Preparation method of high-silicon solution strengthening ferrite ductile iron pipe fitting

Ferrite pellet ink is solved by using mixed ball milling technology of metal oxides such as lanthanum oxide and cerium oxide with ferrosilicon and calcium carbide in the preparation of ferrite pellet pipe fittings, as well as vacuum smelting and fast quenching technology of iron niobium, etc. The problems of low graphite spheroidization rate and uneven microstructure of cast iron pipe fittings have significantly improved their mechanical properties and service life.

CN119040557APending Publication Date: 2024-11-29LIAONING EVER FOUNDRY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411172612.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The graphite spheroidization rate during the casting process of existing ferrite ductile iron pipe fittings is not high, and the microstructure is uneven, resulting in insufficient yield strength and tensile strength when they withstand large external forces, and their service life is short.

Method used

The preparation method of high-silicon solid solution-strengthening ferrite sphere pipe fittings is adopted. By mixing metal oxides such as lanthanum oxide and cerium oxide with ferrosilicon and calcium carbide and ball milling, the lanthanum-containing spheroidizing agent is prepared, and iron niobium and vanadium are niobium- Iron and pig iron are mixed with vacuum smelted to make a composite incubator. The wire feeding equipment is spheroidized and incubated in an intermediate frequency induction furnace to form spheroidized cast iron liquid and annealed heat treatment is performed.

Benefits of technology

It improves graphite spheroidization rate and grain refinement, significantly improves the mechanical properties of iron pipe fittings, including yield strength, tensile strength and tensile ratio, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040557A_ABST
    Figure CN119040557A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a high-silicon solution strengthening ferrite ductile iron pipe fitting, and belongs to the technical field of ductile iron. Comprising the following preparation steps: preparing a cored wire; mixing and melting; primary inoculation treatment; pouring is conducted; and annealing heat treatment. The lanthanum-containing spheroidizing agent is prepared by mixing, ball-milling and smelting metal oxides such as lanthanum oxide and cerium oxide with the reducing agent silicon iron and calcium carbide, on one hand, lanthanum and cerium elements can form stable compounds with sulfur and oxygen in molten iron, so that the adverse effect of sulfur and oxygen on the graphite spheroidizing process is reduced, and the spheroidizing efficiency is improved; on the other hand, the lanthanum and the cerium are added at the same time, so that the nucleation process of the graphite can be promoted, the graphite can form a spherical structure more easily, the spheroidization of the graphite is facilitated, the effect of improving the spheroidization rate is achieved, and the mechanical property of the prepared iron pipe fitting is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ductile iron, and in particular to a method for preparing a high-silicon solid solution strengthened ferrite ductile iron pipe fitting. Background Art

[0002] Ductile iron is widely used in many industrial fields due to its good mechanical properties, corrosion resistance and cost-effectiveness, especially in the manufacture of pipeline systems. Traditional ductile iron pipe fittings are mainly composed of pearlite matrix, while the high-silicon ductile iron developed in recent years improves its tensile strength and corrosion resistance by increasing the silicon content.

[0003] During the casting process of existing ferritic ductile iron pipe fittings, the graphite spheroidization rate is not high and the microstructure distribution is uneven, which results in that they are usually unable to meet the higher yield strength and tensile strength requirements under working conditions where they need to withstand large external forces, resulting in a shorter service life.

[0004] Therefore, it is necessary to propose a preparation method of high-silicon solid solution strengthened ferrite ductile iron pipe fittings with good mechanical properties to extend their service life. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing a high-silicon solid solution strengthened ferrite ductile iron pipe fitting.

