Low-density cobalt-based high-temperature alloy and preparation method thereof

By adding elements such as Ti, V, Nb, Ni to the cobalt-based high-temperature alloy and vacuum smelting and heat treatment, a two-phase co-uniform structure of γ'/γ is formed, which solves the problems of high density and insufficient high-temperature performance of Ni-based high-temperature alloy. A cobalt-based high-temperature alloy with low density and excellent high-temperature performance is achieved.

CN119040698APending Publication Date: 2024-11-29JIANGSU UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411149436.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The density of existing Ni-based high-temperature alloys is limited, which limits its application in aviation materials, and its melting point has reached the upper limit, making it difficult to further improve high-temperature performance.

Method used

Combining elements such as Ti, V, Nb, Ni and Co with Co, it prepares a cobalt-based high-temperature alloy with a density of less than 8.5g·cm-3, and forms γ'/ by vacuum smelting and heat treatment (solid solution treatment and aging treatment) through vacuum smelting and heat treatment (solid solution treatment and aging treatment) to form γ'/ The γ two-phase co-grid structure improves the mechanical properties of the alloy.

Benefits of technology

The low density and good high-temperature mechanical properties of cobalt-based high-temperature alloys are achieved, and the lightweight and performance requirements of modern industry are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040698A_ABST
    Figure CN119040698A_ABST
Patent Text Reader

Abstract

The invention discloses a low-density cobalt-based high-temperature alloy and a preparation method thereof. The high-temperature alloy material is prepared by mixing the following components in percentage by atom: 4-6% of Ti; 9%-11% of V; 0.2 to 2 percent of Nb; 5%-20% of Ni; and the balance of Co. The cobalt-based high-temperature alloy is low in density, the density of the cobalt-based high-temperature alloy is not higher than 8.5 g.cm <-3 >, and the cobalt-based high-temperature alloy has good mechanical properties at high temperature; therefore, the requirements of light weight and more excellent high-temperature performance of the high-temperature material in the modern industry can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a low-density cobalt-based high-temperature alloy and also to a preparation method of the cobalt-based high-temperature alloy. Background Art

[0002] High-temperature alloys are irreplaceable key materials used in the manufacture of high-temperature components in aircraft engines and gas turbines. Currently, Ni-based high-temperature alloys with γ / γ' two-phase coherent strengthening are widely used, but the melting point of Ni is 1455℃. The service temperature of the most mature and widely used nickel-based high-temperature alloys has reached the upper limit of their melting point, so it is necessary to further explore a new type of high-temperature alloy. The melting point of Co is 40℃ higher than that of Ni, so Co-based high-temperature alloys are expected to replace Ni-based high-temperature alloys and become a new generation of high-temperature structural materials.

[0003] The Co-Al-W based alloy has a high density of 9.8 g·cm due to its high W content. -3 , which makes it unsuitable for manufacturing aviation materials. The density of Co-Ti-Cr high-temperature alloy is about 14% lower than that of Co-Al-W. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a low-density cobalt-based high-temperature alloy, which not only has low density but also has good mechanical properties at high temperatures; another purpose of the present invention is to provide a method for preparing the above-mentioned cobalt-based high-temperature alloy.

[0005] Technical solution: The low-density cobalt-based high-temperature alloy material of the present invention is mixed with the following components in atomic percentage: Ti: 4-6%; V: 9-11%; Nb: 0.2-2%; Ni: 5-20%; and the balance is Co.

[0006] The microscopic morphology of the cobalt-based high-temperature alloy prepared by the present invention is as follows: the γ' strengthening phase is cubic, and the matrix channel γ phase in the middle of the γ' strengthening phase is relatively narrow.

[0007] The density of the cobalt-based high-temperature alloy is not higher than 8.5 g·cm -3 .

[0008] The preparation method of the above-mentioned cobalt-based high-temperature alloy is specifically as follows: it includes heat treatment; the heat treatment includes solution treatment and aging treatment; the temperature of the solution treatment is 1100-1150°C, and the treatment time is 48-50h; the temperature of the aging treatment is 850-900°C, and the treatment time is 48-72h.

[0009] The temperature of the solution treatment is 1100°C, and the treatment time is 48h; the temperature of the aging treatment is 870°C, and the treatment time is 72h.

