure to the powder. The sintering process uses a tubular furnace with a radio frequency plasma chamber. A multi-layer sample rack made of alumina ceramic sheets is used in the chamber to place calcium carbonate doped with rare earth oxides. The powder is loose and maintains a high specific surface area.
[0011] The sintering background pressure is 10 -1 -10 -3 Pa, the working pressure is controlled at 1-500 Pa. The atmosphere used is low-activity gas such as argon and carbon dioxide; argon, as an ionized gas, contains less oxygen and water, and its role in the sintering process is to provide high-kinetic energy argon ions, and the role of carbon dioxide is to inhibit the decomposition process of the calcium carbonate matrix during the sintering process and provide sufficient gas pressure to maintain the stability of the calcium carbonate matrix.
[0012] The working atmosphere is low-activity gas and carbon dioxide, the low-activity gas is argon or nitrogen, wherein the flow rate of argon or nitrogen during sintering is controlled to be 500-1000sccm, and the flow rate of carbon dioxide is controlled to be 1000-1500sccm.
[0013] In solid phase sintering, the sintering temperature is lower than 600℃, the sintering time is 2-4 hours, the plasma source frequency is 10-20MHZ, and the power is 500-800W.
[0014] The beneficial effects of the present invention are as follows: 1. White fluorescence of the monomer powder is achieved by co-doping, and the preparation method is simple and easy. 2. Low-temperature sintering in a plasma atmosphere can effectively improve the yield of calcium carbonate phosphors, protect the calcium carbonate powder matrix from decomposition, can be industrialized, simplify the post-processing process, be environmentally friendly and efficient, and have great advantages in large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 The schematic diagram of the structure of the low-temperature plasma sintering furnace is shown in Figure 1. 1 is the RF electrode plate, 2 is the RF power supply, 3 is the plasma atmosphere, 4 is the sintering heating rack, which is made of alumina ceramic wrapped heating wire, 5 is the sintering heating power supply and temperature control equipment, 6 is the vacuum pumping pipeline, 7 is the argon and carbon dioxide filling pipeline, and 8 is the powder sample.
[0016] Figure 2 Morphology diagram of europium-doped phosphors sintered by conventional sintering and low-temperature plasma sintering under CO2 protection, where (a) is conventional sintering and (b) is low-temperature plasma sintering.
[0017] Figure 3 This is the morphology of europium-doped phosphor sintered by low-temperature plasma without CO2 protection.
[0018] Figure 4 This is the XRD pattern of low temperature plasma sintered europium-doped phosphor.
[0019] Figure 5 PL diagram of europium-doped phosphor sintered under CO2 protection.
[0020] Figure 6 This is the morphology of the europium and cerium co-doped phosphor sintered by low-temperature plasma under CO2 protection.
[0021] Figure 7 This is the XRD pattern of europium and cerium co-doped phosphor sintered by low-temperature plasma under CO2 protection.
[0022] Figure 8 PL image of europium and cerium co-doped phosphor sintered by low-temperature plasma under CO2 protection.
[0023] Fig. 9 This is the color shade of europium-cerium co-doped fluorescence sintered under CO2 protected low temperature plasma. DETAILED DESCRIPTION
[0024] In order to make the technical solutions and advantages of the present invention clearer, the technical solutions of the present invention will be described clearly and completely in conjunction with the accompanying drawings. The embodiments described here are only part of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of patent protection of the present invention.
[0025] Reference Figures 1 to 9 A low-temperature plasma sintering method for calcium carbonate white light phosphor powder utilizes a plasma atmosphere to solid-phase sinter calcium carbonate phosphor powder based on rare earth co-doping effect at low temperature without the need for hot pressing and external pressure facilities.
[0026] The phosphor is sintered with calcium carbonate as a matrix, europium and cerium as activators and bismuth as a sensitizer. The molar percentage of europium doping is 1-4%, the molar percentage of cerium doping is 1-5%, and the rare earth element is provided by rare earth oxide.
[0027] The white light powder includes a monomer phosphor having a cyan luminescence peak and a red luminescence powder, wherein europium doping leads to a red fluorescence peak, cerium doping leads to a cyan fluorescence peak, and the luminescence of the two rare earth elements is regulated by bismuth as an energy transfer center.
[0028] Powder excitation wavelength: 200-350nm, luminescence wavelength: two fluorescence peaks at 471nm cyan and 615nm red, powder particle size: 1-20μm, temperature resistance: above 400℃.
