Low-cost light-weight high-strength aluminum-based composite material and preparation method thereof

By adding glass powder to the aluminum-based composite material and using air pressureless sintering and thermal deformation processing, the problems of difficult and cost of forming traditional aluminum-based composite materials are solved, and low density, low cost, high strength and high plasticity are achieved. Aluminum-based composite material, suitable for large-size manufacturing.

CN119040701APending Publication Date: 2024-11-29UNIV OF SCI & TECH BEIJING
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411058648.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional aluminum-based composite materials are difficult to form and costly during hot processing, and the size of the billet is limited, making it difficult to meet the manufacturing needs of large-size aluminum-based composite components, and the ceramic particles reinforced aluminum-based composite materials in the prior art The plastic toughness enhancement effect is not obvious.

Method used

By adding 5-30 wt% glass powder to the aluminum-based composite material, using uniform powder mixing technology and air pressure-free sintering combined with hot extrusion, hot forging and other hot deformation processing processes, the heat treatment temperature is controlled to achieve glass powder particles and matrix. The strong interface combination reduces the difficulty of forming and improves the density and mechanical properties of the material.

Benefits of technology

It realizes a low-density and low-cost aluminum-based composite material, which has high strength and high plasticity, avoids pores and loose defects, broadens the application range of products, adapts to large-size manufacturing needs, and improves the comprehensive performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040701A_ABST
    Figure CN119040701A_ABST
Patent Text Reader

Abstract

The invention provides a low-cost light-weight high-strength aluminum-based composite material and a preparation method thereof, and relates to the technical field of powder metallurgy. The adding amount of the glass powder in the composite material is 5-30 wt%, and the balance is aluminum or aluminum alloy components and inevitable impurities. The method comprises the steps that aluminum alloy matrix powder and a certain amount of glass powder are evenly mixed, and the aluminum matrix composite is prepared through cold isostatic pressing forming, sintering densification and deformation machining. The aluminum-based composite material is prepared by adding the low-cost and low-density glass powder, and the composite material has excellent mechanical properties on the basis of a multi-scale second-phase strengthening mechanism after heat treatment regulation and control. According to the technology, low-cost and efficient manufacturing of the light high-strength aluminum-based composite material can be achieved, the technological process is short, the production efficiency is high, and the method is suitable for large-scale industrial production and has great application potential in the fields of aerospace, automobiles, ships, electronic communication, buildings and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of powder metallurgy and relates to a low-cost, light-weight, high-strength aluminum-based composite material and a preparation method thereof. Background Art

[0002] Aluminum-based composite materials mainly use pure aluminum or aluminum alloy as the matrix, and improve the alloy matrix structure and performance by adding reinforcement phases such as particles, fibers or whiskers. Compared with traditional aluminum alloy materials, aluminum-based composite materials have a broader design space. Different reinforcement phases and flexible component ratios can be selected according to the required performance. Different preparation methods can be used to obtain aluminum-based composite materials with better organization and performance. They have excellent properties such as low specific gravity, high strength and low thermal expansion coefficient, and have played an important role in the development of the national economy.

[0003] However, traditional aluminum-based composite materials mainly use SiC, TiC, TiB2 and other high-hardness, high-melting-point hard ceramic particles as reinforcement phases. Compared with the aluminum matrix, the deformation resistance of aluminum-based composite materials during thermal processing is significantly improved, the forming difficulty is increased, and the manufacturing cost is increased. Glass powder is an amorphous material without a fixed melting point. It softens with increasing temperature. If it is added to the aluminum matrix as a second phase, it is easy to deform with the matrix during thermal processing, greatly reducing the forming difficulty of aluminum-based composite materials. At the same time, glass powder is inexpensive and has the characteristics of low density, high hardness, and high compressive strength. As a reinforcement phase of aluminum-based composite materials, it can significantly improve the specific strength and specific stiffness of the composite material and effectively reduce the density of the composite material.

[0004] Invention patent CN 118048557 A discloses a glass-ceramic particle reinforced aluminum-based composite material and its preparation method and application. The mass proportion of glass-ceramic particles in the composite material is 5-20%, and the particle size is 800-1250 mesh. It is prepared into an aluminum-based composite material by mixing, molding, and hot pressing and sintering with aluminum powder and alloy element powder. The invention improves the interface bonding state between the reinforcing phase and the matrix in the glass-reinforced aluminum-based composite material to a certain extent through hot pressing and sintering technology, and improves the density of the composite material, but hot pressing and sintering is difficult to significantly improve the plastic toughness of the aluminum-based composite material. It can be seen from the embodiments of the invention that the tensile strength of the prepared aluminum-based composite material does not exceed 300 MPa, and the effect of improving the mechanical properties is not obvious. At the same time, the invention needs to be hot-pressed and sintered under vacuum conditions, which has high requirements on equipment, and the size of the prepared billet is limited, which is difficult to meet the manufacturing needs of large-size aluminum-based composite components.

