Electric fire fluorescence temperature measurement and 2000 nm infrared light enhancement material and preparation method thereof

By developing the fluorescence temperature measurement material of Sr2LaNbO6 formula, the use of rare earth ion energy levels to achieve high sensitivity temperature sensing, the problem of insufficient application of traditional thermometers in complex environments and insufficient technical cooperation in the laser industry is solved, and the efficient 2000nm infrared light material is achieved Preparation and temperature measurement.

CN119039987APending Publication Date: 2024-11-29JILIN JIANZHU UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410963323.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional contact thermometers have slow response and poor adaptability in complex environments, making them difficult to apply in environments such as strong magnetic fields and corrosion in the body. In addition, the laser industry lacks technical cooperation with CNC and optoelectronics companies, resulting in limited improvement in core competitiveness.

Method used

Develop a fluorescent temperature measurement material for electrical fires. Based on the Sr2LaNbO6 formula, Yb2O3, Ho2O3 and Nd2O3 are added, and prepared by high-temperature combustion to form a 2000nm infrared light material with high sensitivity and anti-interference ability, and use rare earth ion energy levels to achieve high resolution Temperature sensing.

Benefits of technology

The material has fast response, high sensitivity and high spatial resolution, and is suitable for electrical equipment and military aviation temperature detection. It also exhibits luminescent thermal enhancement under excitation of the 2000nm band, solving the insufficient application of traditional thermometers and lasers in complex environments. The problem of insufficient industrial technological cooperation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039987A_ABST
    Figure CN119039987A_ABST
Patent Text Reader

Abstract

The invention belongs to an electrical fire fluorescence temperature measurement and 2000 nm infrared light enhancement material and a preparation method thereof, and belongs to the field of rare earth luminescence. The preparation method comprises the following steps: weighing Sr2Co3 powder, La2O3 powder, Nb2O5 powder, Yb2O3 powder, Ho2O3 powder and Nd2O3 powder according to a molar ratio, mixing the powder together, putting the mixture into a grinding bowl, grinding for one hour, then putting the mixture into an Al2O3 crucible by adopting a high-temperature solid-phase method, putting the Al2O3 crucible and the Al2O3 crucible into a muffle furnace, and burning for 8 hours at 1250 DEG C, so as to obtain the Sr2Co3-Nb2O5 composite material. And finally, cooling the synthesized sample to room temperature, adding alcohol into an agate mortar, and grinding for 1 hour. The Sr2LaNbO6: Yb < 3 + > / Nd < 3 + > / Ho < 3 + > doped fluorescent powder prepared by the invention has high sensitivity and thermal enhancement characteristic. The invention belongs to the technical field of rare earth fluorescence temperature measurement sensors, and results show that the rare earth fluorescence temperature measurement material is an optical temperature measurement material with high sensitivity, can be used as a fluorescence temperature material for electrical fire and can be used for enhancing 2000nm infrared light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of fluorescent temperature measuring materials, and specifically relates to a fluorescent temperature of electrical fire and enhanced 2000nm infrared light material and a preparation method. Background Art

[0002] Traditional contact thermometers have been widely used in many areas. However, their slow response and poor ability to adapt to complex environments, such as strong magnetic fields in the body and corrosive environments, are the main obstacles limiting their application.

[0003] With the continuous expansion of infrared light sources in space communications, medical surgery, radar system engineering, remote sensing, environmental monitoring and military fields, the importance of infrared light sources emitted by lasers has become increasingly apparent. Lasers in the 2000nm band are becoming more and more popular. 2000nm lasers correspond to the characteristic absorption spectra of many gaseous pollutants and can be strongly absorbed by water molecules and other biological tissues. They are becoming more and more popular in the 2000nm human eye-safe spectrum region because when 2000nm lasers are shot into the eye, they will be strongly absorbed by the cornea and lens in the eye and are difficult to radiate to the highly sensitive retina, thus causing less harm to the human eye. They have broad application prospects in the civil and military fields. In medical surgery, they cause less damage to tissues and can achieve high surgical precision. In industry, 2000nm lasers are very suitable for cutting and welding of plastic materials. Compared with 1-micron laser cutting and welding, non-metallic materials have a very low absorption rate for 1000nm lasers. Additives to enhance absorption must be added during welding, and some materials have a relatively high sensitivity to 2000nm lasers. Strong absorption. In the field of environmental protection, the 2000nm band can detect the content of toxic and harmful gases such as Co, No2, CH4 and Co2 in the air with very high sensitivity. Therefore, it is of great significance to atmospheric environment monitoring and pollution prevention and control. In the military field, 2000nm band lasers have good penetration ability for battlefield smoke and haze, especially single longitudinal mode narrow linewidth and high pulse energy lasers can be used for wind radar, differential absorption radar, portable laser ranging, etc. Compared with previous carbon dioxide lasers, the wavelength of 2000nm lasers is much smaller than that of carbon dioxide gas lasers, and a narrower spectral line width can be obtained, which increases its measurement accuracy by an order of magnitude compared with carbon dioxide gas laser radars, and can accurately track satellites and rockets. In addition, 2000nm lasers can pump nonlinear crystal optical parametric oscillators (OPOs) and amplifiers (OPAs) such as ZnGep to generate mid- and far-infrared lasers for military optoelectronic countermeasure technology.