[0010] Among them, before the heat treatment, it also includes a pretreatment step of the metal raw materials and a vacuum melting step; the vacuum melting includes vacuum arc melting and vacuum induction melting.

[0011] The pretreatment of the metal raw materials is specifically as follows: before smelting, the metal raw materials are polished or pickled to remove surface oxide scale.

[0012] The pickling solution includes the following components in volume fractions: 4-5% HCl, 4-5% H2SO4 and 90-95% H2O.

[0013] The vacuum arc melting is specifically as follows: the formulated amount of Co, Ti, V, Nb, and Ni metal raw materials are pre-loaded into the crucible of the melting furnace, with the powdered metal at the bottom and the block metal at the top; the pressure in the melting furnace is pumped down to 0.1-0.15 bar, and then high-purity argon gas is introduced, the current is first adjusted to 50-60A, the arc is started on the tungsten electrode protruding from the crucible in the sample chamber, and then the current is adjusted to 300-320A, and the alloy is melted in the argon atmosphere.

[0014] After each smelting, the cooled alloy is turned over and then smelted again; the number of times of turning over and smelting is more than 5 times.

[0015] Among them, vacuum induction melting is specifically as follows: pre-load the formulated amount of Co, Ti, V, Nb, and Ni metal raw materials into the crucible of the melting furnace, turn on the cooling water system and the vacuum system, and evacuate the melting chamber to make the vacuum degree less than 5Pa; start the induction heating power supply to gradually melt the metal in the crucible to form a complete molten pool; the heating power is set at 0.2KW per kilogram of alloy material. During the melting process, the power supply is increased according to the amount of alloy added to make the molten pool temperature 1600-1700°C. After the metal in the crucible is completely melted, it is fully stirred; the molten pool temperature is adjusted to 1450-1500°C, evacuated to less than 0.1Pa, and melted for 3-5min; increase the power, adjust the melt temperature to 1550°C, and pour the smelted alloy in a vacuum state and under an argon protective atmosphere to form a remelted alloy ingot.

[0016] High-temperature solution treatment and aging treatment can ensure the uniformity of the alloy and the precipitation of a relatively regular cubic precipitation strengthening phase (γ' strengthening phase). The two-phase structure of the alloy of the present invention, the γ' strengthening phase presents a cubic shape, and the matrix channel γ phase in the middle of the γ' strengthening phase is relatively narrow, so that the alloy obtains good high-temperature performance, that is, has good mechanical properties at high temperatures.

[0017] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the density of the cobalt-based high-temperature alloy of the present invention is low, and the density of the cobalt-based high-temperature alloy is not higher than 8.5g·cm-3 , and has good mechanical properties at high temperatures; it can meet the needs of modern industry for lightweight high-temperature materials and better high-temperature performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 1;

[0019] Figure 2 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 2;

[0020] Figure 3 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 3;

[0021] Figure 4 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 4;

[0022] Figure 5 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 5;

[0023] Figure 6 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 6;

[0024] Figure 7 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 7;

[0025] Figure 8 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 8;

[0026] Fig. 9 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 9;

[0027] Fig.10 is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 10;

[0028] Fig.11 is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 11;

[0029] Fig.12 is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 12;

[0030] Fig.13 is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 13;

[0031] Fig.14 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 14;

[0032] Fig.15 is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 15;

[0033] Fig.16 is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 16;

[0034] Fig.17 is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 17;

[0035] Fig.18 This is a scanning electron microscope image of the cobalt-based high-temperature alloy of Example 18. DETAILED DESCRIPTION

[0036] Example 1

[0037] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 4%; V: 9%; Nb: 0.5%; Ni: 5%; and the balance is Co.

[0038] Expressed as Co-4Ti-9V-0.5Nb-5Ni, the preparation method of the above cobalt-based high-temperature alloy material comprises the following steps:

[0039] (1) Raw material preparation

[0040] High-purity Co, Ti, V, Nb, and Ni metal raw materials are used to prepare the required alloy, and the purity of the metal raw materials is 99.9wt.%; before smelting, the metal materials are polished or pickled to remove surface oxides, etc.; the blocky Co needs to be cleaned with a pickling solution to remove the oxides on its surface, and the composition of the pickling solution is 5% HCl+5% H2SO4+90% H2O (volume fraction); the flake Ni needs to be polished with sandpaper until the surface is bright and presents a metallic color; the treated metal is cleaned with alcohol and blown dry for standby use;

[0041] (2) Vacuum arc melting

[0042] The high-temperature alloy was prepared using a WK-Ⅱ non-consumable vacuum arc melting furnace. Each ingot weighed about 70g and was button-shaped. Before melting, the furnace cavity was wiped with alcohol to prevent the last melting from affecting the alloy composition due to the failure to clean the furnace.