[0005] Therefore, there is an urgent need to develop low-cost and efficient manufacturing technologies for aluminum-based composites with high performance and a wide range of dimensional adjustment. Summary of the invention

[0006] The purpose of the present invention is to provide a low-cost, lightweight, high-strength aluminum-based composite material and a preparation method thereof, which can solve the problems in the prior art that ceramic particle reinforced aluminum-based composite materials are difficult to process and the ingot size does not meet the requirements of structural parts, and has low density, strong interface, and excellent strength-plasticity matching.

[0007] In order to achieve the technical objectives of the present invention, the technical solutions provided by the present invention are as follows:

[0008] A low-cost, lightweight, high-strength aluminum-based composite material, wherein the glass powder addition amount is 5-30 wt%, and the rest is aluminum or aluminum alloy components and inevitable impurities. If the amount of glass powder added is too low, the material performance will not be significantly improved, and the density will not be significantly reduced; if the amount of glass powder added is too high, it will affect the material's forming effect and sintering density, and reduce the material performance.

[0009] The aluminum-based composite material has the characteristics of low cost and low density, and has excellent mechanical properties: the density is 2.5-2.7 g / cm 3 , tensile strength is 260-550 MPa, yield strength is 200-480 MPa, and elongation is 5-14%.

[0010] Furthermore, when the aluminum-based raw material is an aluminum alloy, the aluminum-based composite material has a tensile strength of 420-550 MPa and a yield strength of 360-480 MPa.

[0011] The method for preparing the low-cost, lightweight and high-strength aluminum-based composite material comprises the following steps:

[0012] (1) Composite powder preparation: uniformly mix aluminum powder or aluminum alloy powder with glass powder;

[0013] (2) Cold isostatic pressing: the composite powder obtained in step (1) is placed in a bag and subjected to cold isostatic pressing to obtain a green body;

[0014] (3) Sintering densification: placing the green body obtained in step (2) in a sintering furnace for sintering in an air atmosphere to obtain a sintered ingot of the composite material;

[0015] (4) Deformation and heat treatment: The sintered ingot obtained in step (3) is subjected to deformation processing such as hot extrusion, hot rolling or ring forging according to actual needs, and the deformed ingot is heat treated according to different usage requirements.

[0016] Preferably, the aluminum alloy powder in step (1) can be prepared by an element mixing method or an atomization method. The preferred aluminum alloy type is selected from one or more of 7055 aluminum alloy, 7075 aluminum alloy, 2324 aluminum alloy, and 2024 aluminum alloy.

[0017] Preferably, the glass powder in step (1) is one or more of silicate glass powder, borate glass powder, phosphate glass powder and quartz glass powder. The above glass materials have a low softening temperature and can adapt to subsequent deformation processing, thereby having good temperature matching.

[0018] Preferably, the glass powder in step (1) is irregular or spherical in shape, has an average particle size of 0.5-10 µm, and a density of 1.8-2.5 g / cm 3 Compared with the prior art, the present invention does not need to use high-cost microcrystalline glass, and the selected glass has more forms and smaller particle sizes, and has a more obvious strengthening effect on the substrate.

[0019] Preferably, the aluminum powder or aluminum alloy powder and the glass powder in step (1) are uniformly mixed by one or more of a V-type mixer, a double cone mixer, a rolling ball mill, a planetary ball mill, and a stirring ball mill, with a ball-to-material ratio of 2:1-20:1 and a mixing time of 4-24 hours.

[0020] Preferably, the sheath material in step (2) is rubber or silicone, the green body is in the shape of a rod, a plate, a tube or a ring, the pressing pressure is 120-400 MPa, and the holding time is 20-150 s.

[0021] Preferably, the sintering temperature of step (3) is 500-640 °C and the holding time is 1-6 h. Selecting this sintering temperature range can achieve the densification of aluminum without causing aluminum oxidation. If the sintering temperature is too high, the grains will be too large and the liquid phase will flow out, greatly reducing the sintering density. If the sintering temperature is too low, the particles will not be fully bonded, under-sintering will cause the sample to be not dense, and the performance will be reduced.

