Efficient comprehensive recovery method for copper-cadmium slag

By using continuous reactors and powdered metal zinc particles in the copper cadmium slag recovery process, the enrichment of copper cadmium slag and slurry blowing oxidation treatment of sponge cadmium, the existing process has been solved with small processing capacity and low oxidation efficiency in the existing process. The problem is that efficient copper cadmium slag recycling has been achieved, reducing zinc powder unit consumption and occupational health risks.

CN119040650APending Publication Date: 2024-11-29BAIYIN NONFERROUS GROUP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411151391.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing copper cadmium slag recycling process has problems such as small intermittent leaching processing capacity of single tanks, low oxidation efficiency of sponge cadmium natural storage, high zinc powder unit consumption, and occupational health risks.

Method used

The continuous reactor is used to enrich the copper-cadmium slag, and the powdered metal zinc particles are replaced by a one-time replacement. Combined with the slurry blowing oxidation process of sponge cadmium, the efficient comprehensive recovery of copper-cadmium slag is achieved.

Benefits of technology

It improves the treatment efficiency of copper cadmium slag, reduces labor intensity and zinc powder use, improves the recovery rate of valuable metals, reduces occupational health risks, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040650A_ABST
    Figure CN119040650A_ABST
Patent Text Reader

Abstract

The invention discloses an efficient comprehensive recovery method for copper-cadmium slag, and relates to the technical field of hydrometallurgy, and the method comprises the steps of copper-cadmium slag continuous enrichment, sponge cadmium preparation through primary replacement, sponge cadmium oxidation enrichment, cadmium ingot preparation through secondary replacement and the like. According to the method, the continuous reaction kettle is used for enriching copper and cadmium, the powdery metal zinc particles are used for replacing traditional zinc powder for one-time replacement to prepare sponge cadmium, the slurrying blast oxidation process of the sponge cadmium is creatively applied, and through the method, the copper-cadmium slag treatment efficiency is improved by 20%, the copper content of the copper slag exceeds 75%, the cadmium content of the cadmium-poor liquid is lower than 1 g / L, and the percent of pass exceeds 90%; according to the method, enrichment of cadmium in a purification system is remarkably reduced, efficient comprehensive recovery of the copper-cadmium slag is achieved, and the method is low in safety risk, small in investment and suitable for industrial application and has obvious economic benefits and popularization value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrometallurgy, and more specifically to a method for efficiently and comprehensively recovering copper-cadmium slag. Background Art

[0002] In the hydrometallurgical zinc smelting process, the supernatant produced by the leaching process needs to be purified to remove harmful impurities such as copper, cadmium, cobalt, and nickel to ensure that its content meets the requirements of the electrolytic process. The slag produced during the purification process contains considerable valuable metals. In order to improve the economic benefits and profitability of the company, many companies will further process these slags to recover valuable metals such as cadmium, zinc, and cobalt. This practice not only improves the utilization rate of resources, but also helps reduce environmental pollution and achieve sustainable development.

[0003] In the comprehensive recovery process of valuable metals, enterprises generally adopt traditional processing technology, including single-tank intermittent leaching of copper-cadmium slag, primary replacement, natural storage oxidation of sponge cadmium, secondary replacement and smelting process. However, these traditional processes face some bottleneck problems in actual production, such as small processing capacity of single-tank intermittent leaching, low efficiency of natural storage oxidation of sponge cadmium, long cycle, high unit consumption of zinc powder, high labor intensity and environmental problems that may affect the health of employees. In order to improve efficiency and safety, it is necessary to improve and optimize the existing process. Summary of the invention

[0004] The purpose of the present invention is: in view of the above-mentioned technical problems, the present invention provides a high-efficiency comprehensive recovery method of copper-cadmium slag to solve the existing problems such as small intermittent leaching treatment capacity of a single tank, low natural storage oxidation efficiency of sponge cadmium, high unit consumption of zinc powder and health hazards of employees.

