Large-thickness high-toughness SA516Gr60 steel plate and production method thereof

By using single-pass large deformation, temperature-controlled rolling and normalized + tempering control methods in the rolling stage in the production of SA516Gr60 steel plate, the performance instability of the steel plate in terms of large thickness and high toughness is solved, and the steel plate is realized The comprehensive performance improvement meets the requirements of petrochemical production equipment to improve low hardness and impact work.

CN119040759APending Publication Date: 2024-11-29WUYANG IRON & STEEL +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411077526.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing SA516Gr60 steel plate has unstable performance in terms of large thickness and high toughness, which is difficult to meet the requirements of petrochemical production equipment to improve low hardness and simulated impact work after simulated welding. The special requirements have increased, and the existing production methods are difficult to ensure the comprehensive performance of the steel plate.

Method used

The production methods of single-pass large deformation, temperature-controlled rolling and normalized + tempering control in the rolling stage are adopted to ensure that the thickness of the steel plate is 150-170mm, and the tensile strength of the delivery and mold welding states is 450-550MPa, 1/ The impact work of -50℃ at 2 and 1/4 is ≥80J, the hardness is ≤180HB, the non-plastic transition temperature is ≤-30℃, and the steel plate performance is optimized through refining, heating and rolling and heat treatment processes.

Benefits of technology

The produced high-thickness and high toughness SA516Gr60 steel plate has stable performance, moderate strength and hardness, excellent impact performance, suitable for mass production, and meets the high requirements of petrochemical production equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040759A_ABST
    Figure CN119040759A_ABST
Patent Text Reader

Abstract

The invention discloses a large-thickness high-toughness SA516Gr60 steel plate and a production method thereof. The steel plate comprises the following chemical components: 0.11 to 0.13 percent of C, 0.2 to 0.4 percent of Si, 1.00 to 1.20 percent of Mn, less than or equal to 0.010 percent of P, less than or equal to 0.002 percent of S, 0.25 to 0.30 percent of Ni, 0.015 to 0.020 percent of Nb, 0.020 to 0.050 percent of Alt and the balance of Fe and inevitable impurities. The carbon equivalent CE is 0.35 to 0.38; the production method comprises the steps of smelting, heating and rolling, and heat treatment. The thickness of the steel plate is 150-170mm, and the finish rolling temperature is strictly controlled by adopting rough rolling single-pass large-deformation rolling and temperature-controlled rolling at the finish rolling stage; quenching and tempering processes are adopted for production in the heat treatment stage, and the steel plate is stable in delivery state and die welding state performance, moderate in strength and hardness and suitable for batch production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metallurgy and relates to a thick and high-toughness SA516Gr60 steel plate and a production method thereof. Background Art

[0002] SA516Gr60 steel is a 415MPa grade carbon steel plate for medium and low temperature pressure vessels in the ASMESA-516 / SA-516M standard. It is widely used in the petroleum, chemical, power station, boiler and other industries. It is used to make reactors, heat exchangers, separators, spherical tanks, gas tanks, liquefied gas tanks, nuclear reactor pressure vessels, boiler drums, liquefied petroleum gas cylinders, hydropower station high-pressure water pipes, turbine volutes and other equipment and components. With the substantial improvement of petrochemical refining technology and the continuous growth of product demand, petrochemical production equipment is currently developing towards large-scale development, and the processing capacity of a single set of equipment is constantly expanding. In order to ensure excellent processing performance and safety, low hardness, simulated post-welding, 1 / 2 impact energy and other requirements are generally proposed, and special requirements contracts are increasing year by year. Summary of the invention

[0003] The purpose of the present invention is to provide a thick and high-toughness SA516Gr60 steel plate and a production method thereof. The thickness of the steel plate is 150-170mm. Through single-pass large deformation, temperature-controlled rolling and normalizing + tempering control in the rolling stage, the thick steel plate produced has stable performance in the delivery state and mold welding state, moderate strength and hardness, stable comprehensive performance of the steel plate, and is suitable for mass production.