[0022] Preferably, in step (4), the obtained sintered ingot is subjected to T6 heat treatment. Furthermore, the deformation processing temperature in step (4) is 250-500°C, the solution temperature is 450-550°C, the quenching medium is 40-70°C water, the aging temperature is 100-200°C, and the aging time is 8-24 h.

[0023] The key points of the present invention are:

[0024] (1) The present invention adds 5-30 wt% of low-density glass powder to a high-strength aluminum alloy matrix, ensures that the glass powder particles are evenly distributed in the aluminum matrix through a uniform powder mixing technology, and adopts air pressureless sintering combined with hot extrusion, hot forging and other thermal deformation processing processes to prepare a fully dense powder metallurgy aluminum-based composite material. The glass powder particles and the matrix achieve a strong interface bond, obtain an excellent particle strengthening effect, and the matrix has fine grains, so that the composite material has a good match between strength and plasticity.

[0025] (2) The present invention controls the thermal deformation processing and heat treatment temperature and selects a suitable thermal deformation processing temperature to soften the glass powder particles, thereby reducing the processing difficulty of the particle-reinforced aluminum-based composite material. The heat treatment regulation obtains an excellent precipitation strengthening effect, thereby ensuring the comprehensive performance of the product.

[0026] The beneficial effects of the present invention are:

[0027] (1) The density and price of the glass powder used in the present invention are lower than those of aluminum powder, so that the prepared aluminum-based composite material has "double low" characteristics - low density and low cost; the strong interface bonding between the high-hardness glass powder and the matrix and the fine microstructure of the aluminum matrix grains enable the composite material to obtain "double high" performance - high strength and high plasticity.

[0028] (2) Compared with the stirring casting method for preparing aluminum-based composite materials, the technology of the present invention can avoid the formation of defects such as pores and looseness, and improve the segregation of alloy components and the uneven distribution of reinforcement phases; compared with the hot pressing sintering method for preparing aluminum-based composite materials, the technology of the present invention can achieve efficient manufacturing of large-sized aluminum-based composite products and broaden the application range of products.

[0029] (3) Powder metallurgy pressureless sintering combined with thermal deformation processing to prepare glass powder reinforced aluminum-based composite materials has unique advantages. The use of air pressureless sintering can improve the efficiency of billet making and significantly reduce the cost of billet making. The process has strong adaptability, a wide plastic processing window, and a high yield rate, which can realize large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0031] Figure 1 This is a microstructure diagram of the borate glass powder reinforced aluminum-based composite material prepared in Example 1 of the present invention.

[0032] Figure 2 This is a microstructure diagram of the quartz glass powder reinforced aluminum-based composite material prepared in Example 2 of the present invention.

[0033] Figure 3 This is the XRD spectrum of the 10 wt% quartz glass powder reinforced 2324 aluminum-based composite material prepared in Example 2 of the present invention.

[0034] Figure 4 This is a microstructure diagram of the silicate glass powder reinforced aluminum-based composite material prepared in Example 3 of the present invention.

[0035] Figure 5 This is a microstructure diagram of the phosphate glass powder reinforced aluminum-based composite material prepared in Example 4 of the present invention. DETAILED DESCRIPTION

[0036] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0037] Example 1

[0038] (1) According to the element content of 7055 aluminum alloy, the single powder was mixed by rolling ball milling to prepare 7055 aluminum alloy powder, and the rolling ball milling was carried out for 24 hours. The ball-to-material ratio was 10:1, and the particle size of 7055 aluminum alloy powder was -200 mesh. Irregular borate glass powder with an average particle size of 10 µm was selected and mixed evenly with 7055 aluminum alloy powder by rolling ball milling. The addition amount of borate glass powder was 30wt%, the ball-to-material ratio was 20:1, and the mixing time was 8 hours.

[0039] (2) The composite powder obtained in step (1) is loaded into a rubber sleeve and subjected to cold isostatic pressing to obtain a rod-shaped green body with a pressing pressure of 150 MPa and a holding time of 120 s.

[0040] (3) The green body obtained in step (2) is placed in a sintering furnace for sintering and densification. The sintering atmosphere is air, the sintering temperature is 500°C, and the holding time is 6 h to obtain a sintered ingot of the composite material.