[0006] A method for preparing a high-silicon solid solution strengthened ferrite ductile iron pipe fitting comprises the following steps:

[0007] S1: Preparation of cored wire

[0008] The lanthanum-containing spheroidizing agent and the composite inoculant are wrapped in the steel skin by a winding device to form a cable-shaped wire coil to obtain a spheroidized cored wire and an inoculated cored wire;

[0009] S2: Mixed Melting

[0010] Pig iron, scrap steel and recycled materials are added into a medium frequency induction furnace, and after being fully melted, the temperature is raised to 1500-2000°C, and a carburizer and ferrosilicon are added to obtain mixed molten iron;

[0011] S3: One-time inoculation treatment

[0012] The spheroidized cored wire and the inoculated cored wire are fed into a mixed molten iron ladle with a ladle cover through a wire feeding device to perform spheroidization and primary inoculation treatment to obtain spheroidized cast iron liquid;

[0013] S4: Pouring

[0014] When the temperature of the spheroidized cast iron liquid is reduced to 1420-1480°C, the slag is removed and then poured into a pipe fitting mold. During the pouring process, a flow inoculant is added and then covered with an inoculant alloy for secondary inoculation. The spheroidized cast iron liquid is cooled, solidified and demoulded to obtain a prefabricated pipe fitting.

[0015] S5: Annealing heat treatment

[0016] The prefabricated pipe fittings are annealed at 550-650° C. for 2-4 hours and then cooled to obtain ferrite ductile iron pipe fittings.

[0017] Furthermore, the specific preparation steps of the lanthanum-containing spheroidizing agent are as follows:

[0018] S1.1: Add lanthanum oxide, cerium oxide, magnesium oxide, ferrosilicon and calcium carbide into a mixer, mix thoroughly for 10-20 minutes, add a binder, place in a ball mill, and mix thoroughly to obtain a mixed material;

[0019] S1.2: The above-mentioned mixed material is put into a three-phase electric arc furnace and smelted for 2-3 hours to form an alloy ingot, which is then water-cooled, crushed and sieved to obtain a lanthanum-containing spheroidizer with a particle size of 0.1-0.2 mm.

[0020] Furthermore, the specific preparation steps of the composite inoculant are as follows:

[0021] S2.1: Mix ferroniobium, ferrovanadium and pig iron and put them into a vacuum melting furnace, and melt them at 1500-1600°C for 1-2h to obtain an alloy block;

[0022] S2.2: The alloy block is placed in a crusher for full crushing, and then placed in a water-cooled copper crucible of a vacuum quenching furnace for rapid quenching to obtain a composite inoculant with a thickness of 0.1-0.3 mm.

[0023] Furthermore, the mass fractions of the various elements in the ferrite iron pipe are as follows:

[0024] C: 2.80-3.60%, Si: 3.50-4.60%, Mn≤0.23%, S≤0.0080%, P≤0.025%, 0.06-0.07% Mg, Ba≤0.10%, Sb≤0.009%, V≤0.008%, RE≤0.020%, and the balance is Fe.

[0025] Furthermore, the ratio of pig iron, scrap steel and recycled materials is 10-30wt%: 20wt%: 50-70wt%.

[0026] Furthermore, the main component percentages of the lanthanum-containing spheroidizer are: 42-46% Si, 5.5-6.5% Mg, 2.5-2.9% Ca, 0.45-0.65% RE, and the balance is Fe.

[0027] Furthermore, the main component percentages of the composite inoculant are: 3-5% V, 9-15% Nb, and the balance is Fe.

[0028] Furthermore, the amount of the lanthanum-containing spheroidizer added is 0.9-1.1wt%, and the amount of the composite inoculant added is 0.4-0.6wt%.

[0029] Furthermore, the feeding speed of the spheroidized cored wire and the inoculated cored wire is 20-30 m / min, and the feeding length is 33 m.

[0030] Furthermore, the main component percentages of the inoculant are: 15-35% Ba, 1.4-3.2% Sb, and the balance is Fe, and the added amount of the inoculant is 0.2-0.7wt%.

[0031] Compared with the prior art, the present invention has at least the following beneficial effects:

[0032] 1. The present invention prepares a lanthanum-containing spheroidizing agent by mixing metal oxides such as lanthanum oxide and cerium oxide with reducing agents such as ferrosilicon and calcium carbide, adding a binder for ball milling, and then smelting in a three-phase electric arc furnace. On the one hand, since lanthanum and cerium elements can form stable compounds with sulfur and oxygen in molten iron, the adverse effects of sulfur and oxygen on the spheroidization process of graphite can be reduced, thereby forming a spherical rather than flaky form of graphite. On the other hand, the simultaneous addition of lanthanum and cerium can promote the nucleation process of graphite, making it easier for graphite to form a spherical structure, which is conducive to the spheroidization of graphite, thereby achieving the effect of improving the spheroidization rate, so as to improve the mechanical properties of the obtained iron pipe fittings.