[0004] The core technologies in the development of the laser industry, such as the control software required for laser equipment and the special optical fibers necessary for the production of fiber lasers, have been difficult to achieve breakthroughs due to the lack of technical collaboration with CNC-related companies and optoelectronics-related companies. This has restricted the improvement of the core competitiveness of the laser industry, and the light emission is weak and is greatly affected by temperature. Summary of the invention

[0005] Non-contact thermometers avoid the above problems to a large extent. The present invention provides a fluorescent temperature measurement for electrical fires and a 2000nm infrared light enhancement material and a preparation method.

[0006] Moreover, it has strong anti-interference ability and high signal resolution, and is increasingly valued by people. LIR technology can provide excellent sensitivity and superior temperature resolution. The temperature detection technology based on LIR is divided into two types: thermal coupling level (TCLS) and non-thermal coupling level (NTCLS). The energy level difference ΔE of thermal coupling level is small, about 200-2000cm -1 , the non-thermal coupling energy level difference ΔE is greater than 2000cm -1 Generally speaking, the greater the energy level difference, the higher the sensitivity of temperature sensing. Therefore, the thermal coupling energy level is affected by the energy level difference, and the sensitivity of temperature sensing is generally not high. For rare earth ions, their energy levels are usually NTCLS, and their energy levels are far apart, and the signal resolution is high. Therefore, temperature sensing with LIR of NTCLS is an effective method to improve the sensitivity of temperature measurement. If there are multiple rare earth ion energy level pairs that can be used for temperature measurement in the material at the same time, it is more conducive to the sensitivity of optical temperature measurement.

[0007] The technical solution of the present invention is:

[0008] A method for preparing a fluorescent temperature measurement and 2000nm infrared light enhancement material for electrical fires, the method comprising:

[0009] According to the chemical formula Sr2LaNbO6, weigh Sr2Co3, La2O3 and Nb2O5; mix them as a substrate;

[0010] Weigh the Yb2O3, Ho2O3, and Nd2O3 powders according to their molar content in the substrate, and the molar content satisfies: 5% Yb 3+ / 0.6%Ho 3+ / x%Nd 3+ , x=0,1,2,3,4;

[0011] The powder was weighed to obtain a mixed white powder solid. The white powder solid was ground in an agate mortar with alcohol for 1 hour. The ground powder was transferred to an Al2O3 crucible and placed in a high-temperature box-type electric furnace and burned at 1250°C for 8 hours.

[0012] Furthermore, the purity of Sr2Co3 is 99%, the purity of La2O3 is 99.9%, the purity of Nb2O5 is 99.9%, the purity of Yb2O3 is 99.9%, the purity of Ho2O3 is 99.9%, and the purity of Nd2O3 is 99.9%.

[0013] Further, according to 1 mol of Sr2LaNbO6,

[0014] When x=0, the weight of Sr2Co3 is 1.761g, La2O3 is 0.917g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, and the weight of Ho2O3 is 0.007g;

[0015] When x=1, the weight of Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.010g;

[0016] When x=2, the weighed Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.020g;

[0017] When x=3, the weighed Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.030g;

[0018] When x=4, the weighed Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.040g.

[0019] A fluorescent temperature measurement and enhancement 2000nm infrared material for electrical fires, the composition of the infrared material is: Sr2LaNbO6: 5% Yb 3+ / 0.6%Ho 3+ / x%Nd 3+ , x=0, 1, 2, 3, 4, % represents the molar percentage.

[0020] Furthermore, the composition of the infrared light material is: Sr2LaNbO6: 5% Yb 3+ / 0.6%Ho 3+ / 2%Nd 3+ .

[0021] The beneficial effects of the present invention include:

[0022] The material has the following characteristics: (1) sensitivity and high resolution; (2) resistance to light damage and object compatibility; (3) easy preparation and use, and suitable for various electrical devices.