[0005] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:

[0006] A method for efficiently and comprehensively recovering copper-cadmium slag is mainly achieved by the following steps:

[0007] (1) Continuous enrichment of copper and cadmium in copper-cadmium slag: First, the purified copper-cadmium slag is ground by a ball mill or a slurry tank, and mixed with water or purified residual liquid to form a slurry. The slurry is sent to the copper-cadmium slag slurry storage tank, and then quantitatively pumped into a continuous reactor to enrich copper and cadmium. After the enrichment is completed, the crude copper slag and cadmium-rich liquid are obtained by filter pressing. The crude copper slag is further enriched with copper by acid washing and water washing to obtain high-grade copper slag, which is sold externally, and the cadmium-rich liquid enters the next step.

[0008] (2) Primary replacement and preparation of sponge cadmium: Use powdered zinc metal particles to carry out a primary replacement reaction on the cadmium-rich liquid to prepare sponge cadmium. After the replacement, the sponge cadmium and the filtrate are separated by filtration, of which the sponge cadmium enters the subsequent treatment and the filtrate is returned to the zinc system.

[0009] (3) Oxidation and enrichment of sponge cadmium: The sponge cadmium is slurried and oxidized by air blowing, then acid dissolved and filtered to obtain a cadmium-rich liquid for the secondary replacement process, and the filter residue is returned to the copper slag recovery process.

[0010] (4) Secondary replacement and preparation of cadmium ingots: The cadmium-rich solution is subjected to secondary zinc powder replacement treatment to remove cadmium, obtaining cadmium cotton pellets, which are then smelted into cadmium ingots for sale.

[0011] Preferably, in the step (1) of purifying the copper-cadmium slag, the slag is ground in a ball mill or a slurry tank to a particle size of 120-160 mesh ≥ 80%, and mixed with water or purified residual liquid to form a slurry. The slurry is then transported to a copper-cadmium slurry storage tank at a rate of 12m 3 / h~15m 3 / h rate quantitatively fed into the continuous reactor to enrich copper and cadmium. During the enrichment process, a mixture of industrial-grade 98% concentrated sulfuric acid and produced water is used as a solvent, the liquid-solid ratio of the solvent to the slurry is controlled at 3:1-4:1, the process temperature is 80-85°C, the reaction time is 150min-200min, the stirring speed is 80-85r / min, and when the end point pH value is 1.5-2.0 and is maintained for a long time, the initial enrichment process of copper and cadmium is completed. The filter is pressed, and the filtrate enters the cadmium recovery system. The filter residue is pickled with a liquid-solid ratio of 4:1, Ph2.0-2.5, a temperature of 82-85°C, and a reaction of 150min. It is washed with water with a liquid-solid ratio of 3:1, Ph2.5-3.0, a temperature of 75-80°C, and a reaction of 120min. High-grade copper slag is obtained by filter pressing and sold, and the filtrate is returned to the zinc recovery system.

[0012] Preferably, in the step (2), the control conditions for the replacement of cadmium and the preparation of sponge cadmium are as follows: the front liquid Zn130+5g / L, Cd≥10g / L, Ph 2.5-3.0, the rear liquid Cd≤1g / L, Ph: 3.0-3.5, the powdered metal zinc particles (kg) = the volume of the front liquid (m 3 )× cadmium content in liquid before replacement (g / L)×1.4 times theoretical coefficient, the replacement reaction time is controlled at 20-30min. When the cadmium sponge is observed to be smoke-gray flocculent, it can aggregate and settle naturally, indicating that the replacement reaction is complete. Then the filter press operation is performed, and the filter residue obtained is the sponge cadmium, and the filtrate is returned to the zinc recovery system.

[0013] Preferably, in step (3), the oxidation and enrichment process of sponge cadmium includes mixing sponge cadmium with water, controlling the particle size to 60-80 mesh ≥ 80%, and maintaining the liquid-solid ratio to 3:1-4:1. The mixture is stirred in a slurry tank at a stirring speed of 60r / min, and then subjected to air blast oxidation, and the air volume is controlled at 6-8m 3 / h, and the blast oxidation time lasts for 120-150min. The slurry after oxidation will be used in the subsequent steps.