[0033] 2. The present invention prepares a composite inoculant by vacuum melting a mixture of ferroniobium, ferrovanadium, ferrobismuth and pig iron to prepare an alloy block, and then crushes the alloy block and puts it into a water-cooled copper crucible in a vacuum quenching furnace for rapid quenching. Since vanadium and niobium can form stable carbides with carbon, these carbides can be evenly distributed in the matrix during the cooling process and can also serve as the core of grain nucleation, promoting the nucleation process of the grains, increasing the number of grains, reducing the grain size, and achieving the effect of grain refinement, thereby further improving the mechanical properties of the iron pipe fittings. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, further serve to explain the principles of the invention and to enable those skilled in the relevant art to make and use the invention.

[0035] Figure 1 This is a flow chart of the method for preparing high-silicon solid solution strengthened ferrite ductile iron pipe fittings used in an embodiment of the present invention. DETAILED DESCRIPTION

[0036] The following is a detailed description of a method for preparing a high-silicon solid solution strengthened ferrite ductile iron pipe provided by the present invention in conjunction with the accompanying drawings and specific embodiments.

[0037] Example 1

[0038] A method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe fitting, such as Figure 1 As shown, the following steps are included:

[0039] S1: Preparation of cored wire

[0040] The lanthanum-containing spheroidizing agent and the composite inoculant are wrapped in the steel skin by a winding device to form a cable-shaped wire coil to obtain a spheroidized cored wire and an inoculated cored wire;

[0041] The specific preparation steps of the lanthanum-containing spheroidizer are as follows:

[0042] S1.1: Add lanthanum oxide, cerium oxide, magnesium oxide, ferrosilicon and calcium carbide into a mixer, mix thoroughly for 10 minutes, add a binder, place in a ball mill, and mix thoroughly to obtain a mixed material;

[0043] S1.2: The above-mentioned mixed material is put into a three-phase electric arc furnace, smelted for 2 hours, and made into alloy ingots, and then water-cooled, crushed and sieved to obtain a lanthanum-containing nodulizer with a particle size of 0.1 mm. The main components of the lanthanum-containing nodulizer are: 42% Si, 5.5% Mg, 2.5% Ca, 0.45% RE, and the balance is Fe;

[0044] The specific preparation steps of the composite inoculant are as follows:

[0045] S2.1: Mix ferroniobium, ferrovanadium and pig iron and put them into a vacuum melting furnace, and melt them at 1500°C for 1 hour to obtain an alloy block;

[0046] S2.2: The alloy block is placed in a crusher for full crushing, and then placed in a water-cooled copper crucible in a vacuum quenching furnace for rapid quenching to obtain a composite inoculant with a thickness of 0.1 mm. The main components of the composite inoculant are 3% V, 9% Nb, and the balance is Fe;

[0047] S2: Mixed Melting

[0048] Pig iron, scrap steel and recycled materials are added into a medium frequency induction furnace, and after being fully melted, the temperature is raised to 1500°C, and a carburizer and ferrosilicon are added to obtain mixed molten iron, wherein the ratio of pig iron, scrap steel and recycled materials is 10wt%: 20wt%: 70wt%;

[0049] S3: One-time inoculation treatment

[0050] The spheroidized cored wire and the inoculated cored wire are fed into a mixed molten iron ladle with a cover by a wire feeding device, and spheroidized and inoculated once to obtain spheroidized cast iron liquid, wherein the amount of lanthanum-containing spheroidizer added is 0.9wt%, the amount of composite inoculant added is 0.4wt%, and the feeding speed of the spheroidized cored wire and the inoculated cored wire is 20m / min, and the feeding length is 33m;