[0004] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme: A thick and high-toughness SA516Gr60 steel plate, whose chemical composition and mass percentage are: C: 0.11-0.13%, Si: 0.2-0.4%, Mn: 1.00-1.20%, P≤0.010%, S≤0.002%, Ni: 0.25-0.30%, Nb: 0.015-0.020%, Alt: 0.020-0.050%, the balance is Fe and unavoidable impurities; carbon equivalent CE: 0.35-0.38.

[0005] Furthermore, the steel plate of the present invention has a thickness of 150 to 170 mm.

[0006] Furthermore, the steel plate of the present invention is qualified if its tensile strength Rm in the delivery state and die-welded state is 450-550MPa, its impact energy at -50°C at 1 / 2 and 1 / 4 is ≥80J, its hardness is ≤180HB, and its non-plastic transition (NDT) temperature is ≤-30°C.

[0007] The steel plate mold welding process of the present invention is: 600-640°C, heat preservation for 17-20h.

[0008] The production method of the thick and high-toughness SA516Gr60 steel plate of the present invention comprises smelting, hot rolling and heat treatment processes.

[0009] Preferably, the smelting process of the present invention: the argon pressure of the refining seat is 0.8-1.5MPa, the aluminum feed is 600-800m3, the refining process [Al] is guaranteed to be ≥0.015%, the lime addition is controlled at 12-14 Kg / t, the desulfurization temperature is ≥1580℃, and the argon flow rate of the VD process is controlled at 3-7Nm3. 3 / h, the diameter of argon boiling on the steel liquid surface is 200-300mm.

[0010] Preferably, in the heating rolling process of the present invention, the steel ingot is placed in a soaking furnace with a temperature of 100-150°C, and the target temperature of the steel ingot is 1260-1280°C.

[0011] Preferably, the hot rolling process of the present invention is as follows: stage I rough rolling single pass large deformation rolling: the reduction amount during longitudinal rolling is 20-30mm, and the rolling to 280-400mm is transferred to the finishing mill for temperature-controlled rolling, stage II finishing mill rolling: starting rolling temperature is 860-880℃, single roller maximum torque is 2800-3000KNm, final rolling temperature is 800-830℃, the red return temperature is controlled at 600-650℃, and stacking is performed for 50-60h after rolling.

[0012] Preferably, the heat treatment process of the present invention includes normalizing in a thick plate quenching furnace or a car bottom furnace, with a normalizing holding temperature of 890-920°C, a holding time of 2-2.5 min / mm, water cooling to accelerate cooling, a tempering holding temperature of 630-670°C, and air cooling.

[0013] The inventive principle and beneficial technical effects of the present invention are: The present invention adopts single-pass rough rolling with large deformation, temperature-controlled rolling in the finishing rolling stage, strictly controls the final rolling temperature, and adopts normalizing + tempering process in the heat treatment stage to produce large-thickness SA516Gr60 steel plates. The thickness of the steel plates is: 150-170mm, the tensile strength Rm in the delivery state and the die-welded state is: 450-550MPa, the impact energy at -50°C at 1 / 2 and 1 / 4 is ≥80J, the hardness is ≤180HB, and the non-plastic transition (NDT) temperature is ≤-30°C to be qualified.

[0014] The steel plate of the present invention has stable impact performance, moderate strength and hardness, stable comprehensive performance and is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is the microstructure diagram of the SA516Gr60 steel plate in Example 1. DETAILED DESCRIPTION

[0016] The present invention is further described in detail below with reference to the embodiments. Example 1

[0017] The thickness of the SA516Gr60 steel plate in this embodiment is 150 mm, and its chemical composition and mass percentage are: C: 0.11%, Si: 0.2%, Mn: 1.00%, P: 0.010%, S: 0.002%, Ni: 0.25%, Nb: 0.015%, Alt: 0.020%, and the remainder is Fe and unavoidable impurities; carbon equivalent CE: 0.35.

