Preparation method of 600 DEG C high-temperature titanium alloy sheet for superplastic forming
Through the rolling route of near constant temperature and large deformation combined with intermediate quenching, the problem of the inability to prepare 600℃ high-temperature titanium alloy thin plates in the existing technology has been solved, and the high-temperature strength and superplasticity of titanium alloy thin plates have been improved, meeting the high-temperature performance needs of aerospace equipment are achieved. .
Patent Information
- Application Number
- CN202411196402.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art cannot effectively prepare super-plastic titanium alloy thin plates for high temperatures of 600°C, and cannot meet the high-temperature performance requirements of aerospace equipment components.
The rolling route with near constant temperature and large deformation combined with intermediate quenching is adopted. By controlling the rolling temperature and deformation amount, a large amount of equiaxed α phases exist in the titanium alloy structure, which improves high temperature strength and superplasticity, and achieves it through a small number of rolling passes. Rolling near constant temperature ensures smooth forming of the plate.
A 600℃ titanium alloy thin plate with excellent superplastic forming performance and high-temperature long-lasting performance was prepared to meet the high-temperature use needs of aerospace equipment and fill the gap in the preparation technology of 600℃ high-temperature titanium alloy superplastic plates.
Smart Images

Figure CN119040781A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium and titanium alloy sheet preparation, and specifically relates to a method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming. Background Art
[0002] Titanium alloy has many advantages such as low density, high strength, corrosion resistance, high temperature resistance, non-magnetic, small linear expansion coefficient, etc. It is widely used in aerospace, automobile and shipbuilding, petrochemical, biomedicine and marine engineering. The main advantage of titanium alloy is its high specific strength. Replacing traditional steel and high-temperature alloys can reduce weight by about 40%. In addition, titanium alloy has good processing performance and can be processed into large-sized parts with complex structures to meet the needs of structural designers. With these advantages, titanium alloy has been used to manufacture aircraft engine blades, blisks, integral blisks, drums, suspensions, integral frames and landing gears and other parts.
[0003] In recent years, with the gradual increase in the thrust-to-weight ratio of aircraft engines, the operating temperature of titanium alloys has gradually increased from 300°C to 600°C, while the conventional high-temperature titanium alloys used for superplastic forming are TC4 and SP700, and their maximum operating temperature is 400°C, which can no longer meet the needs of 600°C high-temperature components. The three patents with publication numbers CN1037885684A, CN103934301A and CN106955893A all mention the preparation of high-temperature titanium alloy plates for superplastic forming, but the maximum operating temperature of the plates is 500°C. The patent with publication number CN109750185A provides a method for preparing a high-temperature titanium alloy plate for short-term use at 650°C, but it does not describe the high-temperature durability of the plate. From the current status of the above technical research, it can be seen that there are few reports on 600°C high-temperature titanium alloy plates for superplastic forming. Therefore, in order to meet the needs of aerospace equipment components, it is urgent to develop a preparation technology for high-temperature titanium alloy thin plates with excellent superplastic properties and capable of long-term service at 600°C. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming in view of the deficiencies of the above-mentioned prior art. The method adopts a rolling route of near-constant temperature large deformation combined with intermediate quenching, and controls the rolling temperature to ensure that there are a large number of equiaxed α phases in the titanium alloy structure, so that the sheet has a higher high-temperature strength, and adopts a larger rolling deformation to improve the recrystallization ability and increase the superplasticity of the sheet, and adopts fewer rolling passes to achieve near-constant temperature rolling, ensuring smooth forming of the sheet, and obtaining a titanium alloy sheet with excellent superplastic forming performance and used at 600°C, filling the gap in the prior art field.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming, characterized in that the method comprises the following steps:
[0006] Step 1: Apply high-temperature anti-oxidation coating to the entire surface of the titanium alloy slab, and after the surface is completely dry, put it into a roller hearth furnace for heat preservation and heat treatment. When the temperature reaches the time, after the heat preservation and heat treatment is completed, perform one-fire rolling to obtain a semi-finished slab of one fire; the total deformation of the one-fire rolling does not exceed 70%;
[0007] Step 2, grinding the upper and lower surfaces of the semi-finished slab obtained in step 1, and then cutting it into pieces by two fires, and then brushing the surface of the cut semi-finished slab by high temperature anti-oxidation coating, putting it into a roller hearth furnace for heat preservation after the surface is completely dry, and after the temperature is reached, rolling it into two fires after the heat preservation is completed to obtain the semi-finished slab by two fires; the total deformation of the two fires rolling does not exceed 70%, and the rolling direction is the same as the direction of the one fire rolling in step 1;
[0008] Step 3: Place the semi-finished slab obtained in step 2 into a resistance furnace for heat preservation treatment, and when the temperature reaches the timer, place the slab into a quenching tank for quenching treatment after the heat preservation treatment is completed;
[0009] Step 4: grind the semi-finished slab after quenching in step 3, apply high-temperature anti-oxidation coating on the surface, put it into a roller hearth furnace for heat preservation after the surface is completely dry, and perform three-fire rolling after the heat preservation is completed to obtain a three-fire semi-finished slab; the total deformation of the three-fire rolling does not exceed 60%, and the rolling direction is the same as the direction of the two-fire rolling in step 2;
[0010] Step 5, grinding the upper and lower surfaces of the three-fired semi-finished slab obtained in step 4, and then cutting it into four-fired pieces, and then putting the cut three-rolled slab into a roller hearth furnace for heat preservation and heat treatment, and when the temperature reaches the time, after the heat preservation and heat treatment is completed, four-fire rolling is performed to obtain a four-fired semi-finished slab; the total deformation of the four-fire rolling does not exceed 60%, and the rolling direction is perpendicular to the direction of the three-fire rolling in step 4;
[0011] Step 6: Cut the four-fire semi-finished slab obtained in step 5 into pieces, and then use 3 to 4 pieces of the cut four-fire semi-finished slab as a group, and use steel plates to package and weld them to obtain a coated rolling package;
[0012] Step 7, subjecting the clad rolling package obtained in step 6 to a heat preservation treatment, and after the temperature reaches the time, subjecting the clad rolling to the completion of the heat preservation treatment, to obtain a semi-finished titanium alloy plate; the total deformation of the clad rolling does not exceed 80%, and the rolling direction is the same as the direction of the four-fire rolling in step 5;
[0013] Step 8: subjecting the semi-finished titanium alloy sheet obtained in step 7 to shape correction annealing, water sanding and pickling to obtain a 600°C high-temperature titanium alloy sheet for superplastic forming; the thickness of the titanium alloy sheet is 0.8 mm to 1.2 mm.
[0014] The above-mentioned method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming is characterized in that the high-temperature anti-oxidation coating in step 1 is GZH-4, and the insulation temperature T1 of the insulation heat treatment is (T β -10~25)℃, holding time t1=(H1+110~140)min, H1 is the thickness of titanium alloy plate blank, unit is mm; the deformation rate of the first hot rolling is not more than 30%, and the total rolling process is not more than 4 times.
[0015] The above-mentioned method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming is characterized in that the high-temperature anti-oxidation coating in step 2 is GZH-4, and the insulation temperature T2 of the insulation heat treatment is (T β -50~80)℃, holding time t2=(H2+90~120)min, H2 is the thickness of the semi-finished plate after slitting, in mm; the deformation rate of the second-fire rolling pass is not more than 30%, and the total rolling process does not exceed 5 times.
[0016] The above-mentioned method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming is characterized in that the insulation temperature T3 of the insulation heat treatment in step 3 is (T β +15~30)℃, holding time t3=(H3+60~90)min, H3 is the thickness of the second-fire semi-finished plate blank, in mm; the medium for the quenching treatment is room temperature circulating water.
[0017] The above-mentioned method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming is characterized in that the high-temperature anti-oxidation coating in step 4 is GZH-4; the insulation temperature T4 of the insulation heat treatment is (T β -50~80)℃, holding time t4=(H3+60~90)min, H3 is the thickness of the semi-finished plate billet after two fires, in mm; the deformation rate of the three-fire rolling pass is not more than 25%, and the total rolling process does not exceed 5 times.