[0029] Low-pressure plasma atmosphere solid-phase sintering is used. During the sintering process, there is no need to apply external mechanical high pressure to the powder. The sintering process uses a tubular furnace with a radio frequency plasma chamber. A multi-layer sample rack made of alumina ceramic sheets is used in the chamber to place calcium carbonate doped with rare earth oxides. The powder is loose and maintains a high specific surface area.
[0030] The sintering background pressure is 10 -1 -10 -3 Pa, the working pressure is controlled at 1-500 Pa. The atmosphere used is low-activity gas such as argon and carbon dioxide; argon, as an ionized gas, contains less oxygen and water, and its role in the sintering process is to provide high-kinetic energy argon ions, and the role of carbon dioxide is to inhibit the decomposition process of the calcium carbonate matrix during the sintering process and provide sufficient gas pressure to maintain the stability of the calcium carbonate matrix.
[0031] The working atmosphere is low-activity gas and carbon dioxide, the low-activity gas is argon or nitrogen, wherein the flow rate of argon or nitrogen during sintering is controlled to be 500-1000sccm, and the flow rate of carbon dioxide is controlled to be 1000-1500sccm.
[0032] In solid phase sintering, the sintering temperature is lower than 600℃, the sintering time is 2-4 hours, the plasma source frequency is 10-20MHZ, and the power is 500-800W.
[0033] In this embodiment, the physical mechanism of energy resonance transfer between rare earth ions is utilized, and rare earths that can cause red and blue emission are co-doped and sintered. The rare earth element europium that causes red emission is 1-4% of the molar mass of the matrix calcium carbonate, and the rare earth element cerium that causes blue emission is 1-5% of the molar mass of the matrix calcium carbonate. Europium trioxide and cerium trioxide provide rare earth particles Eu 3+ and Ce 3+ , bismuth oxide provides Bi 3+ As an energy resonance transfer center,
[0034] K2CO3 or Li2CO3 is a flux and a charge compensator.
[0035] Calcium carbonate powder is solid-phase sintered in a low-pressure plasma atmosphere. A radio frequency power source is used to excite working gases such as argon or nitrogen, carbon dioxide, etc. in a low-pressure environment to generate a plasma atmosphere to activate the powder surface. Another function of carbon dioxide gas is to inhibit the decomposition of calcium carbonate to produce carbon dioxide.
[0036] The rare earth raw materials to be doped, europium trioxide, cerium trioxide and calcium carbonate powder are mixed and ground in proportion and placed in a cylindrical sintering cavity. This cavity structure with a certain symmetry is conducive to the uniform distribution of plasma. Figure 1 As shown, the sintering furnace is equipped with a vacuum system and a gas filling system. A planar electrode with a spacing of 5-10 cm is built into the sintering chamber, and the electrode is externally connected to a radio frequency power supply with a voltage of 1-5kV, a frequency of 10-20MHZ, and a power of 500-800W. A multi-layer powder rack is also placed in the chamber. The multi-layer distribution of powder increases the probability of powder particles being exposed to plasma, and plasma is used to promote the surface doping activity of particles.
[0037] The powder was placed on a multi-layer powder rack in the sintering furnace and the background vacuum of the cavity was set to 10 -1 -10 -3 Pa, filled with working gas argon and carbon dioxide, the molar proportion of carbon dioxide is controlled by flow meter to be 60%-70%, and the working gas pressure is controlled to be 1-500 Pa. After gas ignition, the doped calcium carbonate powder is solid-phase sintered at low temperature under low pressure environment, the sintering temperature is controlled at 500℃-600℃, the sintering time is 2-4 hours, and no grinding and re-calcination are required in the middle.
[0038] The final product, white light fluorescent powder, has an excitation wavelength of 200-350nm, a light emission wavelength of two fluorescence peaks: 471nm cyan and 615nm red, a powder particle size of 1-20μm, and a temperature tolerance of over 400°C.
[0039] Example 1
[0040] In order to illustrate the protective effect of low-temperature plasma sintering on the calcium carbonate matrix and the feasibility of low-temperature doping, Example 1 demonstrates the low-temperature plasma sintering of europium-doped red calcium carbonate phosphor.