[0018] The production method of the SA516Gr60 steel plate in this embodiment includes smelting, hot rolling, and heat treatment processes, which are specifically as follows: (1) Smelting process: The argon pressure of the refining seat is 0.8MPa, the aluminum feed is 600m3, the refining process [Al] is guaranteed to be 0.015%, the lime addition is controlled at 12 Kg / t, the desulfurization temperature is 1580℃, and the argon flow rate of the VD process is controlled at 3Nm3 3 / h, the diameter of argon boiling on the steel liquid surface is 200mm.

[0019] (2) Heating and rolling process: the steel ingot is heated in a soaking furnace, the temperature of the heated furnace is 100°C, and the target temperature of the steel ingot is 1260°C. Phase I rough rolling single pass large deformation rolling: the longitudinal rolling reduction is 20mm, and the rolling is transferred to the finishing mill for temperature control rolling when the rolling is 280mm. Phase II finishing mill rolling: the starting rolling temperature is 860°C, the maximum torque of a single roll is 2800KNm, the final rolling temperature is 800°C, and the red-return temperature is controlled at 600°C; stacking after rolling for 50h.

[0020] (3) Heat treatment process: normalizing in a car bottom furnace, normalizing holding temperature 890℃, holding time 2min / mm, water cooling to accelerate cooling, tempering holding temperature 630℃, air cooling.

[0021] The die welding process of SA516Gr60 steel plate in this embodiment is: 600°C, insulation for 17 hours.

[0022] In this embodiment, the tensile strength Rm of the SA516Gr60 steel plate in the delivery state and the die-welded state is 460MPa, the impact energy at -50°C at 1 / 2 and 1 / 4 is 120J, the hardness is 175HB, and the non-plastic transition (NDT) temperature is -30°C, which is qualified.

[0023] The microstructure of the SA516Gr60 steel plate in this embodiment is as follows: Figure 1 As shown by Figure 1 It can be seen that the microstructure is ferrite and pearlite. The microstructures of the steel plates of other embodiments are similar and are not listed one by one. Example 2

[0024] The thickness of the SA516Gr60 steel plate in this embodiment is 170 mm, and its chemical composition and mass percentage are: C: 0.13%, Si: 0.4%, Mn: 1.20%, P: 0.009%, S: 0.002%, Ni: 0.30%, Nb: 0.020%, Alt: 0.050%, and the remainder is Fe and unavoidable impurities; carbon equivalent CE: 0.38.

[0025] The production method of the SA516Gr60 steel plate in this embodiment includes smelting, hot rolling, and heat treatment processes, which are specifically as follows: (1) Smelting process: The argon pressure of the refining seat is 1.5MPa, the aluminum feed is 800m3, the refining process [Al] is guaranteed to be 0.016%, the lime addition is controlled at 14 Kg / t, the desulfurization temperature is 1590℃, and the argon flow rate of the VD process is controlled at 7Nm3 3 / h, the diameter of argon boiling on the steel liquid surface is 300mm.

[0026] (2) Heating and rolling process: the steel ingot is heated in a soaking furnace, the temperature of the heated furnace is 150°C, and the target temperature of the steel ingot is 1280°C. Stage I rough rolling single pass large deformation rolling: the longitudinal rolling reduction is 30mm, and the rolling is carried out to 400mm before the temperature control rolling of the finishing mill. Stage II finishing mill rolling: the starting rolling temperature is 880°C, the maximum torque of a single roll is 3000KNm, the final rolling temperature is 830°C, and the red-return temperature is controlled at 650°C; stacking after rolling for 60h.

[0027] (3) Heat treatment process: thick plate quenching furnace, normalizing holding temperature 920℃, holding time 2.5min / mm, water cooling for accelerated cooling, tempering holding temperature 670℃, air cooling.