[0041] (4) The sintered ingot obtained in step (3) was hot extruded to prepare a rod, the hot extrusion temperature was 400 °C, and the extrusion ratio was 36:1; finally, T6 heat treatment was performed: solid solution at 475 °C for 1 h, quenching medium was 70 °C water, and then aging at 120 °C for 24 h, and air cooling. The performance test showed that the tensile strength was 550 MPa, the yield strength was 480 MPa, the elongation was 5%, and the density was 2.51 g / cm 3 .

[0042] Example 2

[0043] (1) According to the element content ratio of 2324 aluminum alloy, 2324 aluminum alloy powder was prepared by nitrogen atomization method with an average particle size of 25 μm. Spherical quartz glass powder with an average particle size of 7 μm was selected and mixed evenly with 2324 aluminum alloy powder by a V-type mixer. The amount of quartz glass powder added was 10 wt%, and the mixing time was 24 hours.

[0044] (2) The composite powder obtained in step (1) is placed in a silica gel package and subjected to cold isostatic pressing to obtain a plate-shaped green body with a pressing pressure of 400 MPa and a holding time of 20 s.

[0045] (3) The green body obtained in step (2) is placed in a sintering furnace for sintering and densification. The sintering atmosphere is air, the sintering temperature is 620°C, and the holding time is 2 h to obtain a sintered ingot of the composite material.

[0046] (4) The sintered ingot obtained in step (3) was hot rolled into a plate at a rolling temperature of 250 °C; finally, T6 heat treatment was performed: solution treatment at 510 °C for 1 h, quenching medium was 40 °C water, and then aging at 180 °C for 10 h. The performance test showed that the tensile strength was 420 MPa, the yield strength was 360 MPa, the elongation was 14%, and the density was 2.63 g / cm 3 .

[0047] Example 3

[0048] (1) According to the element content of 2024 aluminum alloy, the single powder was planetarily ball milled to prepare 2024 aluminum alloy powder, and the planetary ball milling was 12 hours, the ball-to-material ratio was 8:1, and the average particle size of the 2024 aluminum alloy powder was 15 µm. Irregular silicate glass powder with an average particle size of 0.5 µm was selected and mixed evenly with the 2024 aluminum alloy powder by rolling ball milling. The amount of silicate glass powder added was 5wt%, the ball-to-material ratio was 2:1, and the mixing time was 6 hours.

[0049] (2) The composite powder obtained in step (1) is loaded into a rubber sleeve and subjected to cold isostatic pressing to obtain a rod-shaped green body with a pressing pressure of 180 MPa and a holding time of 90 s.

[0050] (3) The green body obtained in step (2) is placed in a sintering furnace for sintering and densification. The sintering atmosphere is air, the sintering temperature is 580°C, and the holding time is 3 h to obtain a sintered ingot of the composite material.

[0051] (4) The sintered ingot obtained in step (3) was hot extruded into a rod at an extrusion temperature of 420 °C and an extrusion ratio of 50:1; finally, a T6 heat treatment was performed: solid solution at 520 °C for 1 h, quenching medium was 50 °C water, and then aging at 190 °C for 8 h. The performance test showed that the tensile strength was 528 MPa, the yield strength was 431 MPa, the elongation was 10.5%, and the density was 2.67 g / cm 3 .

[0052] Example 4

[0053] (1) According to the element content ratio of 7075 aluminum alloy, 7075 aluminum alloy powder was prepared by nitrogen atomization method with an average particle size of 25 μm. Irregular phosphate glass powder with an average particle size of 2 μm was selected and mixed with 7075 aluminum alloy powder by stirring and ball milling. The amount of phosphate glass powder added was 10 wt%, the ball-to-material ratio was 8:1, and the mixing time was 15 hours.

[0054] (2) The composite powder obtained in step (1) is loaded into a rubber sleeve and subjected to cold isostatic pressing to obtain a rod-shaped green body. The pressing pressure is 300 MPa and the holding time is 40 s.

[0055] (3) The green body obtained in step (2) is placed in a sintering furnace for sintering and densification. The sintering atmosphere is air, the sintering temperature is 550°C, and the holding time is 4 h to obtain a sintered ingot of the composite material.

[0056] (4) The sintered ingot obtained in step (3) was hot extruded into a plate at an extrusion temperature of 440 °C and an extrusion ratio of 20:1; finally, a T6 heat treatment was performed: solution treatment at 470 °C for 1 h, quenching medium was 60 °C water, and aging at 130 °C for 24 h. The performance test showed that the tensile strength was 517 MPa, the yield strength was 469 MPa, the elongation was 7.3%, and the density was 2.59 g / cm 3 .