[0023] The fluorescence intensity ratio technology based on the energy level of rare earth ions has the advantages of fast response, high sensitivity and spatial resolution, and has quickly become a research hotspot in the field of temperature detection. Compared with traditional fluorescent temperature probe materials, rare earth doped down-conversion temperature measurement materials have broad development potential in temperature detection of electrical equipment or military aviation due to their excellent luminescence properties, low toxicity, low biological background fluorescence interference, and deep tissue penetration. Specifically, under 980nm excitation, the temperature sensing characteristics of this fluorescent temperature measurement material were tested (in 5% Yb 3+ As a sensitizer, 0.6% Ho was doped as an activator. 3+ / 2%Nd 3+ ). Sr2LaNbO6:5%Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+ 3D waterfall diagram of the sample upconversion in the temperature range of 293 to 493 K. Sr2LaNbO6:5%Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+ Normalized spectra of the samples in the temperature range of 293 to 493 K. Sr2LaNbO6:5%Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+ In the range of 303 to 493K, FIR, S A , S R picture.

[0024] The 2000nm infrared band has been effectively solved through reasonable experimental design, which effectively solves biological, military, industrial and other problems. Specifically, under 808nm excitation, the temperature sensing characteristics of this fluorescent temperature measurement material were tested (in 5% Yb 3+ As a sensitizer, 0.6% Ho was doped as an activator. 3+ / 2%Nd 3+ ), Sr2LaNbO6:5%Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+ 3D waterfall diagram of the sample upconversion in the temperature range of 293 to 493 K. At the same pump power, 906 nm (Nd 3 + : 4 F 3 / 2 → 4 I9 / 2 ), around 1016nm (Yb 3+ : 2 F 5 / 2 → 4 I 11 / 2 ), 1074nm(Nd 3+ : 4 F 3 / 2 → 4 I 11 / 2 ), 1347nm(Nd 3+ : 4 F 3 / 2 → 4 I 13 / 2 ) The emission intensity increases with increasing temperature. Studies have shown that Sr2LaNbO6:5%Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+ The sample produced a phenomenon of thermal enhancement of luminescence. Figure 7 (b) Sr2LaNbO6:5%Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+ Normalized spectra of the samples in the temperature range of 293 to 493 K. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A flow chart of a high temperature solid phase method for preparing materials according to an embodiment of the present invention;

[0026] Figure 2 A flow chart of the up-down conversion spectrum of the Sr2LaNbO6 phosphor provided in an embodiment of the present invention;

[0027] Figure 3 The XRD spectrum of Sr2LaNbO6 provided in the embodiment of the present invention;

[0028] Figure 4 SEM structure diagram of Sr2LaNbO6 provided in the embodiment of the present invention: (a) 2% Nd 3+ / 0.6%Ho 3+ (b) 20% Yb 3+ / 0.6%Ho 3+ (c) 5% Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+

[0029] Figure 5 Fourier transform infrared spectrum of Sr2LaNbO6 provided in the embodiment of the present invention: (a) 2% Nd 3+ / 0.6%Ho 3 +(b) 20% Yb 3+ / 0.6%Ho 3+ (c) 5% Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+

[0030] Figure 6 (a) Sr2LaNbO6: x% Nd provided in the embodiment of the present invention 3+ / 0.6%Ho 3+ NIR emission spectrum under 808nm excitation. (b) Sr2LaNbO6: 5% Yb 3+ / x%Nd 3+ / 0.6%Ho 3+ NIR emission spectrum under 808nm excitation. (c) Sr2LaNbO6:Yb 3+ / Nd 3+ / Ho 3+ Comparison of NIR emitters' spectral intensity at 808 nm excitation.

[0031] Figure 7 (a) UC emission spectrum of Sr2LaNbO6 provided in the embodiment of the present invention: 20% Yb 3+ / x%Ho 3+ Excitation at 980nm. (b) Sr2LaNbO6: 20% Yb 3+ / 0.6%Ho 3+ The logarithmic linear fitting line of pump power and emission intensity. DS emission spectrum of Sr2LaNbO6: 20% Yb 3+ / x%Ho 3+ Excitation at 980nm (c) 1000nm-1250nm. (d) 1800nm-2250nm.

[0032] Figure 8 Sr2LaNbO6:5%Yb provided in the embodiment of the present invention 3+ / x%Nd 3+ / 0.6%Ho 3+ Emission spectra of UC excited at 980nm (a) 500nm-700nm. (b) 700nm-960nm.

[0033] Fig. 9 Sr2LaNbO6:5%Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+3D waterfall plots of the emission intensity at temperatures of 293K-493K for (a) 850nm-1500nm, (b) 1700nm-2250nm. Histogram of the relationship between emission intensity and temperature (293K-493K) for (c) 850nm-1500nm, (d) 1700nm-2250nm. Normalized plot of the relationship between temperature and emission intensity for (e) 850nm-1500nm, (f) 1700nm-2250nm.

[0034] Fig.10 Using Sr2LaNbO6:5%Yb at 293K-493K 3+ / 2%Nd 3+ / 0.6%Ho 3+ (a) 3D mapping of UC emission intensity projection. Histogram of the relationship between temperature and UC emission intensity (b) 500nm-700nm, (c) 700nm-960nm. Normalized curve of the relationship between temperature and UC emission intensity (d) 500nm-700nm, (e) 700nm-960nm.