[0014] Preferably, in step (4), the oxidized slurry obtained in step (3) is used for secondary replacement and preparation of cadmium ingots. First, the oxidized slurry is sent to a cadmium cotton acid dissolution reactor, and 98% sulfuric acid and water are added for acid dissolution. The acid dissolution reaction is carried out at a temperature of 70-80°C, the pH value is controlled at 2.0-2.5, and the reaction time is 3-4h. Subsequently, pressure filtration is carried out, and the resulting filter residue is returned to the copper slag system, and zinc powder is added to the filtrate for secondary replacement to prepare cadmium cotton pressed balls. Amount of zinc powder (kg) = volume of liquid before replacement (m 3 )× cadmium content in liquid before replacement (g / L)×0.5 (theoretical coefficient). The secondary replacement adopts a cyclic replacement method, by adding zinc powder in small amounts multiple times to ensure the full reaction and complete replacement of cadmium. After 20-30 minutes of reaction, when the cadmium wool is observed to be smoky gray flocs, can clump and settle naturally, it indicates that the secondary replacement reaction is complete. Next, by opening the secondary replacement bottom flow valve, the cadmium wool is collected and the subsequent pressing and smelting ingot operations are carried out.

[0015] Preferably, in step (2), the powdered metallic zinc particles are the product of a redox reaction between the cathode zinc (zinc skin) and the air during the process of melting the cathode zinc (zinc skin) into zinc liquid and casting it into zinc ingots, and then sieving the product.

[0016] Preferably, in step (4), the secondary replacement zinc powder is electric furnace blown zinc powder (60 mesh-80 mesh), purchased from outside or prepared in the company's own zinc powder workshop.

[0017] Preferably, the above-mentioned industrial 98% sulfuric acid is a by-product of the acid-making process of a hydrometallurgical zinc smelting enterprise and does not need to be purchased from outside.

[0018] Preferably, the heating source for the above-mentioned leaching and acid dissolution process can be provided by the waste heat steam from the roasting furnace of the wet zinc smelting enterprise, without the need for external purchase.

[0019] The present invention achieves efficient and comprehensive recovery of copper-cadmium slag by using a continuous reactor to enrich copper and cadmium, using powdered metal zinc particles to replace traditional zinc powder for one-time replacement to produce sponge cadmium, and innovatively using the slurry blast oxidation process of sponge cadmium. The main advantages of this method include: 1. The continuous reactor has a large processing capacity, higher efficiency, and greatly reduces labor intensity. 2. The continuous reactor provides a more stable reaction environment, which is conducive to the effective enrichment of copper and cadmium. 3. Powdered metal zinc particles replace zinc powder, which not only saves the amount of zinc powder used, but also improves the overall recovery rate of zinc. 4. Compared with natural stockpiling oxidation, the slurry oxidation process of sponge cadmium has higher efficiency and lower labor intensity, while reducing occupational health and safety risks. 5. The method is simple and reliable to operate, very suitable for industrial production, and has significant economic potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1The present invention discloses a flow chart of a method for efficiently and comprehensively recovering copper-cadmium slag. DETAILED DESCRIPTION

[0021] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The exemplary embodiments and descriptions of the present invention are used to explain the present invention, but are not intended to limit the present invention.

[0022] Example 1

[0023] Raw materials: first-stage purified slag, Zn 42.26%, Cd 5.87%, Cu 12.4%, H2O 24%.

[0024] (1) Pretreatment of copper-cadmium slag and preparation of cadmium liquid: The purified copper-cadmium slag is ground to 80-160 mesh ≥ 80% by ball mill or slurry tank, and mixed with water or purified residual liquid to form slag slurry. The slag slurry is then transported to the copper-cadmium slag storage tank at a rate of 13-15m 3 / h rate to the continuous reactor to enrich copper and cadmium, 98% sulfuric acid was added to fine-tune the acidity during the enrichment process, the liquid-solid ratio was controlled at 4:1, the temperature was 83°C, the stirring speed was 83r / min, and when the end pH value reached 2.0, the initial enrichment process of copper-cadmium slag was completed, and the filtrate was filtered and entered the cadmium recovery system (Zn 2+ 132.25g / L, Cd 2+ 12.3g / L), filtrate and residue acid wash liquid solid ratio 4:1, Ph2.0, temperature 83℃, reaction 150min, water wash liquid solid ratio 3:1, Ph2.5, temperature 78℃, reaction 120min, filter press to obtain high copper slag (Zn 3.44%, Cd 0.89%, Cu 76.19%), filtrate (Zn 2+ 9.72g / L, Cd 2+ 0.38g / L) returns to the zinc recovery system.