[0057] Example 5

[0058] (1) Pure aluminum powder was prepared by gas atomization method with an average particle size of 20 µm. Irregular silicate glass powder with an average particle size of 10 µm was selected and mixed evenly with pure aluminum powder by stirring and ball milling. The amount of silicate glass powder added was 10 wt%, the ball-to-material ratio was 5:1, and the mixing time was 10 h.

[0059] (2) The composite powder obtained in step (1) is loaded into a rubber sleeve and subjected to cold isostatic pressing to obtain a rod-shaped green body with a pressing pressure of 200 MPa and a holding time of 30 s.

[0060] (3) The green body obtained in step (2) is placed in a sintering furnace for sintering and densification. The sintering atmosphere is air, the sintering temperature is 620°C, and the holding time is 2 h to obtain a sintered ingot of the composite material.

[0061] (4) The sintered ingot obtained in step (3) was hot extruded into a rod, the extrusion temperature was 430 °C, and the extrusion ratio was 16:1. The performance test showed that the tensile strength was 264 MPa, the yield strength was 205 MPa, the elongation was 11%, and the density was 2.57 g / cm 3 .

[0062] The above embodiment was subjected to optical microscopy and X-ray diffraction tests, and the specific results are as follows:

[0063] Figure 1 The microstructure of the borate glass powder reinforced aluminum-based composite material prepared in Example 1 of the present invention is shown in FIG. The product has 7055 aluminum alloy as the matrix and irregular borate glass powder (black particles) with an average particle size of 10 μm as the reinforcement phase. The amount of borate glass powder added is 30 wt%, which is evenly distributed in the matrix and closely combined with the matrix, and the structure is dense and has no holes.

[0064] Figure 2 The microstructure of the quartz glass powder reinforced aluminum-based composite material prepared in Example 2 of the present invention. The product has 2324 aluminum alloy as the matrix and spherical quartz glass powder (spherical black particles) with an average particle size of 7 μm as the reinforcement phase. The amount of quartz glass powder added is 10 wt%, and it can be seen that the glass powder retains a complete spherical morphology, there is a fine second phase in the matrix, and the structure is dense and has no holes.

[0065] Figure 3 The XRD spectrum of the 10 wt% quartz glass powder reinforced 2324 aluminum-based composite material prepared in Example 2 of the present invention shows that the main phase is elemental aluminum.

[0066] Figure 4 The microstructure of the silicate glass powder reinforced aluminum-based composite material prepared in Example 3 of the present invention. The product uses 2024 aluminum alloy as the matrix and irregular silicate glass powder (black particles) with an average particle size of 0.5 μm as the reinforcement phase. The amount of silicate glass powder added is 5 wt%, and the glass powder is fine and evenly distributed in the matrix, tightly combined with the matrix, and has a dense structure without holes.

[0067] Figure 5 The microstructure of the phosphate glass powder reinforced aluminum-based composite material prepared in Example 4 of the present invention. The product has 7075 aluminum alloy as the matrix and irregular phosphate glass powder (black particles) with an average particle size of 2 μm as the reinforcement phase. The amount of phosphate glass powder added is 10 wt%, and the glass powder is evenly distributed in the matrix without obvious segregation, and is tightly combined with the matrix, with a dense structure and no holes.

[0068] Comparative Example 1

[0069] In step (1), borate glass powder and 7055 aluminum alloy powder are rolled and ball-milled, and the amount of borate glass powder added is 45 wt %. The other steps are the same as in Example 1.

[0070] The performance test shows that the tensile strength is 383 MPa, the yield strength is 278 MPa, the elongation is 1.1%, and the density is 2.44 g / cm 3This indicates that if the proportion of glass powder added is too high, the forming effect and sintering density of the material will be reduced, and the material performance will be affected.

[0071] Comparative Example 2

[0072] In step (3), the green body is sintered and densified by hot pressing sintering technology at a sintering temperature of 550° C. for a holding time of 2 h to obtain a sintered ingot of the composite material. The other steps are the same as those in Example 2.

[0073] The performance test shows that the tensile strength is 312 MPa, the yield strength is 264 MPa, the elongation is 4.2%, and the density is 2.66 g / cm 3 This shows that it is difficult to significantly improve the plastic toughness of the material by hot pressing sintering, and the improvement of mechanical properties is not obvious.