[0041] In such Figure 1 The sample is placed in the device shown. The sample holder is a multi-layer alumina ceramic sheet structure with a heating wire embedded in the ceramic. The alumina is in direct contact with the sample to keep the sample pure. In this example, only red calcium carbonate fluorescent powder doped with europium oxide is prepared. A certain amount of CaCO3, Eu2O3 and Li2CO3 are weighed. The purity requirements of calcium carbonate and lithium carbonate are AR, and the purity requirement of europium oxide is 4N. The ratio of the three is 100:2:3, where Eu2O3 is 4N. 3+ As an activator, Li2CO3 is a cosolvent and charge compensator, and Mn can also be added 3+ As a sensitizer, the mixture was placed in a planetary ball mill and fully ground for 3 hours. After grinding, the powder was placed on an alumina multilayer powder rack and vacuumed to 10 -3 Pa, argon and carbon dioxide gas are introduced, with flow rates of 500sccm and 750sccm respectively, and the overall gas pressure is 100Pa. Argon is used as the ionized gas, and the pulse power is set. When the pulse voltage reaches a certain value, the pulse voltage can break through the argon gas, and the generated argon ions bombard the powder surface, so that the active area on the surface of the powder particles forms a hot zone, and the high-speed migration of the doped ions achieves the effect of high-speed diffusion, which promotes the full migration of the doped elements into the matrix to form good doping. The RF frequency used in this example is 12.56MHz, and the power used is 300W. The role of carbon dioxide as a protective gas is to inhibit the decomposition reaction of calcium carbonate powder during the sintering process. The sintering temperature is 560℃, and the sintering time is 4 hours. This sintering method has high thermal efficiency, and due to the diffuse distribution of the discharge points, uniform heating can be achieved, thus creating conditions for the preparation of high-quality phosphors. Figure 2 Comparing the product morphology of fluorescent powders prepared by plasma-assisted sintering under carbon dioxide protection and conventional sintering at 900 degrees at normal pressure, it can be seen that the powder does not condense due to the low sintering temperature of plasma sintering. However, the powder condenses under conventional high-temperature sintering at normal pressure, which is more unfavorable for the diffusion and doping of rare earth elements into the interior. In order to compare the protective effect of carbon dioxide on calcium carbonate powder, Figure 3 The product morphology of low temperature plasma sintering without carbon dioxide protection is shown, and it can be seen that the powder morphology is completely different. Figure 4 By comparing the effect of carbon dioxide protection on the powder lattice, it can be seen that the powder without carbon dioxide protection has a large number of diffraction peaks of calcium oxide, indicating that part of the calcium carbonate has decomposed into calcium oxide, which is not conducive to the application of fluorescent powder. Figure 5By comparing the fluorescence qualities of powders sintered at low temperature plasma and sintered at traditional high temperature under the same other conditions, it can be seen that the fluorescence of powders sintered at low temperature plasma is stronger, proving that the sintering method of the present invention is more uniform and in-depth in doping.
[0042] Example 2
[0043] To illustrate that using bismuth as the energy resonance transfer center and co-doping with europium and cerium can realize a monomer white light phosphor, Example 2 demonstrates the low temperature plasma sintering of europium and cerium co-doped calcium carbonate phosphor.
[0044] Weigh a certain amount of CaCO3, Eu2O3, Ce2O3 and Li2CO3. The purity of calcium carbonate and lithium carbonate should be AR, the purity of europium oxide and cerium oxide should be 4N, and the ratio of the three is 100:0.3:0.7:3. 3+ and Ce 3+ As an independent activator, Li2CO3 is a cosolvent and charge compensator, and Bi can also be added 3+ As the transfer center, the mixture is placed in a planetary ball mill and ground thoroughly for 3 hours. For co-doped powders, a pre-calcination process needs to be added. After grinding, the powder is placed on an alumina multilayer powder rack, 500°C is set as the calcination temperature, and pretreated for 120 minutes. The pretreated powder is placed in a planetary ball mill and ground again for 6 hours. Carbon dioxide and argon are introduced, the pulse power is set to 600W, the RF frequency is still 12.56MHz, the sintering temperature is 600°C, and the sintering time is 300 minutes. Figure 6 and Figure 7 They are the morphology and structural diffraction patterns of europium-cerium co-doped calcium carbonate phosphors. It can be seen that the powder has no obvious agglomeration and the lattice structure of the calcium carbonate matrix is intact and unchanged. Figure 8 This is the fluorescence spectrum of the phosphor. It can be seen that cyan and red light emissions exist simultaneously. Compared with pure cerium-doped and pure europium-doped phosphors, the red light emission peak of europium-cerium co-doped phosphors has changed significantly. For example, the blue light emission of pure cerium-doped phosphors has become cyan light emission, which indicates the existence of energy resonance transfer. The two discrete red light peaks of pure europium-doped phosphors have become one peak, indicating that the effect of co-doping on the product energy level exists.