[0035] Fig.11 (ac) Non-TCL based Sr2LaNbO6:5%Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+ LIR, SA and SR. DETAILED DESCRIPTION

[0036] The present invention is further described below in conjunction with the accompanying drawings and schematic diagrams of experimental phenomena.

[0037] Figure 1 A flow chart of a high temperature solid phase method for preparing materials according to an embodiment of the present invention;

[0038] Example 1

[0039] A method for preparing a fluorescent temperature measurement and 2000nm infrared light enhancement material for electrical fires, the method comprising:

[0040] According to the chemical formula Sr2LaNbO6, weigh Sr2Co3, La2O3 and Nb2O5; mix them as a substrate;

[0041] Weigh the Yb2O3, Ho2O3, and Nd2O3 powders according to their molar content in the substrate, and the molar content satisfies: 5% Yb 3+ / 0.6%Ho 3+ / x%Nd 3+ , x = 0;

[0042] The powder was weighed to obtain a mixed white powder solid. The white powder solid was ground in an agate mortar with alcohol for 1 hour. The ground powder was transferred to an Al2O3 crucible and placed in a high-temperature box-type electric furnace and burned at 1250°C for 8 hours.

[0043] The purity of Sr2Co3 is 99%, the purity of La2O3 is 99.9%, the purity of Nb2O5 is 99.9%, the purity of Yb2O3 is 99.9%, the purity of Ho2O3 is 99.9%, and the purity of Nd2O3 is 99.9%.

[0044] Among them, according to 1 mol of Sr2LaNbO6,

[0045] When x=0, the weight of Sr2Co3 is 1.761g, La2O3 is 0.917g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, and the mass of Ho2O3 is 0.007g.

[0046] When x=1, the weight of Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.010g;

[0047] When x=2, the weighed Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.020g;

[0048] When x=3, the weighed Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.030g;

[0049] When x=4, the weighed Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.040g.

[0050] Example 2

[0051] A method for preparing a fluorescent temperature measurement and 2000nm infrared light enhancement material for electrical fires, the method comprising:

[0052] According to the chemical formula Sr2LaNbO6, weigh Sr2Co3, La2O3 and Nb2O5; mix them as a substrate;

[0053] Weigh the Yb2O3, Ho2O3, and Nd2O3 powders according to their molar content in the substrate, and the molar content satisfies: 5% Yb 3+ / 0.6%Ho 3+ / x%Nd 3+ , x=1;

[0054] The powder was weighed to obtain a mixed white powder solid. The white powder solid was ground in an agate mortar with alcohol for 1 hour. The ground powder was transferred to an Al2O3 crucible and placed in a high-temperature box-type electric furnace and burned at 1250°C for 8 hours.

[0055] The purity of Sr2Co3 is 99%, the purity of La2O3 is 99.9%, the purity of Nb2O5 is 99.9%, the purity of Yb2O3 is 99.9%, the purity of Ho2O3 is 99.9%, and the purity of Nd2O3 is 99.9%.

[0056] Among them, according to 1 mol of Sr2LaNbO6,

[0057] When x=1, the weight of Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.010g.

[0058] Example 3

[0059] A method for preparing a fluorescent temperature measurement and 2000nm infrared light enhancement material for electrical fires, the method comprising:

[0060] According to the chemical formula Sr2LaNbO6, weigh Sr2Co3, La2O3 and Nb2O5; mix them as a substrate;

[0061] Weigh the Yb2O3, Ho2O3, and Nd2O3 powders according to their molar content in the substrate, and the molar content satisfies: 5% Yb 3+ / 0.6%Ho 3+ / x%Nd 3+ , x = 2;

[0062] The powder was weighed to obtain a mixed white powder solid. The white powder solid was ground in an agate mortar with alcohol for 1 hour. The ground powder was transferred to an Al2O3 crucible and placed in a high-temperature box-type electric furnace and burned at 1250°C for 8 hours.

[0063] The purity of Sr2Co3 is 99%, the purity of La2O3 is 99.9%, the purity of Nb2O5 is 99.9%, the purity of Yb2O3 is 99.9%, the purity of Ho2O3 is 99.9%, and the purity of Nd2O3 is 99.9%.

[0064] Among them, according to 1 mol of Sr2LaNbO6,

[0065] When x=2, 1.761g of Sr2Co3, 0.907g of La2O3, 0.793g of Nb2O5, 0.059g of Yb2O3, 0.007g of Ho2O3, and 0.020g of Nd2O3 were weighed.