[0028] The die welding process of SA516Gr60 steel plate in this embodiment is: 640°C, insulation for 20h.

[0029] The tensile strength Rm of the SA516Gr60 steel plate in the delivery state and the die-welded state in this embodiment is 520 MPa, the impact energy at -50°C at 1 / 2 and 1 / 4 is 130 J, the hardness is 170 HB, and the non-plastic transition (NDT) temperature is -35°C, which is qualified. Example 3

[0030] The thickness of the SA516Gr60 steel plate in this embodiment is 160 mm, and its chemical composition and mass percentage are: C: 0.12%, Si: 0.3%, Mn: 1.15%, P: 0.008%, S: 0.0015%, Ni: 0.27%, Nb: 0.017%, Alt: 0.030%, and the remainder is Fe and unavoidable impurities; carbon equivalent CE: 0.37.

[0031] The production method of the SA516Gr60 steel plate in this embodiment includes smelting, hot rolling, and heat treatment processes, which are specifically as follows: (1) Smelting process: The argon pressure of the refining seat is 1.0MPa, the aluminum feed is 700m3, the refining process [Al] is guaranteed to be 0.017%, the lime addition is controlled at 13 Kg / t, the desulfurization temperature is 1585℃, and the argon flow rate of the VD process is controlled at 5Nm3 3 / h, the diameter of argon boiling on the steel liquid surface is 250mm.

[0032] (2) Heating and rolling process: the steel ingot is heated in a soaking furnace, the temperature of the heated furnace is 130℃, and the target temperature of the steel ingot is 1270℃. Phase I rough rolling single pass large deformation rolling: the longitudinal rolling reduction is 25mm, and the rolling is transferred to the finishing mill for temperature control rolling when the rolling is 350mm. Phase II finishing mill rolling: the starting rolling temperature is 870℃, the maximum torque of a single roll is 2900 KNm, the final rolling temperature is 820℃, and the red return temperature is controlled at 630℃; stacking after rolling for 55h.

[0033] (3) Heat treatment process: thick plate quenching furnace, normalizing holding temperature 900℃, holding time 2.2min / mm, water cooling for accelerated cooling, tempering holding temperature 640℃, air cooling.

[0034] The die welding process of SA516Gr60 steel plate in this embodiment is: 620°C, insulation for 18 hours.

[0035] In this embodiment, the tensile strength Rm of the SA516Gr60 steel plate in the delivery state and the die-welded state is 510 MPa, the impact energy at -50°C at 1 / 2 and 1 / 4 is 140 J, the hardness is 171 HB, and the non-plastic transition (NDT) temperature is -40°C, which is qualified. Example 4

[0036] The thickness of the SA516Gr60 steel plate in this embodiment is 165 mm, and its chemical composition and mass percentage are: C: 0.12%, Si: 0.35%, Mn: 1.12%, P: 0.010%, S: 0.002%, Ni: 0.26%, Nb: 0.016%, Alt: 0.040%, and the remainder is Fe and unavoidable impurities; carbon equivalent CE: 0.37.

[0037] The production method of the SA516Gr60 steel plate in this embodiment includes smelting, hot rolling, and heat treatment processes, which are specifically as follows: (1) Smelting process: the argon pressure of the refining seat is 0.9MPa, the aluminum feed is 650m3, the refining process [Al] is guaranteed to be 0.015%, the lime addition is controlled at 13.5 Kg / t, the desulfurization temperature is 1589℃, and the argon flow rate of the VD process is controlled at 4Nm3 3 / h, the diameter of argon boiling on the steel liquid surface is 210mm.

[0038] (2) Heating and rolling process: the steel ingot is heated in a soaking furnace, the temperature of the heated furnace is 110°C, and the target temperature of the steel ingot is 1265°C. Phase I rough rolling single pass large deformation rolling: the longitudinal rolling reduction is 23mm, and the rolling is transferred to the finishing mill for temperature-controlled rolling when the rolling is 290mm. Phase II finishing mill rolling: the starting rolling temperature is 865°C, the maximum torque of a single roll is 2900KNm, the final rolling temperature is 810°C, and the red-return temperature is controlled at 610°C; stacking after rolling for 52h.