[0051] S4: Pouring

[0052] When the temperature of the spheroidized cast iron liquid is reduced to 1420° C., the slag is removed and then poured into a pipe fitting mold. During the pouring process, a flow inoculant is added, and then covered with an inoculating alloy, a secondary inoculation treatment is performed, and the mold is cooled and solidified, and demolded to obtain a prefabricated pipe fitting, wherein the main component percentages of the flow inoculant are: 15% Ba, 1.4% Sb, and the balance is Fe, and the amount of the flow inoculant added is 0.2wt%;

[0053] S5: Annealing heat treatment

[0054] The prefabricated pipe fittings are annealed at 550°C for 2h and cooled to obtain ferrite ductile iron pipe fittings, wherein the mass fractions of the various element components in the ferrite iron pipe fittings are as follows:

[0055] C: 2.80%, Si: 3.50%, Mn≤0.23%, S≤0.0080%, P≤0.025%, 0.06% Mg, Ba≤0.10%, Sb≤0.009%, V≤0.008%, RE≤0.020%, and the balance is Fe.

[0056] Example 2

[0057] A method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe fitting, such as Figure 1 As shown, the following steps are included:

[0058] S1: Preparation of cored wire

[0059] The lanthanum-containing spheroidizing agent and the composite inoculant are wrapped in the steel skin by a winding device to form a cable-shaped wire coil to obtain a spheroidized cored wire and an inoculated cored wire;

[0060] The specific preparation steps of the lanthanum-containing spheroidizer are as follows:

[0061] S1.1: Add lanthanum oxide, cerium oxide, magnesium oxide, ferrosilicon and calcium carbide into a mixer, mix thoroughly for 15 minutes, add a binder, place in a ball mill, and mix thoroughly to obtain a mixed material;

[0062] S1.2: The above-mentioned mixed material is put into a three-phase electric arc furnace, smelted for 2.5 hours, and made into an alloy ingot, and then water-cooled, crushed and sieved to obtain a lanthanum-containing nodulizer with a particle size of 0.15 mm. The main components of the lanthanum-containing nodulizer are: 43.7% Si, 6.3% Mg, 2.76% Ca, 0.55% RE, and the balance is Fe;

[0063] The specific preparation steps of the composite inoculant are as follows:

[0064] S2.1: Mix ferroniobium, ferrovanadium and pig iron and put them into a vacuum melting furnace, and melt them at 1550°C for 1.5 hours to obtain an alloy block;

[0065] S2.2: The alloy block is placed in a crusher for full crushing, and then placed in a water-cooled copper crucible in a vacuum quenching furnace for rapid quenching to obtain a composite inoculant with a thickness of 0.2 mm. The main components of the composite inoculant are 4% V, 12% Nb, and the balance is Fe;

[0066] S2: Mixed Melting

[0067] Pig iron, scrap steel and recycled materials are added into a medium frequency induction furnace, and after being fully melted, the temperature is raised to 1750°C, and a carburizer and ferrosilicon are added to obtain mixed molten iron, wherein the ratio of pig iron, scrap steel and recycled materials is 20wt%:20wt%:60wt%;

[0068] S3: One-time inoculation treatment

[0069] The spheroidized cored wire and the inoculated cored wire are fed into a mixed molten iron ladle with a cover by a wire feeding device, and spheroidized and inoculated once to obtain spheroidized cast iron liquid, wherein the amount of the lanthanum-containing spheroidizer added is 1wt%, the amount of the composite inoculant added is 0.5wt%, and the feeding speed of the spheroidized cored wire and the inoculated cored wire is 25m / min, and the feeding length is 33m;

[0070] S4: Pouring

[0071] When the temperature of the spheroidized cast iron liquid is reduced to 1460° C., the slag is removed and then poured into a pipe fitting mold. During the pouring process, a flow inoculant is added, and then covered with an inoculating alloy, a secondary inoculation treatment is performed, and the mold is cooled and solidified, and demolded to obtain a prefabricated pipe fitting, wherein the main component percentages of the flow inoculant are: 25% Ba, 1.8% Sb, and the balance is Fe, and the amount of the flow inoculant added is 0.5wt%;

[0072] S5: Annealing heat treatment

[0073] The prefabricated pipe fittings are annealed at 600°C for 3 hours and cooled to obtain ferrite ductile iron pipe fittings, wherein the mass fractions of the various element components in the ferrite iron pipe fittings are as follows:

[0074] C: 3.25%, Si: 3.97%, Mn≤0.23%, S≤0.0080%, P≤0.025%, 0.064% Mg, Ba≤0.10%, Sb≤0.009%, V≤0.008%, RE≤0.020%, and the balance is Fe.