[0066] Embodiment 41

[0067] A method for preparing a fluorescent temperature measurement and 2000nm infrared light enhancement material for electrical fires, the method comprising:

[0068] According to the chemical formula Sr2LaNbO6, weigh Sr2Co3, La2O3 and Nb2O5; mix them as a substrate;

[0069] Weigh the Yb2O3, Ho2O3, and Nd2O3 powders according to their molar content in the substrate, and the molar content satisfies: 5% Yb 3+ / 0.6%Ho 3+ / x%Nd 3+ , x = 3;

[0070] The powder was weighed to obtain a mixed white powder solid. The white powder solid was ground in an agate mortar with alcohol for 1 hour. The ground powder was transferred to an Al2O3 crucible and placed in a high-temperature box-type electric furnace and burned at 1250°C for 8 hours.

[0071] The purity of Sr2Co3 is 99%, the purity of La2O3 is 99.9%, the purity of Nb2O5 is 99.9%, the purity of Yb2O3 is 99.9%, the purity of Ho2O3 is 99.9%, and the purity of Nd2O3 is 99.9%.

[0072] Among them, according to 1 mol of Sr2LaNbO6,

[0073] When x=3, 1.761g of Sr2Co3, 0.907g of La2O3, 0.793g of Nb2O5, 0.059g of Yb2O3, 0.007g of Ho2O3, and 0.030g of Nd2O3 were weighed.

[0074] Example 5

[0075] A method for preparing a fluorescent temperature measurement and 2000nm infrared light enhancement material for electrical fires, the method comprising:

[0076] According to the chemical formula Sr2LaNbO6, weigh Sr2Co3, La2O3 and Nb2O5; mix them as a substrate;

[0077] Weigh the Yb2O3, Ho2O3, and Nd2O3 powders according to their molar content in the substrate, and the molar content satisfies: 5% Yb 3+ / 0.6%Ho 3+ / x%Nd 3+ , x = 4;

[0078] The powder was weighed to obtain a mixed white powder solid. The white powder solid was ground in an agate mortar with alcohol for 1 hour. The ground powder was transferred to an Al2O3 crucible and placed in a high-temperature box-type electric furnace and burned at 1250°C for 8 hours.

[0079] The purity of Sr2Co3 is 99%, the purity of La2O3 is 99.9%, the purity of Nb2O5 is 99.9%, the purity of Yb2O3 is 99.9%, the purity of Ho2O3 is 99.9%, and the purity of Nd2O3 is 99.9%.

[0080] Among them, according to 1 mol of Sr2LaNbO6,

[0081] When x=4, the weighed Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.040g.

[0082] Figure 2 The up-down conversion spectrum flow chart of Sr2LaNbO6 phosphor provided by the embodiment of the present invention is mainly composed of a 980nm diode laser, a λ500 spectrometer, a phase-locked amplifier, a photon counter and a computer.

[0083] Figure 3 XRD spectrum of Sr2LaNbO6; XRD and SEM characterize CaIn2O4 as belonging to the orthorhombic system; FTIR characterizes the low phonon energy of the CaIn2O4 matrix, making it an excellent material for preparing phosphors; the control accuracy of the temperature sensing characteristics of the prepared material is 0.1℃;

[0084] Figure 4 SEM structure diagram of Sr2LaNbO6: (a) 2% Nd 3+ / 0.6%Ho 3+ (b) 20% Yb 3+ / 0.6%Ho 3+ (c) 5% Yb3+ / 2% Nd 3+ / 0.6%Ho 3+The morphology of the sample was recorded using a JEOL scanning electron microscope (FE-SEM, Quanta 450, FEI). It was found that the sample was composed of regular, smooth crystalline particles with a dumbbell-like shape and reached the micrometer level. The prepared particles were almost uniform in size, with an average diameter of about 2.5 μm.

[0085] Figure 5 Fourier transform infrared spectrum of Sr2LaNbO6: (a) 2% Nd 3+ / 0.6%Ho 3+ (b) 20% Yb 3+ / 0.6%Ho 3 + (c) 5% Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+ Fourier-transform infrared spectroscopy (FTIR) was performed on the two groups of samples using a PerkinElmer SpectrumTwo (PerkinElmer, USA). The test results showed that the wavelength of the infrared spectroscopy was 524-663 cm -1 The strong absorption band at 826cm is due to the symmetrical stretching and asymmetrical bending of the octahedron, while -1 The sharp peaks near 660 cm are due to the stretching vibrations of the Ia-O-Ia and Ia-OO-Ia bridge bonds. -1 This is consistent with the previous study that the phonon energy of the Sr2LaNbO6 matrix is ​​670cm -1 From the spectroscopic point of view, Sr2LaNbO6 oxide is a promising host material for lanthanide ion doping.