[0043] First, the formulated amount of Co, Ti, V, Nb, and Ni metal raw materials are pre-loaded into the crucible of the melting furnace, with the powdered metal at the bottom and the block metal at the top, and the furnace cover is tightened; the pressure in the furnace is first pumped to 0.1 bar, and then high-purity argon is introduced, and the current regulator of the remote control switch is rotated to adjust the current to 60A, and an arc is struck on the tungsten electrode protruding from the crucible in the sample chamber, and then the current is adjusted to 300A, and the alloy is melted in an argon atmosphere; in order to prevent some refractory elements from not being completely melted and to ensure the uniformity of the alloy composition, after each melting is completed, the alloy is turned over by the melting furnace's built-in manipulator after cooling, and the melting must be turned over for more than 5 times to ensure the uniformity of the composition; after the melting is completed, the furnace is cooled to room temperature and the metal ingot is taken out;

[0044] (3) Heat treatment of alloy

[0045] After the smelted metal ingot is wire-cut, acetone and alcohol are used to remove oil stains in an ultrasonic cleaner and blown dry for use; the metal ingot is placed in a quartz glass tube and sealed, and then the glass tube is placed in a box-type resistance furnace for solution aging treatment; the temperature of the solution treatment is 1100°C and the treatment time is 48h; the temperature of the aging treatment is 870°C and the treatment time is 72h.

[0046] The measured density of the cobalt-based superalloy Co-4Ti-9V-0.5Nb-5Ni of Example 1 is shown in Table 1, and the precipitation strengthening phase photographed by scanning electron microscope is shown in Table 1. Figure 1 As shown, the yield strength of the cobalt-based high-temperature alloy Co-4Ti-9V-0.5Nb-5Ni compressed at 900°C is 459 MPa and the ultimate strength is 540 MPa.

[0047] The yield strength of ordinary nickel-based high-temperature alloy under compression at 900°C is 275Mpa, and the ultimate strength is 312Mpa.

[0048] Example 2

[0049] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 4%; V: 9%; Nb: 1%; Ni: 10%; and the balance is Co.

[0050] Expressed as Co-4Ti-9V-1Nb-10Ni, the preparation method of the above cobalt-based high-temperature alloy material comprises the following steps:

[0051] (1) Raw material preparation

[0052] High-purity Co, Ti, V, Nb, and Ni metal raw materials are used to prepare the required alloy, and the purity of the metal raw materials is 99.9wt.%; before smelting, the metal materials are polished or pickled to remove surface oxides, etc.; the blocky Co needs to be cleaned with a pickling solution to remove the oxides on its surface, and the composition of the pickling solution is 5% HCl+5% H2SO4+90% H2O (volume fraction); the flake Ni needs to be polished with sandpaper until the surface is bright and presents a metallic color; the treated metal is cleaned with alcohol and blown dry for standby use;

[0053] (2) Vacuum induction melting

[0054] First, the formula amount of Co, Ti, V, Nb, and Ni metal raw materials are pre-loaded into the crucible of the smelting furnace, the cooling water system and the vacuum system are turned on, and the smelting chamber is evacuated to a vacuum degree of less than 5Pa; the induction heating power supply is started to gradually melt the metal in the crucible to form a complete molten pool, and the heating power is set at 0.2KW per kilogram of alloy material. During the smelting process, the power supply is increased according to the amount of alloy added to make the molten pool temperature at about 1650°C. After the metal in the crucible is completely melted, electromagnetic stirring is performed for 15 minutes; the alloy is refined: the equipment smelting power is appropriately reduced, that is, the molten pool temperature is adjusted to about 1500°C, the vacuum is evacuated to less than 1Pa, the smelting is performed for 3 to 5 minutes, and the alloy melt is electromagnetically stirred for 10 minutes; the power is increased to control the melt temperature at 1550°C, and the smelted alloy is poured in a vacuum state and under an argon protective atmosphere to form a remelted alloy ingot, and the ingot is taken out;

[0055] (3) Heat treatment of alloy

[0056] After the smelted metal ingot is wire-cut, acetone and alcohol are used to remove oil stains in an ultrasonic cleaner and blown dry for use; the metal ingot is placed in a quartz glass tube and sealed, and then the glass tube is placed in a box-type resistance furnace for solution aging treatment; the temperature of the solution treatment is 1100°C and the treatment time is 48h; the temperature of the aging treatment is 870°C and the treatment time is 72h.