[0075] Example 3

[0076] A method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe fitting, such as Figure 1 As shown, the following steps are included:

[0077] S1: Preparation of cored wire

[0078] The lanthanum-containing spheroidizing agent and the composite inoculant are wrapped in the steel skin by a winding device to form a cable-shaped wire coil to obtain a spheroidized cored wire and an inoculated cored wire;

[0079] The specific preparation steps of the lanthanum-containing spheroidizer are as follows:

[0080] S1.1: Add lanthanum oxide, cerium oxide, magnesium oxide, ferrosilicon and calcium carbide into a mixer, mix thoroughly for 20 minutes, add a binder, place in a ball mill, and mix thoroughly to obtain a mixed material;

[0081] S1.2: The above-mentioned mixed material is put into a three-phase electric arc furnace, smelted for 3 hours, and made into alloy ingots, and then water-cooled, crushed and sieved to obtain a lanthanum-containing nodulizer with a particle size of 0.2 mm. The main components of the lanthanum-containing nodulizer are: 46% Si, 6.5% Mg, 2.9% Ca, 0.65% RE, and the balance is Fe;

[0082] The specific preparation steps of the composite inoculant are as follows:

[0083] S2.1: Mix ferroniobium, ferrovanadium and pig iron and put them into a vacuum melting furnace, and smelt them at 1600°C for 2h to obtain an alloy block;

[0084] S2.2: The alloy block is placed in a crusher for full crushing, and then placed in a water-cooled copper crucible in a vacuum quenching furnace for rapid quenching to obtain a composite inoculant with a thickness of 0.3 mm. The main components of the composite inoculant are 5% V, 15% Nb, and the balance is Fe;

[0085] S2: Mixed Melting

[0086] Pig iron, scrap steel and recycled materials are added into a medium frequency induction furnace, and after being fully melted, the temperature is raised to 2000°C, and a carburizer and ferrosilicon are added to obtain mixed molten iron, wherein the ratio of pig iron, scrap steel and recycled materials is 30wt%: 20wt%: 50wt%;

[0087] S3: One-time inoculation treatment

[0088] The spheroidized cored wire and the inoculated cored wire are fed into a mixed molten iron ladle with a cover by a wire feeding device, and spheroidized and inoculated once to obtain spheroidized cast iron liquid, wherein the amount of lanthanum-containing spheroidizing agent added is 1.1wt%, the amount of composite inoculant added is 0.6wt%, and the feeding speed of the spheroidized cored wire and the inoculated cored wire is 30m / min, and the feeding length is 33m;

[0089] S4: Pouring

[0090] When the temperature of the spheroidized cast iron liquid is reduced to 1480° C., the slag is removed and then poured into a pipe fitting mold. During the pouring process, a flow inoculant is added, and then covered with an inoculating alloy, a secondary inoculation treatment is performed, and the mold is cooled and solidified, and demolded to obtain a prefabricated pipe fitting, wherein the main component percentages of the flow inoculant are: 35% Ba, 3.2% Sb, and the balance is Fe, and the amount of the flow inoculant added is 0.7wt%;

[0091] S5: Annealing heat treatment

[0092] The prefabricated pipe fittings are annealed at 650°C for 4 hours and cooled to obtain ferrite ductile iron pipe fittings, wherein the mass fractions of the various element components in the ferrite iron pipe fittings are as follows:

[0093] C: 3.60%, Si: 4.60%, Mn≤0.23%, S≤0.0080%, P≤0.025%, 0.07% Mg, Ba≤0.10%, Sb≤0.009%, V≤0.008%, RE≤0.020%, and the balance is Fe.