[0018] The above-mentioned method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming is characterized in that the insulation temperature T5 of the insulation heat treatment in step 5 is (T β -50~80)℃, holding time t5=(H4+40~60)min, H4 is the thickness of the three-fire semi-finished plate after slitting, in mm; the deformation rate of the four-fire rolling pass is not more than 25%, and the total rolling process does not exceed 5 times.
[0019] The above-mentioned method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming is characterized in that the thickness of the steel plate in the cladding rolling package in step six is 20 mm.
[0020] The above-mentioned method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming is characterized in that the insulation temperature T6 of the insulation heat treatment in step 7 is (T β -50~80)℃, holding time t6=(H5+60~90)min, H5 is the thickness of the cladding rolling material, in mm; the deformation rate of the cladding rolling pass is not more than 25%, and the total rolling process does not exceed 8 times.
[0021] The above-mentioned method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming is characterized in that the temperature of the shape correction annealing treatment in step eight is 550°C to 800°C, and the insulation time is 120min to 360min.
[0022] The above-mentioned method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming is characterized in that the room temperature tensile strength of the 600°C high-temperature titanium alloy sheet for superplastic forming in step eight is above 1100MPa, the yield strength is above 1000MPa, and the elongation is above 10%; the 600°C tensile strength is above 600MPa, the yield strength is above 550MPa, the elongation is above 12%, the 600°C endurance strength is 200MPa, and the endurance time is above 100h; at 900°C to 950°C and a tensile rate of 10 - 4 s -1 ~10 -3 s -1 Under these conditions, the superplastic elongation of titanium alloy sheet is over 500%.
[0023] The chemical composition (by weight percentage) of the 600°C high-temperature titanium alloy thin plate of the present invention includes: Al 5.2% to 6.5%, Sn 3.0% to 4.5%, Zr 2.5% to 4.0%, Mo 0.2% to 1.2%, Si 0.2% to 0.6%, Ta 0.7% to 1.5%, Nb 0.2% to 0.7%, Fe≤0.25%, C 0.04% to 0.08%, O≤0.15%, and the balance is Ti.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] 1. The present invention adopts a rolling route of near-constant temperature large deformation combined with intermediate quenching. The rolling temperature is controlled to be below the temperature of the β phase transformation point of the titanium alloy to ensure that there are a large number of equiaxed α phases in the titanium alloy structure, thereby ensuring that the titanium alloy sheet has high high-temperature strength. The titanium alloy structure is fully broken by adopting a large rolling deformation amount, and the recrystallization ability is improved, thereby effectively increasing the superplasticity of the titanium alloy sheet. At the same time, by adopting fewer rolling passes, the temperature loss is significantly reduced, and near-constant temperature rolling is achieved, which reduces the risk of cracking during the rolling process, ensures the smooth forming of the plate, and obtains a titanium alloy sheet with excellent superplastic forming performance and can be used at 600°C.
[0026] 2. In the preparation process of the present invention, the semi-finished slab after two-fire rolling is quenched in the β phase region, so that finer lamellae α are generated in the slab structure, and the deformation texture formed in the previous rolling process can be eliminated, thereby ensuring the refinement of the structure in the subsequent deformation process.
[0027] 3. The present invention adopts one reversal during the rolling process, i.e., four-fire rolling, which effectively reduces the deformation texture strength caused by the rolling process, reduces the anisotropy of the titanium alloy sheet, and ensures uniform forming during later use.
[0028] 4. The titanium alloy thin plate prepared by the present invention has excellent superplastic forming performance, with a superplastic elongation of more than 500% at 900℃~950℃, and a high yield strength at 600℃ with excellent high-temperature durability, which meets the needs of aerospace equipment components and fills the gap in the preparation technology of 600℃ high-temperature titanium alloy superplastic plates.
[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is the metallographic structure diagram (200×) of the 600°C high-temperature titanium alloy sheet for superplastic forming prepared in Example 1 of the present invention.
[0031] Figure 2 This is the metallographic structure diagram (200×) of the 600°C high-temperature titanium alloy thin plate for superplastic forming prepared in Example 2 of the present invention.