[0057] Example 2 The measured density of the cobalt-based high-temperature alloy Co-4Ti-9V-1Nb-10Ni is shown in Table 1, and the scanning electron microscope image is shown in Figure 2 As shown, the yield strength obtained by compression at 900°C is 488 MPa and the ultimate strength is 540 MPa.

[0058] Example 3

[0059] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 4%; V: 10%; Nb: 1.5%; Ni: 15%; and the balance is Co.

[0060] Represented by Co-4Ti-10V-1.5Nb-15Ni, the preparation method of the above cobalt-based high-temperature alloy material is the same as that of Example 1.

[0061] Example 3 Cobalt-based superalloy Co-4Ti-10V-1.5Nb-15Ni The measured density is shown in Table 1, and the scanning electron microscope image is shown in Figure 3 As shown, the yield strength obtained by compression at 900°C is 515 MPa and the ultimate strength is 527 MPa.

[0062] Example 4

[0063] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 4%; V: 10%; Nb: 2%; Ni: 20%; and the balance is Co.

[0064] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-4Ti-10V-2Nb-20Ni, and its preparation method is the same as that in Example 2.

[0065] Example 4 Cobalt-based superalloy Co-4Ti-10V-2Nb-20Ni The measured density is shown in Table 1, and the scanning electron microscope image is shown in Figure 4 As shown, the yield strength obtained by compression at 900°C is 439 MPa and the ultimate strength is 505 MPa.

[0066] Example 5

[0067] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 4%; V: 11%; Nb: 0.5%; Ni: 5%; and the balance is Co.

[0068] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-4Ti-11V-0.5Nb-5Ni, and its preparation method is the same as that in Example 1.

[0069] Example 5 Cobalt-based superalloy Co-4Ti-11V-0.5Nb-5Ni The measured density is shown in Table 1, and the scanning electron microscope image is shown in Figure 5 As shown, the yield strength obtained by compression at 900°C is 410 MPa and the ultimate strength is 489 MPa.

[0070] Example 6

[0071] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 4%; V: 11%; Nb: 1%; Ni: 10%; and the balance is Co.

[0072] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-4Ti-11V-1Nb-10Ni, and its preparation method is the same as that in Example 2.

[0073] Example 6 The measured density of the cobalt-based superalloy Co-4Ti-11V-1Nb-10Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Figure 6 As shown, the yield strength obtained by compression at 900°C is 425 MPa and the ultimate strength is 441 MPa.

[0074] Example 7

[0075] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 5%; V: 9%; Nb: 1.5%; Ni: 15%; and the balance is Co.

[0076] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-5Ti-9V-1.5Nb-15Ni, and its preparation method is the same as that in Example 1.

[0077] Example 7 The measured density of the cobalt-based superalloy Co-5Ti-9V-1.5Nb-15Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Figure 7 As shown, the yield strength of the alloy obtained by compression at 900°C is 409 MPa and the ultimate strength is 465 MPa.

[0078] Example 8

[0079] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 5%; V: 9%; Nb: 2%; Ni: 20%; and the balance is Co.

[0080] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-5Ti-9V-2Nb-20Ni, and its preparation method is the same as that in Example 2.

[0081] Example 8 The measured density of the cobalt-based superalloy Co-5Ti-9V-2Nb-20Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Figure 8 As shown, the yield strength obtained by compression at 900°C is 406 MPa and the ultimate strength is 443 MPa.

[0082] Example 9

[0083] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 5%; V: 10%; Nb: 2%; Ni: 5%; and the balance is Co.

[0084] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-5Ti-10V-2Nb-5Ni, and its preparation method is the same as that in Example 1.