[0025] (2) One-time replacement cadmium removal and sponge cadmium preparation, the pre-replacement liquid Zn 132.25g / L, Cd 12.3g / L, Ph 2.5, powdered metal particles 17.2 (g / L) reaction for 25min. It was observed that the cadmium sponge showed a smoky gray flocculent, which could aggregate and settle naturally, and the replacement reaction was completed. Then a filter press operation was performed to obtain a one-time replacement sponge cadmium, and the filtrate (Cd≤0.88g / L, Ph: 3.5) was returned to the zinc recovery system.

[0026] (3) Oxidation and enrichment of primary sponge cadmium: the sponge cadmium was mixed with water at a liquid-to-solid ratio of 3:1. The mixture was stirred in a slurry tank at a stirring speed of 83 r / min, and the particle size was controlled at 60-80 mesh ≥ 80%. Then, air blast oxidation was performed with an air volume of 6.3 m 3 / h, the oxidation time lasts for 120min, and the slurry after oxidation will be used in the subsequent steps.

[0027] (4) The oxidation slurry is subjected to secondary replacement and preparation of cadmium ingots. The oxidation slurry is sent to the cadmium wool acid dissolution reactor, and 98% sulfuric acid is added for acid dissolution. The acid dissolution reaction is carried out at a temperature of 75°C, the pH value reaches 2.5, and the reaction is carried out for 3.5 hours. Then, the filter is pressed, and the obtained filter residue is returned to the copper slag system, and the filtrate (Cd28.6g / L) is added with zinc powder for secondary replacement to remove cadmium, and 14.3g / L of zinc powder is added. The secondary replacement adopts a cyclic replacement method, and zinc powder is added in small amounts multiple times to ensure the full reaction and complete replacement of cadmium. After reacting for 25 minutes, it is observed that the cadmium wool presents a smoke-gray flocculent, which can be lumped and naturally settled, and the secondary replacement reaction is completed. Open the secondary replacement bottom flow valve, collect the cadmium wool and carry out subsequent pressing and smelting ingot operations.

[0028] The results show that: by using the above method, the copper-cadmium slag treatment efficiency is increased by 22%, the copper slag contains 76.19% copper, the cadmium-lean liquid contains 0.88g / L cadmium, the enrichment of cadmium in the purification system is significantly reduced, and 180 tons of zinc powder are saved annually.

[0029] Example 2

[0030] Raw materials: first-stage purified slag, Zn 41.98%, Cd 6.02%, Cu 12.6%, H2O 26%.

[0031] (1) Pretreatment of copper-cadmium slag and preparation of cadmium liquid: The purified copper-cadmium slag is ground to 80-160 mesh ≥ 80% by ball mill or slurry tank, and mixed with water or purified residual liquid to form slag slurry. The slag slurry is then transported to the copper-cadmium slag storage tank at a rate of 13-15m 3 / h rate to the continuous reactor to enrich copper and cadmium, 98% sulfuric acid was added to fine-tune the acidity during the enrichment process, the liquid-solid ratio was controlled at 3:1, the temperature was 82°C, the stirring speed was 83r / min, and when the end pH value reached 1.5, the initial enrichment process of copper-cadmium slag was completed, and the filtrate was filtered and entered the cadmium recovery system (Zn 2+ 131.77 g / L, Cd 2+ 11.8g / L), the filtrate and residue acid wash liquid solid ratio 4:1, Ph2.0, temperature 83℃, reaction 150min, water wash liquid solid ratio 3:1, Ph2.5, temperature 77℃, reaction 120min, filter pressure to obtain high copper slag (Zn 3.58%, Cd 0.87%, Cu 75.47%), sold outside, the filtrate returned to the zinc recovery system (Zn 2+ 10.18 g / L, Cd 2+ 0.29g / L,).