[0039] (3) Heat treatment process: normalizing in a bottom furnace, normalizing holding temperature 895°C, holding time 2.1 min / mm, water cooling to accelerate cooling, tempering holding temperature 635°C, air cooling.

[0040] The die welding process of SA516Gr60 steel plate in this embodiment is: 635°C, insulation for 19.5h.

[0041] The tensile strength Rm of the SA516Gr60 steel plate in the delivery state and the die-welded state in this embodiment is 470 MPa, the impact energy at -50°C at 1 / 2 and 1 / 4 is 110, the hardness is 169 HB, and the non-plastic transition (NDT) temperature is -35°C, which is qualified.

Claims

1. A thick and high-toughness SA516Gr60 steel plate, characterized in that: The chemical composition of the steel plate and its mass percentage are: C: 0.11-0.13%, Si: 0.2-0.4%, Mn: 1.00-1.20%, P≤0.010%, S≤0.002%, Ni: 0.25-0.30%, Nb: 0.015-0.020%, Alt: 0.020-0.050%, and the balance is Fe and unavoidable impurities; carbon equivalent CE: 0.35-0.

38.

2. The thick and high-toughness SA516Gr60 steel plate according to claim 1 is characterized in that: The steel plate has a thickness of 150 to 170 mm.

3. The thick and high-toughness SA516Gr60 steel plate according to claim 1 is characterized in that: The steel plate is qualified if its tensile strength Rm in the delivery state and die-welded state is 450-550MPa, the impact energy at -50°C at 1 / 2 and 1 / 4 is ≥80J, the hardness is ≤180HB, and the non-plastic transition (NDT) temperature is ≤-30°C.

4. The thick and high-toughness SA516Gr60 steel plate according to claim 3 is characterized in that: The steel plate mold welding process: 600-640°C, heat preservation 17-20h.

5. A method for producing a thick and high-toughness SA516Gr60 steel plate according to any one of claims 1 to 4, characterized in that: Including smelting, hot rolling and heat treatment processes.

6. The method for producing a thick and high-toughness SA516Gr60 steel plate according to claim 5, characterized in that: The smelting process: the argon pressure of the refining seat is 0.8-1.5MPa, the aluminum feed is 600-800m3, the refining process [Al] is guaranteed to be ≥0.015%, the lime addition is controlled at 12-14 Kg / t, the desulfurization temperature is ≥1580℃, and the argon flow rate of the VD process is controlled at 3-7Nm3 3 / h, the diameter of argon boiling on the steel liquid surface is 200-300mm.

7. The method for producing a thick and high-toughness SA516Gr60 steel plate according to claim 5, characterized in that: The heating rolling process includes: the steel ingot is placed in a soaking furnace with a temperature of 100-150°C, and the target temperature of the steel ingot is 1260-1280°C.

8. The method for producing a thick and high-toughness SA516Gr60 steel plate according to claim 5, characterized in that: The heating rolling process includes: stage I rough rolling single pass large deformation rolling: longitudinal rolling reduction of 20-30 mm, rolling to 280-400 mm and then turning to the finishing mill for temperature controlled rolling; stage II finishing mill rolling: starting rolling temperature of 860-880°C, single roller maximum torque of 2800-3000 KNm, final rolling temperature of 800-830°C, and controlled red-returning temperature of 600-650°C; stacking for 50-60 hours after rolling.

9. The method for producing a thick and high-toughness SA516Gr60 steel plate according to claim 5, characterized in that: The heat treatment process includes normalizing in a thick plate quenching furnace or a car bottom furnace, normalizing holding temperature of 890-920°C, holding time of 2-2.5min / mm, water cooling for accelerated cooling, tempering holding temperature of 630-670°C, and air cooling.