[0085] Example 9 The measured density of the cobalt-based superalloy Co-5Ti-10V-2Nb-5Ni is shown in Table 1, and the strengthening phase photographed by scanning electron microscope is shown in Table 1. Fig. 9 As shown, the yield strength obtained by compression at 900°C is 354Mpa and the ultimate strength is 450Mpa.

[0086] Example 10

[0087] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 5%; V: 10%; Nb: 1%; Ni: 10%; and the balance is Co.

[0088] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-5Ti-10V-1Nb-10Ni, and its preparation method is the same as that in Example 2.

[0089] Example 10 The measured density of the cobalt-based superalloy Co-5Ti-10V-1Nb-10Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Fig.10 As shown, the yield strength obtained by compression at 900°C is 403Mpa and the ultimate strength is 464Mpa.

[0090] Embodiment 11

[0091] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 5%; V: 11%; Nb: 0.5%; Ni: 5%; and the balance is Co.

[0092] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-5Ti-11V-0.5Nb-5Ni, and its preparation method is the same as that in Example 1.

[0093] Example 11 The measured density of the cobalt-based superalloy Co-5Ti-11V-0.5Nb-5Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Fig.11 As shown, the yield strength obtained by compression at 900°C is 443Mpa and the ultimate strength is 484Mpa.

[0094] Example 12

[0095] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 5%; V: 11%; Nb: 1%; Ni: 10%; and the balance is Co.

[0096] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-5Ti-11V-1Nb-10Ni, and its preparation method is the same as that in Example 2.

[0097] Example 12 The measured density of the cobalt-based superalloy Co-5Ti-11V-1Nb-10Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Fig.12 As shown, the yield strength obtained by compression at 900°C is 485 MPa and the ultimate strength is 524 MPa.

[0098] Embodiment 13

[0099] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 6%; V: 9%; Nb: 1.5%; Ni: 15%; and the balance is Co.

[0100] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-6Ti-9V-1.5Nb-15Ni, and its preparation method is the same as that in Example 1.

[0101] Example 13 The measured density of the cobalt-based superalloy Co-6Ti-9V-1.5Nb-15Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Fig.13 As shown, the yield strength obtained by compression at 900°C is 478 MPa and the ultimate strength is 512 MPa.

[0102] Embodiment 14

[0103] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 6%; V: 9%; Nb: 2%; Ni: 20%; and the balance is Co.

[0104] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-6Ti-9V-2Nb-20Ni, and its preparation method is the same as that in Example 2.

[0105] Example 14 The measured density of the cobalt-based superalloy Co-6Ti-9V-2Nb-20Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Fig.14 As shown, the yield strength obtained by compression at 900°C is 423Mpa and the ultimate strength is 468Mpa.

[0106] Embodiment 15

[0107] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 6%; V: 10%; Nb: 0.5%; Ni: 5%; and the balance is Co.

[0108] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-6Ti-10V-0.5Nb-5Ni, and its preparation method is the same as that in Example 1.

[0109] Example 15 The measured density of the cobalt-based superalloy Co-6Ti-10V-0.5Nb-5Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Fig.15 As shown, the yield strength obtained by compression at 900°C is 482 MPa and the ultimate strength is 517 MPa.

[0110] Example 16

[0111] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 6%; V: 10%; Nb: 1%; Ni: 10%; and the balance is Co.

[0112] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-6Ti-10V-1Nb-10Ni, and its preparation method is the same as that in Example 2.

[0113] Example 16 The measured density of the cobalt-based superalloy Co-6Ti-10V-1Nb-10Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Fig.16As shown, the yield strength obtained by compression at 900°C is 415 MPa and the ultimate strength is 457 MPa.

[0114] Embodiment 17

[0115] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 6%; V: 11%; Nb: 1.5%; Ni: 15%; and the balance is Co.

[0116] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-6Ti-11V-1.5Nb-15Ni, and its preparation method is the same as that in Example 1.

[0117] Example 17 The measured density of the cobalt-based superalloy Co-6Ti-11V-1.5Nb-15Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Fig.17 As shown, the yield strength obtained by compression at 900°C is 472 MPa and the ultimate strength is 491 MPa.

[0118] Embodiment 18

[0119] The cobalt-based high-temperature alloy of the present invention is composed of the following metal elements in atomic percentage: Ti: 6%; V: 11%; Nb: 2%; Ni: 20%; and the balance is Co.