[0094] Performance Testing:

[0095] The yield strength, tensile strength and elongation of the ferritic ductile iron pipe fittings prepared in Examples 1, 2 and 3 were tested according to the GB / T232-2010 and GB / T16491-1996 electronic universal material testing machine testing standards. The results are shown in Table 1.

[0096] Table 1: Summary of performance test results of Examples 1-3

[0097] Yield strength(MPa) Tensile strength(MPa) Elongation (%) Example 1 444 543 13.9 Example 2 454 547 14.8 Example 3 448 545 14.5

[0098] Comparative Example 1

[0099] The difference between this comparative example 1 and example 1 is that the lanthanum oxide and cerium oxide in step S1.1 are replaced by an equal amount of magnesium oxide, and then the performance test is carried out according to the performance test method of example 1. The results are shown in Table 2 below.

[0100] Comparative Example 2

[0101] The difference between Comparative Example 2 and Example 1 is that the lanthanum oxide in step S1.1 is replaced by an equal amount of cerium oxide, and then the performance test is carried out according to the performance test method of Example 1. The results are shown in Table 2 below.

[0102] Comparative Example 3

[0103] The difference between this comparative example 3 and example 1 is that the cerium oxide in step S1.1 is replaced by an equal amount of lanthanum oxide, and then the performance test is carried out according to the performance test method of example 1. The results are shown in Table 2 below.

[0104] Table 2: Comparison of performance test results of Comparative Examples 1-3 and Example 1

[0105] Yield strength(MPa) Tensile strength(MPa) Elongation (%) Example 1 444 543 13.9 Comparative Example 1 358 417 8.2 Comparative Example 2 395 482 11.1 Comparative Example 3 413 506 11.8

[0106] It can be seen from Table 2 that the yield strength, tensile strength and elongation in Comparative Examples 1-3 are all less than that in Example 1, and the yield strength, tensile strength and elongation of Comparative Examples 2 and 3 are all greater than that of Comparative Example 1. It can be seen that by mixing metal oxides such as lanthanum oxide and cerium oxide with reducing agents ferrosilicon and calcium carbide, adding a binder for ball milling, and then smelting in a three-phase electric arc furnace to prepare a lanthanum-containing spheroidizing agent, on the one hand, lanthanum and cerium elements can form stable compounds with sulfur and oxygen in molten iron, reducing the adverse effects of sulfur and oxygen on the graphite spheroidization process, thereby being able to form a spherical rather than flaky form that helps graphite precipitate. On the other hand, the simultaneous addition of lanthanum and cerium can promote the nucleation process of graphite, making it easier for graphite to form a spherical structure, which is helpful for graphite spheroidization, achieving the effect of improving the spheroidization rate, thereby improving the mechanical properties of the obtained iron pipe fittings.

[0107] Comparative Example 4

[0108] The difference between this comparative example 4 and example 1 is that the composite inoculant in step S1 is replaced by an equal amount of a silicon-calcium-barium inoculant, whose weight percentages are 40% silicon, 1.5% barium, 0.4% calcium, and the remainder is iron. Then, a performance test is carried out according to the performance test method of example 1, and the results are shown in Table 3.

[0109] Table 3: Summary of performance test results of Comparative Example 4 and Example 1

[0110] Yield strength(MPa) Tensile strength(MPa) Elongation (%) Example 1 444 543 13.9 Comparative Example 4 409 484 11.6

[0111] It can be seen from Table 3 that the yield strength, tensile strength and elongation of the iron pipe fittings prepared in Comparative Example 4 are all lower than those in Example 1. It can be seen that by vacuum melting the mixture of ferroniobium, ferrovanadium, ferrobismuth and pig iron to form an alloy block, and then crushing the alloy block and placing it in a water-cooled copper crucible in a vacuum quenching furnace for rapid quenching to prepare a composite inoculant, vanadium and niobium can form stable carbides with carbon, and these carbides can be evenly distributed in the matrix during the cooling process, and can also serve as the core of grain nucleation, promote the nucleation process of the grains, increase the number of grains, reduce the grain size, and achieve the effect of grain refinement, thereby further improving the mechanical properties of the iron pipe fittings.