[0032] (2) One-time replacement cadmium removal and sponge cadmium preparation, the pre-replacement liquid Zn 131.77g / L, Cd ≥ 11.8g / L, Ph 2.5, powdered metal particles 16.5 (g / L) reaction time 25min. It was observed that the cadmium sponge showed a smoky gray flocculent, which could aggregate and settle naturally, and the replacement reaction was completed. Then a filter press operation was performed to obtain a one-time replacement sponge cadmium, and the filtrate (Cd ≤ 0.89g / L, Ph: 3.5) was returned to the zinc recovery system.

[0033] (3) Oxidation and enrichment of primary sponge cadmium: the sponge cadmium was mixed with water at a liquid-to-solid ratio of 3:1. The mixture was stirred in a slurry tank at a stirring speed of 83 r / min, and the particle size was controlled at 60-80 mesh ≥ 80%. Then, air blast oxidation was performed at an air volume of 6.5 m 3 / h, the oxidation time lasts for 120min, and the slurry after oxidation will be used in the subsequent steps.

[0034] (4) The oxidation slurry is subjected to secondary replacement and preparation of cadmium ingots. The oxidation slurry is sent to the cadmium wool acid dissolution reactor, and 98% sulfuric acid is added for acid dissolution. The acid dissolution reaction is carried out at a temperature of 75°C, the pH value reaches 2.5, and the reaction is carried out for 3.5 hours. Then, the filter is pressed, and the resulting filter residue is returned to the copper slag system, and the filtrate (Cd26.8g / L) is added with zinc powder for secondary replacement to remove cadmium, and 13.6g / L of zinc powder is added. The secondary replacement adopts a cyclic replacement method, and zinc powder is added in small amounts multiple times to ensure the full reaction and complete replacement of cadmium. After 25 minutes of reaction, it is observed that the cadmium wool presents a smoke-gray flocculent. When it can clump and settle naturally, the secondary replacement reaction is completed. Open the secondary replacement bottom flow valve, collect the cadmium wool and carry out subsequent pressing and smelting ingot operations.

[0035] The results show that by using the above method, the copper-cadmium slag treatment efficiency is increased by 23%, the output copper slag contains 75.47% copper, the cadmium-lean liquid contains 0.89g / L cadmium, which significantly reduces the enrichment of cadmium in the purification system and saves 185 tons of zinc powder annually.

[0036] Example 3

[0037] Raw materials: first-stage purified slag, Zn 41.56%, Cd 6.06%, Cu 13.2%, H2O 25%.

[0038] (1) Pretreatment of copper-cadmium slag and preparation of cadmium liquid: The purified copper-cadmium slag is ground to 80-160 mesh ≥ 80% by ball mill or slurry tank, and mixed with water or purified residual liquid to form slag slurry. The slag slurry is then transported to the copper-cadmium slag storage tank at a rate of 13-15m 3 / h rate to the continuous reactor to enrich copper and cadmium, 98% sulfuric acid was added to fine-tune the acidity during the enrichment process, the liquid-solid ratio was controlled at 4:1, the temperature was 84°C, the stirring speed was 83r / min, and when the end pH value reached 2.0, the initial enrichment process of copper-cadmium slag was completed, and the filtrate was filtered and entered the cadmium recovery system (Zn 2+ 130.44 g / L, Cd 2+ 10.8g / L), the filtrate and residue acid wash liquid solid ratio 4:1, Ph2.0, temperature 84℃, reaction 150min, water wash liquid solid ratio 4:1, Ph2.5, temperature 78℃, reaction 120min, filter pressure to obtain high copper slag (Zn 3.8%, Cd 0.9%, Cu 75.4%), sold outside, the filtrate returned to the zinc recovery system (Zn 2+ 9.8g / L, Cd 2+ 0.30g / L,).

[0039] (2) One-time replacement cadmium removal and sponge cadmium preparation, the pre-replacement liquid Zn 131.75g / L, Cd ≥ 10.9g / L, Ph 2.5, powdered metal particles 15.6 (g / L) reaction time 25min. It was observed that the cadmium sponge showed a smoky gray flocculent, which could aggregate and settle naturally, and the replacement reaction was completed. Then a filter press operation was performed to obtain a one-time replacement sponge cadmium, and the filtrate (Cd ≤ 0.9g / L, Ph: 3.5) was returned to the zinc recovery system.