[0086] Figure 6 (a) Sr2LaNbO6: x%Nd 3+ / 0.6%Ho 3+ NIR emission spectrum under 808nm excitation. (b) Sr2LaNbO6: 5% Yb 3+ / x%Nd 3+ / 0.6%Ho 3+ NIR emission spectrum under 808nm excitation. (c) Sr2LaNbO6:Yb 3+ / Nd 3+ / Ho 3+ Comparative spectral intensity of NIR emitters excited at 808 nm. SLNO:x%Nd was measured at 808 nm excitation. 3+ / 0.6%Ho 3+DS NIR emission spectra of the samples (x=0, 1, 2, 3, 4) at 850nm-1500nm and 1700nm-2250nm. Nd 3+ The three emission peaks are 906nm ​​(Nd 3+ : 4 F 3 / 2 → 4 I 9 / 2 ), 1074nm(Nd 3+ : 4 F 3 / 2 → 4 I 11 / 2 ), 1347nm(Nd 3+ : 4 F 3 / 2 → 4 I 13 / 2 ), the broadband at 1700nm-1920nm in the emission spectrum range of 1700nm-2250nm belongs to Nd 3+ : 4 F 3 / 2 → 4 I 15 / 2 Energy level transition, the broadband at 1920nm-2250nm belongs to Ho 3+ : 5 I7→ 5 The energy level transition of I8, due to the Stark splitting effect, the energy level transition of 5I7→5I8 will have three emission peaks, which are 1938nm, 1974nm, and 2008nm. In this emission process, SLNO:4%Nd 3+ / 0.Ho 3+ The sample emission intensity is the largest, which also proves that Nd 3+ →Ho 3+ The energy transfer process of SLNO:5%Yb was measured under 808nm excitation. 3+ / x%Nd 3+ / 0.6%Ho 3+ DS NIR emission spectra of the samples (x=0, 0.01, 0.002, 0.03, 0.04) at 850nm-1500nm and 1700nm-2250nm. There are four emission peaks in the emission spectrum in the range of 850nm-1500nm, which are 906nm ​​(Nd 3+ : 4 F 3 / 2 → 4 I 9 / 2 ), around 1016nm (Yb 3+ : 2 F 5 / 2→ 4 I 11 / 2 ), 1074nm(Nd 3+ : 4 F 3 / 2 → 4 I 11 / 2 ), 1347nm(Nd 3+ : 4 F 3 / 2 → 4 I 13 / 2 ), realizing Nd 3+ →Yb 3+ In the energy transfer process, the position of the emission peak in the emission spectrum in the range of 1700nm-2250nm does not change significantly, but the emission intensity changes significantly. The luminescence intensity increases first and then decreases. 3+ / 2%Nd 3+ / 0.6%Ho 3+ The emission intensity is the largest, in order to more clearly contrast Yb 3+ The effect of adding SLNO:5%Yb on the sample was compared under the same conditions. 3+ / 0.6%Ho 3+ ; SLNO: 2% Nd 3+ ; SLNO: 2% Nd 3+ / 0.6%Ho 3+ SLNO:5%Yb 3+ / 2%Nd 3+ SLNO:5%Yb 3+ / 2%Nd 3+ The emission spectra of the five samples with 0.6% Ho under 808nm laser clearly show that the DS NIR emission spectra at 850nm-1500nm and 1700nm-2250nm increase with the increase of Yb 3+ Addition of Nd ions 3+ All emission peaks of the Yb 3+ : 2 F 5 / 2 → 4 I 11 / 2 ) transition and Ho 3+ Around 2000nm ( 5 I7→5I8) position, indicating that Yb 3+ The addition of ions creates a new energy transfer pathway Nd 3+ →Yb 3+ →Ho 3+ Enhanced Ho 3+ emission peak, but weakens the Nd 3+ emission peak.

[0087] Figure 7 (a) UC emission spectrum of Sr2LaNbO6: 20% Yb 3+ / x%Ho 3+ Excitation at 980nm. (b) Sr2LaNbO6: 20% Yb 3+ / 0.6%Ho 3+ The logarithmic linear fitting line of pump power and emission intensity. DS emission spectrum of Sr2LaNbO6: 20% Yb 3+ / x%Ho 3+ SLNO:20%Yb was measured under 980nm excitation (c) 1000nm-1250nm. (d) 1800nm-2250nm. 3+ / x%Ho 3+ The UC emission spectra of the pure SLNO samples at 500nm-700nm, and the DS NIR emission spectra at 1000nm-1250nm and 1800nm-2250nm, two emission peaks were obtained at 500nm-700nm, namely, the strong green at 550nm comes from Ho 3+ : 5 S2, 5 F4→ 5 I8, red at 670nm comes from Ho 3+ : 5 F5→ 5 I8, where the luminous intensity increases first and then decreases, in SLNO:20%Yb 3+ / 0.6%Ho 3+ The sample emission intensity reached the strongest, and the SLNO:20%Yb 3+ / x%Ho 3+ The UC emission spectra of the pure SLNO samples at 500nm-700nm, and the DS NIR emission spectra at 1000nm-1250nm and 1800nm-2250nm, two emission peaks were obtained at 500nm-700nm, namely, the strong green at 550nm comes from Ho 3+ : 5 S2, 5 F4→ 5 I8, red at 670nm comes from Ho 3+ : 5 F5→ 5 I8, where the luminous intensity increases first and then decreases, in SLNO:20%Yb 3+ / 0.6%Ho 3+ The emission intensity of the sample reaches the highest level.