[0074] Comparative Example 3

[0075] In step (3), the obtained green body is placed in a sintering furnace for sintering and densification, the sintering atmosphere is air, the sintering temperature is 400°C, and the holding time is 3 hours to obtain a sintered ingot of the composite material. The other steps are the same as in Example 3.

[0076] The performance test shows that the tensile strength is 252 MPa, the yield strength is 194 MPa, the elongation is 3.5%, and the density is 2.61 g / cm 3 This indicates that too high a sintering temperature will lead to the growth of the grains of the material, accompanied by the outflow of the liquid phase, the increase of the porosity of the material, the decrease of the sintering density, and thus the reduction of the mechanical properties of the material.

[0077] Comparative Example 4

[0078] In step (4), the obtained sintered ingot is hot extruded into a plate, the extrusion temperature is 520 °C, the extrusion ratio is 20:1, and the sample is obviously cracked; finally, T6 heat treatment is performed: solution treatment at 470 °C for 1 h, quenching medium is 60 °C water, and aging at 130 °C for 24 h.

[0079] The performance test shows that the tensile strength is 362 MPa, the yield strength is 241 MPa, the elongation is 5%, and the density is 2.63 g / cm 3 This indicates that the extrusion temperature is too high, resulting in obvious cracking on the material surface, micro cracks inside the material, and reduced plastic toughness of the material.

[0080] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A low-cost, lightweight, high-strength aluminum-based composite material, characterized in that: The amount of glass powder added is 5-30 wt%, and the rest is aluminum or aluminum alloy components and inevitable impurities.

2. The aluminum-based composite material according to claim 1, characterized in that: Its density is 2.5-2.7 g / cm 3 , tensile strength is 260-550 MPa, yield strength is 200-480 MPa, and elongation is 5-14%.

3. The method for preparing the low-cost, lightweight, high-strength aluminum-based composite material according to claim 1 or 2, characterized in that: The following steps are involved: (1) Preparation of composite powder: uniformly mix aluminum powder or aluminum alloy powder with glass powder; (2) Cold isostatic pressing: the composite powder obtained in step (1) is placed in a bag and subjected to cold isostatic pressing to obtain a green body; (3) Sintering densification: placing the green body obtained in step (2) in a sintering furnace for sintering in an air atmosphere to obtain a sintered ingot of the composite material; (4) Deformation and heat treatment: The sintered ingot obtained in step (3) is subjected to deformation processing such as hot extrusion, hot rolling or ring forging according to actual needs, and the deformed ingot is heat treated according to different usage requirements.

4. The preparation method according to claim 3, characterized in that: The aluminum alloy type in step (1) is selected from one or more of 7055 aluminum alloy, 7075 aluminum alloy, 2324 aluminum alloy, and 2024 aluminum alloy.

5. The preparation method according to claim 3, characterized in that: The glass powder in step (1) is one or more of silicate glass powder, borate glass powder, phosphate glass powder and quartz glass powder.

6. The preparation method according to claim 5, characterized in that: The glass powder in step (1) is irregular or spherical in shape, with an average particle size of 0.5-10 µm and a density of 1.8-2.5 g / cm 3 .

7. The preparation method according to claim 3, characterized in that: In step (1), the aluminum powder or aluminum alloy powder and the glass powder are uniformly mixed by one or more of a V-type mixer, a double cone mixer, a rolling ball mill, a planetary ball mill, and a stirring ball mill, with a ball-to-material ratio of 2:1-20:1 and a mixing time of 4-24 hours.

8. The preparation method according to claim 3, characterized in that: The sheath material of step (2) is rubber or silicone, the green body shape is rod-shaped, plate-shaped, tubular or ring-shaped, the pressing pressure is 120-400 MPa, and the holding time is 20-150 s.

9. The preparation method according to claim 3, characterized in that: The sintering temperature of step (3) is 500-640°C, and the holding time is 1-6 h.

10. The preparation method according to claim 3, characterized in that: The deformation processing temperature in step (4) is 250-500°C, the solution temperature is 450-550°C, the quenching medium is 40-70°C water, the aging temperature is 100-200°C, and the aging time is 8-24 h.

Citation Information

Patent Citations

  • Powder metallurgic method preparation technique for glass / aluminum-base composite material

    CN101265532A

  • Conducting ring made of silicon carbide-metal composite material and preparation method thereof

    CN110814355A

  • Aluminum-based composite material and preparation method thereof

    CN116590564A

  • Glass ceramic particle reinforced aluminum-based composite material as well as preparation method and application thereof