[0040] (3) Oxidation and enrichment of primary sponge cadmium: the sponge cadmium was mixed with water at a liquid-to-solid ratio of 3:1. The mixture was stirred in a slurry tank at a stirring speed of 83 r / min, and the particle size was controlled at 60-80 mesh ≥ 80%. Then, air blast oxidation was performed at an air volume of 6.5 m 3 / h, the oxidation time lasts for 120min, and the slurry after oxidation will be used in the subsequent steps.

[0041] (4) The oxidation slurry is subjected to secondary replacement and preparation of cadmium ingots. The oxidation slurry is sent to the cadmium wool acid dissolution reactor, and 98% sulfuric acid is added for acid dissolution. The acid dissolution reaction is carried out at a temperature of 76°C, the pH value reaches 2.5, and the reaction is carried out for 3.5 hours. Then, the filter press is performed, and the obtained filter residue is returned to the copper slag system, and the filtrate (28.9g / L) is added with zinc powder for secondary replacement to remove cadmium, and 14.5g / L of zinc powder is added. The secondary replacement adopts a cyclic replacement method, and zinc powder is added in small amounts multiple times to ensure the full reaction and complete replacement of cadmium. After 25 minutes of reaction, it is observed that the cadmium wool presents a smoke-gray flocculent. When it can clump and settle naturally, the secondary replacement reaction is completed. Open the secondary replacement bottom flow valve, collect the cadmium wool and carry out subsequent pressing and smelting ingot operations.

[0042] The results show that by using the above method, the copper-cadmium slag treatment efficiency is increased by 23.5%, the output copper slag contains 75.4% copper, the cadmium-lean liquid contains 0.9g / L cadmium, which significantly reduces the enrichment of cadmium in the purification system and saves 190 tons of zinc powder annually.

[0043] The technical solutions provided by the embodiments of the present invention are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the embodiments of the present invention. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present invention. At the same time, for those skilled in the art, according to the embodiments of the present invention, there may be changes in the specific implementation methods and application scopes. In summary, the contents of this specification should not be understood as limiting the present invention.

Claims

1. A method for efficiently and comprehensively recovering copper-cadmium slag, comprising the following steps: (1) Continuous enrichment of copper and cadmium in copper-cadmium slag: First, the purified copper-cadmium slag is ground by a ball mill or a slurry tank, and mixed with water or purified residual liquid to form a slag slurry; the slag slurry is sent to a copper-cadmium slag slurry storage tank, and then quantitatively pumped into a continuous reactor to enrich copper and cadmium. After the enrichment is completed, the crude copper slag and cadmium-rich liquid are obtained by filter pressing. The crude copper slag is further enriched with copper by acid washing and water washing to obtain high-grade copper slag, which is sold externally, and the cadmium-rich liquid enters the next step; (2) Primary replacement and preparation of sponge cadmium: a primary replacement reaction is carried out on the cadmium-rich liquid using powdered zinc metal particles to prepare sponge cadmium; after the replacement, the sponge cadmium and the filtrate are separated by filtration, wherein the sponge cadmium enters the subsequent treatment and the filtrate is returned to the zinc system; (3) Oxidation and enrichment of sponge cadmium: The sponge cadmium is slurried and oxidized by air blast, then acid-dissolved, and filtered to obtain a cadmium-rich liquid to enter the secondary replacement process, and the filter residue is returned to the copper slag recovery process; (4) Secondary replacement and preparation of cadmium ingots: The cadmium-rich solution is subjected to secondary zinc powder replacement treatment to remove cadmium, obtaining cadmium cotton pellets, which are then smelted into cadmium ingots for sale.