[0045] The solution of this embodiment adopts low-temperature plasma solid-phase sintering of calcium carbonate powder, which avoids the decomposition of calcium carbonate caused by high temperature, and low-temperature sintering is conducive to overcoming the fluorescence quenching phenomenon caused by agglomeration during sintering of conventional powders. The white light phosphor prepared by the present invention is simpler and cheaper than the existing preparation method of three-primary color phosphor powder, and has a wider range of applications and stronger luminescence performance.
[0046] The contents described in the embodiments of this specification are merely enumerations of implementation forms of the inventive concept and are for illustrative purposes only. The protection scope of the present invention should not be considered to be limited to the specific forms described in this embodiment, and the protection scope of the present invention also extends to equivalent technical means that can be thought of by ordinary technicians in this field based on the inventive concept.
Claims
1. A low temperature plasma sintering method for calcium carbonate white light phosphor, It is characterized in that The calcium carbonate fluorescent powder based on the rare earth co-doping effect is sintered at low temperature in a plasma atmosphere without the need for hot pressing and external pressure facilities.
2. The low temperature plasma sintering method of calcium carbonate white light phosphor according to claim 1, It is characterized in that The phosphor is sintered with calcium carbonate as a matrix, europium and cerium as activators and bismuth as a sensitizer. The molar percentage of europium doping is 1-4%, the molar percentage of cerium doping is 1-5%, and the rare earth element is provided by rare earth oxide.
3. The low-temperature plasma sintering method of calcium carbonate white light phosphor as described in claim 2 is characterized in that the white light powder includes a monomer phosphor having a cyan luminescence peak and a red luminescence powder, wherein europium doping results in a red fluorescence peak, cerium doping results in a cyan fluorescence peak, and the luminescence of the two rare earth elements is regulated by bismuth as an energy transfer center.
4. The low temperature plasma sintering method of calcium carbonate white light phosphor according to claim 2, It is characterized in that Powder excitation wavelength: 200-350nm, luminescence wavelength: two fluorescence peaks at 471nm cyan and 615nm red, powder particle size: 1-20μm, temperature resistance: above 400℃.
5. The low temperature plasma sintering method of calcium carbonate white light phosphor according to claim 1, It is characterized in that Low-pressure plasma atmosphere solid-phase sintering is used. During the sintering process, there is no need to apply external mechanical high pressure to the powder. The sintering process uses a tubular furnace with a radio frequency plasma chamber. A multi-layer sample rack made of alumina ceramic sheets is used in the chamber to place calcium carbonate doped with rare earth oxides. The powder is loose and maintains a high specific surface area.
6. The low temperature plasma sintering method of calcium carbonate white light phosphor according to claim 5, It is characterized in that The sintering background pressure is 10 -1 -10 -3 Pa, the working air pressure is controlled at 1-500Pa. The atmosphere used is low-activity gas such as argon and carbon dioxide; argon as an ionized gas contains less oxygen and water, and its role in the sintering process is to provide high-kinetic energy argon ions, and the role of carbon dioxide is to inhibit the decomposition process of the calcium carbonate matrix during the sintering process and provide sufficient gas pressure to maintain the stability of the calcium carbonate matrix.
7. The low temperature plasma sintering method of calcium carbonate white light phosphor according to claim 6, It is characterized in that The working atmosphere is low-activity gas and carbon dioxide, the low-activity gas is argon or nitrogen, wherein the flow rate of argon or nitrogen during sintering is controlled to be 500-1000sccm, and the flow rate of carbon dioxide is controlled to be 1000-1500sccm.
8. The low temperature plasma sintering method of calcium carbonate white light phosphor according to claim 5, It is characterized in that In solid phase sintering, the sintering temperature is lower than 600°C, the sintering time is 2-4 hours, the plasma source frequency is 10-20MHZ, and the power is 500-800W.
Citation Information
Patent Citations
Ground limestone-based bismuth and europium co-doped yellow fluorescent powder
CN102585816A
Novel three-primary-color fluorescent powder based on heavy calcium carbonate and preparation method of novel three-primary-color fluorescent powder
CN114989810A
Hydrophobic calcium carbonate up-conversion red fluorescent powder and preparation method thereof
CN115353879A
Up-conversion fluorescent powder based on heavy calcium carbonate and preparation method of up-conversion fluorescent powder
CN115353883A
Calcium carbonate-based fluorescent material and method for producing the same