[0112] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe fitting, characterized in that: The steps include: S1: Preparation of cored wire The lanthanum-containing spheroidizing agent and the composite inoculant are wrapped in the steel skin by a winding device to form a cable-shaped wire coil to obtain a spheroidized cored wire and an inoculated cored wire; S2: Mixed Melting Pig iron, scrap steel and recycled materials are added into a medium frequency induction furnace, and after being fully melted, the temperature is raised to 1500-2000°C, and a carburizer and ferrosilicon are added to obtain mixed molten iron; S3: One-time inoculation treatment The spheroidized cored wire and the inoculated cored wire are fed into a mixed molten iron ladle with a ladle cover through a wire feeding device to perform spheroidization and primary inoculation treatment to obtain spheroidized cast iron liquid; S4: Pouring When the temperature of the spheroidized cast iron liquid is reduced to 1420-1480°C, the slag is removed and then poured into a pipe fitting mold. During the pouring process, a flow inoculant is added and then covered with an inoculant alloy for secondary inoculation. The spheroidized cast iron liquid is cooled, solidified and demoulded to obtain a prefabricated pipe fitting. S5: Annealing heat treatment The prefabricated pipe fittings are annealed at 550-650° C. for 2-4 hours and then cooled to obtain ferrite ductile iron pipe fittings.

2. The method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe according to claim 1, characterized in that: The specific preparation steps of the lanthanum-containing spheroidizer are as follows: S1.1: Add lanthanum oxide, cerium oxide, magnesium oxide, ferrosilicon and calcium carbide into a mixer, mix thoroughly for 10-20 minutes, add a binder, place in a ball mill, and mix thoroughly to obtain a mixed material; S1.2: The above-mentioned mixed material is put into a three-phase electric arc furnace and smelted for 2-3 hours to form an alloy ingot, which is then water-cooled, crushed and sieved to obtain a lanthanum-containing spheroidizer with a particle size of 0.1-0.2 mm.

3. The method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe according to claim 2, characterized in that: The specific preparation steps of the composite inoculant are as follows: S2.1: Mix ferroniobium, ferrovanadium and pig iron and put them into a vacuum melting furnace, and smelt them at 1500-1600°C for 1-2h to obtain an alloy block; S2.2: The alloy block is placed in a crusher for full crushing, and then placed in a water-cooled copper crucible of a vacuum rapid quenching furnace for rapid quenching to obtain a composite inoculant with a thickness of 0.1-0.3 mm.

4. The method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe according to claim 1, characterized in that: The mass fractions of each element in ferrite iron pipe fittings are as follows: C: 2.80-3.60%, Si: 3.50-4.60%, Mn≤0.23%, S≤0.0080%, P≤0.025%, 0.06-0.07% Mg, Ba≤0.10%, Sb≤0.009%, V≤0.008%, RE≤0.020%, and the balance is Fe.

5. The method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe according to claim 1, characterized in that: The ratio of pig iron, scrap steel and recycled materials is 10-30wt%: 20wt%: 50-70wt%.

6. The method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe fitting according to claim 2, characterized in that: The main component percentages of the lanthanum-containing spheroidizer are: 42-46% Si, 5.5-6.5% Mg, 2.5-2.9% Ca, 0.45-0.65% RE, and the balance is Fe.

7. The method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe according to claim 3, characterized in that: The main component percentages of the composite inoculant are: 3-5% V, 9-15% Nb, and the balance is Fe.

8. The method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe according to claim 3, characterized in that: The amount of the lanthanum-containing spheroidizer added is 0.9-1.1wt%, and the amount of the composite inoculant added is 0.4-0.6wt%.

9. The method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe fitting according to claim 1, characterized in that: The feeding speed of spheroidized cored wire and inoculated cored wire is 20-30m / min, and the feeding length is 33m.

10. The method for preparing a high silicon solid solution strengthened ferrite ductile iron pipe according to claim 1, characterized in that: The main component percentages of the inoculant are: 15-35% Ba, 1.4-3.2% Sb, and the balance is Fe, and the added amount of the inoculant is 0.2-0.7wt%.