[0088] Figure 8 Sr2LaNbO6:5%Yb 3+ / x%Nd 3+ / 0.6%Ho 3+ UC emission spectra of SLNO:5%Yb under excitation at 980nm (a) 500nm-700nm. (b) 700nm-960nm. Under excitation at 980nm in the 500nm-700nm band, SLNO:5%Yb 3+ / 2%Nd 3+ There is a very faint green at 530nm from Nd 3+ : 4 G 7 / 2 → 4 I 9 / 2 , and the strong green color of other samples at 550 nm comes from Ho 3+ : 5 S2, 5 F4→ 5 I8, red at 670nm comes from Ho 3+ : 5 F5→ 5 I8, it can be clearly seen that because Nd 3+ After joining, Ho 3+ The luminescence is less than that of undoped Nd 3+ To reduce, and doping Nd 3+ After that, the luminous intensity first increases and then decreases. 3+ / 2%Nd 3+ / 0.6%Ho 3+ The luminescence reaches the maximum value, which proves that Nd 3+ The doping of Yb 3+ to Ho 3+ Transfer energy.

[0089] SLNO:5%Yb under 980nm excitation in the 700nm-960nm band 3+ / 0.6%Ho 3+ The sample has a very weak Ho 3+ : 5 S2, 5 F4→ 5 The weak red light of I7 and other samples at 755nm (Nd 3+ : 4 F 7 / 2 → 4 I 9 / 2 ), 820nm(Nd 3+ : 4F 5 / 2 → 4 I 9 / 2 ), 875nm(Nd 3+ : 4 F 3 / 2 → 4 I 9 / 2 ), it can be clearly seen that because Ho 3+ After the addition of 3+ The luminescence is less than that of undoped Ho 3+ To reduce, and doping Ho 3+ After that, the luminous intensity first increases and then decreases. 3 + / 2%Nd 3+ / 0.6%Ho 3+ The luminescence reaches the maximum value, which proves that Ho 3+ The doping of Yb 3+ To Nd 3+ Transfer energy.

[0090] Fig. 9 Sr2LaNbO6:5%Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+ 3D waterfall plots of the emission intensity at 293K-493K (a) 850nm-1500nm, (b) 1700nm-2250nm. Histogram of the relationship between emission intensity and temperature (293K-493K) (c) 850nm-1500nm, (d) 1700nm-2250nm. Normalized graph of the relationship between temperature and emission intensity (e) 850nm-1500nm, (f) 1700nm-2250nm. In the emission spectrum in the 850nm-1500nm range, 906nm ​​(Nd 3+ : 4 F 3 / 2 → 4 I 9 / 2) The integrated intensity is about 3.02 times that at 293K, and at 493K around 1016nm (Yb 3+ : 2 F 5 / 2 → 4 I 11 / 2 ) has an emission intensity about 2.02 times higher than that at 293K. At 493K, the emission intensity near 1074nm (Nd 3+ : 2 F 3 / 2 → 4 I 11 / 2 ) has an emission intensity about 2.36 times higher than that at 293K. 3+ :4 F 3 / 2 → 4 I 13 / 2) The emission intensity is about 2.31 times higher than that at 293K. The thermal enhancement of each emission band is different. In the figure, the emission intensities at 906nm, 1016nm, 1074nm and 1347nm at different temperatures are shown. In the emission spectrum in the range of 1700nm-2250nm, the broadband (Nd 3+ : 4 F 3 / 2 → 4 I 15 / 2 ) The integrated intensity at 493K is about 1.72 times that at 293K, and the broadband at 1920nm-2250nm belongs to Ho 3+ : 5 I7→ 5 The energy level transition of I8 is due to the Stark splitting effect 5 I7→ 5 The energy level transition of I8 will produce three emission peaks at 1938nm, 1974nm, and 2008nm. The integrated intensity at 493K is about 1.35, 1.54, and 1.39 times that at 293K. The thermal enhancement of each emission band is different. The emission intensity of 1838nm, 1938nm, 1974nm, and 2008nm at different temperatures. The possible reason for the enhancement of luminescence intensity is that as the temperature increases, Nd 3+ The absorption peak of Nd ions becomes broader with increasing temperature, resulting in enhanced absorption, which in turn enhances the 3+ →Yb 3+ →Ho 3+ energy transfer channel, which further manifests as overall luminescence enhancement.