2. A method for efficient comprehensive recovery of copper-cadmium slag according to claim 1, characterized in that: In the step (1) of purifying the copper-cadmium slag, the slag is ground by a ball mill or a slurry tank to a particle size of 120-160 mesh ≥ 80%, and mixed with water or purified residual liquid to form a slurry; the slurry is then transported to a copper-cadmium slurry storage tank at a rate of 12m 3 / h~15m 3 / h rate quantitatively fed into the continuous reactor to enrich copper and cadmium. During the enrichment process, a mixture of industrial-grade 98% concentrated sulfuric acid and produced water is used as a solvent, the liquid-solid ratio of the solvent to the slurry is controlled at 3:1-4:1, the process temperature is 80-85°C, the reaction time is 150min-200min, the stirring speed is 80-85r / min, and when the end point pH value is 1.5-2.0 and is maintained for a long time, the initial enrichment process of copper and cadmium is completed. The filter is pressed, and the filtrate enters the cadmium recovery system. The filter residue is pickled with a liquid-solid ratio of 4:1, Ph2.0-2.5, a temperature of 82-85°C, and a reaction of 150min. It is washed with water with a liquid-solid ratio of 3:1, Ph2.5-3.0, a temperature of 75-80°C, and a reaction of 120min. High-grade copper slag is obtained by filter pressing and sold, and the filtrate is returned to the zinc recovery system.

3. A method for efficient comprehensive recovery of copper-cadmium slag according to claim 1, characterized in that: In the step (2), the cadmium removal by substitution and the preparation of sponge cadmium are controlled under the following conditions: the front liquid Zn 130+5g / L, Cd≥10g / L, Ph 2.5-3.0, the rear liquid Cd≤1g / L, Ph: 3.0-3.5, the powdered metal zinc particles (kg) = the volume of the front liquid (m 3 )× cadmium content in the liquid before replacement (g / L)×1.4 times the theoretical coefficient, the replacement reaction time is controlled at 20-30min; when the cadmium sponge is observed to be smoky gray flocs that can aggregate and settle naturally, it indicates that the replacement reaction is completed; then a filter press operation is performed, and the filter residue obtained is sponge cadmium, and the filtrate is returned to the zinc recovery system.

4. A method for efficient comprehensive recovery of copper-cadmium slag according to claim 1, characterized in that: In the step (2), the powdered metal zinc particles are the products of the oxidation-reduction reaction of the zinc liquid in contact with air during the process of melting the cathode zinc (zinc skin) into zinc liquid and casting it into zinc ingots, and then sieving.

5. The method for efficient comprehensive recovery of copper-cadmium slag according to claim 1, characterized in that: In the step (3), the oxidation and enrichment process of the sponge cadmium includes mixing the sponge cadmium with water, controlling the particle size to 60-80 mesh ≥ 80%, and maintaining the liquid-solid ratio to 3:1-4:1; stirring the mixture in a slurry tank at a stirring speed of 60r / min, and then performing blown oxidation, and the blown air volume is controlled at 6-8m 3 / h, and the blast oxidation time lasts for 120-150min; the slurry after oxidation will be used in subsequent steps.

6. The method for efficient comprehensive recovery of copper-cadmium slag according to claim 1, characterized in that: In the step (4), the oxidation slurry obtained in the step (3) is used for secondary replacement and preparation of cadmium ingots; first, the oxidation slurry is sent to a cadmium cotton acid dissolution reaction kettle, and 98% sulfuric acid and water are added for acid dissolution; the acid dissolution reaction is carried out at a temperature of 70-80°C, the pH value is controlled at 2.0-2.5, and the reaction time is 3-4h; then, pressure filtration is carried out, and the obtained filter residue is returned to the copper slag system, and zinc powder is added to the filtrate for secondary replacement to prepare cadmium cotton pressed agglomerates; the amount of zinc powder (kg) = the volume of the liquid before replacement (m 3 )× cadmium content in the liquid before replacement (g / L)×0.5 (theoretical coefficient); the secondary replacement adopts a cyclic replacement method, by adding zinc powder in small amounts multiple times to ensure the full reaction and complete replacement of cadmium; after 20-30 minutes of reaction, when the cadmium wool is observed to appear as smoky gray flocs that can clump and settle naturally, it indicates that the secondary replacement reaction is complete; next, by opening the secondary replacement bottom flow valve, the cadmium wool is collected and subsequent agglomeration and smelting operations are carried out.

7. The method for efficient comprehensive recovery of copper-cadmium slag according to claim 1, characterized in that: In the step (4), the secondary replacement zinc powder is electric furnace blown zinc powder (60 mesh-80 mesh).

Citation Information

Cited By

  • Method for preparing fine cadmium from sponge cadmium

    CN122773129A