[0120] The above-mentioned cobalt-based high-temperature alloy material is represented by Co-6Ti-11V-2Nb-20Ni, and its preparation method is the same as that in Example 2.

[0121] Example 18 The measured density of the cobalt-based superalloy Co-6Ti-11V-2Nb-20Ni is shown in Table 1, and the strengthening phase photographed by the scanning electron microscope is shown in Table 1. Fig.18 As shown, the yield strength obtained by compression at 900°C is 479 MPa and the ultimate strength is 498 MPa.

[0122] Table 1 shows the density of the cobalt-based high-temperature alloys obtained in Examples 1 to 18.

[0123]

[0124]

[0125] pass Figures 1 to 18 It can be seen from the SEM image that the alloy prepared by the present invention has a γ / γ' two-phase coherent structure, and both the matrix γ phase and the γ' strengthening phase are face-centered cubic structures. The structural alloy can maintain high strength and excellent anti-oxidation, thermal corrosion resistance, and creep resistance at high temperatures, and has good organizational stability.

Claims

1. A low-density cobalt-based high-temperature alloy, characterized in that: The high temperature alloy material is mixed with the following components in atomic percentage: Ti: 4-6%; V: 9-11%; Nb: 0.2-2%; Ni: 5-20%; and the balance is Co.

2. The low-density cobalt-based high-temperature alloy according to claim 1, characterized in that: The density of the cobalt-based high-temperature alloy is not higher than 8.5 g·cm -3 .

3. The method for preparing the cobalt-based high-temperature alloy according to claim 1, characterized in that: Specifically: it includes a heat treatment step; the heat treatment includes a solution treatment and an aging treatment process; the temperature of the solution treatment is 1100~1150℃, and the treatment time is 48~50h; the temperature of the aging treatment is 850~900℃, and the treatment time is 48~72h.

4. The method for preparing a cobalt-based high-temperature alloy according to claim 3, characterized in that: The temperature of the solution treatment is 1100° C., and the treatment time is 48 h; the temperature of the aging treatment is 870° C., and the treatment time is 72 h.

5. The method for preparing a cobalt-based high-temperature alloy according to claim 3, characterized in that: Before heat treatment, it also includes pretreatment and vacuum melting of metal raw materials.

6. The method for preparing a cobalt-based high-temperature alloy according to claim 5, characterized in that: The pretreatment of the metal raw materials is specifically as follows: before smelting, the metal raw materials are polished or pickled to remove surface oxide scale.

7. The method for preparing a cobalt-based high-temperature alloy according to claim 6, characterized in that: The pickling solution includes the following components in volume fractions: 4~5% HCl, 4~5% H2SO4 and 90~95% H2O.

8. The method for preparing a cobalt-based high-temperature alloy according to claim 5, characterized in that: The specific steps of vacuum melting are as follows: pre-load the formulated amount of Co, Ti, V, Nb, and Ni metal raw materials into the crucible of the melting furnace; pump the pressure in the melting furnace to 0.1~0.15bar, then introduce high-purity argon gas, first adjust the current to 50~60A, start an arc on the protruding tungsten electrode on the crucible in the sample chamber, and then adjust the current to 300~320A to melt the alloy in an argon atmosphere.

9. The method for preparing a cobalt-based high-temperature alloy according to claim 8, characterized in that: After each smelting, the cooled alloy is turned over and then smelted again; the number of times of turning over and smelting is more than 5 times.

10. The method for preparing a cobalt-based high-temperature alloy according to claim 5, characterized in that: The vacuum melting is specifically as follows: the formulated amount of Co, Ti, V, Nb, and Ni metal raw materials are pre-loaded into the crucible of the melting furnace, and the melting chamber is evacuated to a vacuum degree of less than 5 Pa; the induction heating power supply is started to make the molten pool temperature 1600-1700°C, and after the metal in the crucible is completely melted, it is fully stirred; The molten pool temperature is adjusted to 1450-1500°C, the vacuum is evacuated to less than 0.1 Pa, and the smelting is performed for 3-5 minutes; the melt temperature is adjusted to not less than 1550°C, and the smelted alloy is poured in a vacuum state and an argon protective atmosphere to form an alloy ingot.