[0091] Fig.10 Using Sr2LaNbO6:5%Yb at 293K-493K 3+ / 2%Nd 3+ / 0.6%Ho 3+ (a) Three-dimensional mapping of UC emission intensity projection. Histogram of the relationship between temperature and UC emission intensity (b) 500nm-700nm, (c) 700nm-960nm. Normalized curve of the relationship between temperature and UC emission intensity (d) 500nm-700nm, (e) 700nm-960nm. Keep the excitation power low (50mW) under 980nm excitation to avoid self-heating of the sample under high pump power. The emission spectrum of SLNO:20%Yb3+ / 2%Nd3+ / 0.6%Ho3+ phosphor in the temperature range of 293~493K was measured. In the temperature range of 293K-493K, it can be clearly observed that the Ho 3+The emission bands centered at 542nm, 555nm, and 670nm decrease significantly with increasing temperature, while the emission intensity of Nd 3+ The relevant emission bands centered at 755 nm, 820 nm, and 875 nm vary significantly with increasing temperature. For the near-infrared emission, thermal enhancement occurs because the near-infrared emission is obtained through a multi-phonon-assisted energy transfer process that increases with increasing temperature. The relative intensities of the different emission bands appear to be different and vary with increasing temperature. Fig.11 (be) This phenomenon is more clearly reflected by drawing the normalized graph of each peak emission intensity. Using this law, the temperature measurement sensitivity of SLNO: 20% Yb3+ / 2% Nd3+ / 0.6% Ho3+ phosphor based on non-thermal coupling energy level is studied. 542nm and 555nm are collectively referred to as one peak and counted as 555nm, and 755nm, 820nm and 875nm are collectively referred to as one peak and counted as 820nm.

[0092] Fig.11 (ac) Non-TCL based Sr2LaNbO6:5%Yb 3+ / 2%Nd 3+ / 0.6%Ho 3+ The absolute and relative temperature measurement sensitivities corresponding to the three LIRs gradually increase with the increase of temperature, especially for I820 nm / I670 nm at 293K. R The maximum value reached 5.4755336% K-1. The results show that the purpose of optimizing the sensitivity of rare earth fluorescence temperature measurement has been achieved and good results have been achieved.

Claims

1. A method for preparing a material for fluorescent temperature measurement and 2000nm infrared light enhancement for electrical fires, characterized in that: The method includes: According to the chemical formula Sr2LaNbO6, weigh Sr2Co3, La2O3 and Nb2O5; mix them as a substrate; Weigh the Yb2O3, Ho2O3, and Nd2O3 powders according to their molar content in the substrate, and the molar content satisfies: 5% Yb 3+ / 0.6%Ho 3+ / x%Nd 3+ , x=0,1,2,3,4; The powder was weighed to obtain a mixed white powder solid. The white powder solid was ground in an agate mortar with alcohol for 1 hour. The ground powder was transferred to an Al2O3 crucible and placed in a high-temperature box-type electric furnace and burned at 1250°C for 8 hours.

2. The method for preparing the material for fluorescent temperature measurement and 2000nm infrared light enhancement for electrical fires according to claim 1, characterized in that: The purity of Sr2Co3 is 99%, the purity of La2O3 is 99.9%, the purity of Nb2O5 is 99.9%, the purity of Yb2O3 is 99.9%, the purity of Ho2O3 is 99.9%, and the purity of Nd2O3 is 99.9%.

3. The method for preparing the material for fluorescent temperature measurement and 2000nm infrared light enhancement for electrical fires according to claim 1, characterized in that: According to 1 mol of Sr2LaNbO6, When x=0, the weight of Sr2Co3 is 1.761g, La2O3 is 0.917g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, and the weight of Ho2O3 is 0.007g; When x=1, the weight of Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.010g; When x=2, the weighed Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.020g; When x=3, the weighed Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.030g; When x=4, the weighed Sr2Co3 is 1.761g, La2O3 is 0.907g, Nb2O5 is 0.793g, Yb2O3 is 0.059g, Ho2O3 is 0.007g, and Nd2O3 is 0.040g.

4. A fluorescent temperature measurement and 2000nm infrared light enhancement material for electrical fires, characterized in that: The composition of the infrared light material is: Sr2LaNbO6: 5% Yb 3+ / 0.6%Ho 3+ / x%Nd 3+ , x=0, 1, 2, 3, 4, % represents the molar percentage.

5. The fluorescent temperature measurement and 2000nm infrared light enhancement material for electrical fires according to claim 4, characterized in that: The composition of the infrared light material is: Sr2LaNbO6: 5% Yb 3+ / 0.6%Ho 3+ / 2%Nd 3+ .