[0032] Figure 3 This is the metallographic structure diagram (200×) of the 600°C high-temperature titanium alloy sheet for superplastic forming prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0033] Example 1
[0034] This embodiment includes the following steps:
[0035] Step 1: Apply high-temperature anti-oxidation coating GZH-4 to the entire surface of the titanium alloy slab with a specification of thickness × width × length of 130mm × 830mm × 1000mm, and put it into a roller hearth furnace for heat treatment after the surface is completely dry. When the temperature reaches the time, the heat preservation temperature T1 = (T β -10~25)℃, holding time t1=240min, after the holding heat treatment is completed, first-fire rolling is carried out, the total deformation of first-fire rolling does not exceed 70%, it is divided into 3 passes, the pressing deformation rate of each pass is 26%, 23%, 20% respectively, to obtain a first-fire semi-finished slab with a thickness of 60mm;
[0036] Step 2: Grind the upper and lower surfaces of the semi-finished slab obtained in step 1 and cut it into pieces for the second fire. Then, apply the high-temperature anti-oxidation coating GZH-4 on the surface of the cut semi-finished slab. After the surface is completely dry, put it into a roller hearth furnace for heat insulation treatment. When the temperature reaches the time, the insulation temperature T2 = (T β -50~80)℃, holding time t2=180min, after the holding heat treatment is completed, the second-fire rolling is carried out, the total deformation of the second-fire rolling does not exceed 70%, it is divided into 4 passes, the pressing deformation rate of each pass is 25%, 27%, 19%, 23% respectively, and the rolling direction is the same as the first-fire rolling direction in step 1, and the second-fire semi-finished slab with a thickness of 20mm is obtained;
[0037] Step 3: Place the semi-finished slab obtained in step 2 into a resistance furnace for heat preservation treatment. When the temperature reaches the time, the heat preservation temperature of the heat preservation treatment is T3 = (T β +15~30)℃, insulation time t3=120min, after the insulation heat treatment is completed, put it into the quenching tank for quenching treatment, and the quenching medium is room temperature circulating water;
[0038] Step 4: After grinding, apply high-temperature anti-oxidation coating GZH-4 on the surface of the semi-finished slab after quenching in step 3, and put it into a roller hearth furnace for heat preservation after the surface is completely dry. When the temperature reaches the time, the insulation temperature T4 = (T β -50~80)℃, holding time t4=120min, after the holding heat treatment is completed, three-fire rolling is performed, the total deformation of the three-fire rolling does not exceed 60%, it is divided into 3 passes, the pressing deformation rate of each pass is 17%, 24%, 16% respectively, and the rolling direction is the same as the direction of the two-fire rolling in step 2, and a three-fire semi-finished slab with a thickness of 10.5mm is obtained;
[0039] Step 5: Grind the upper and lower surfaces of the three-fired semi-finished slab obtained in step 4, and then cut it into four-fired pieces. Then put the cut three-fired semi-finished slab into a roller hearth furnace for heat preservation. When the temperature reaches the time, the insulation temperature T5 = (T β-50~80)℃, holding time t5=60min, after the holding heat treatment is completed, four-fire rolling is performed, the total deformation of the four-fire rolling does not exceed 60%, it is divided into 3 passes, the pressing deformation rate of each pass is 19%, 17%, 14% respectively, and the rolling direction is perpendicular to the direction of the three-fire rolling in step 4, and a four-fire semi-finished slab with a thickness of 6mm is obtained;
[0040] Step 6: Cut the four-fire semi-finished slab obtained in step 5 into pieces, and then use 3 pieces of the cut four-fire semi-finished slab as a group, and use a steel plate with a thickness of 20 mm for assembly welding to obtain a coated rolling package with a size of thickness × length × width of 56.6 mm × 1165 mm × 745 mm;
[0041] Step 7: The coated rolled package obtained in step 6 is subjected to heat preservation heat treatment. When the temperature reaches the temperature, the insulation temperature T6 = (T β -50~80)℃, holding time t6=120min, after the holding heat treatment is completed, cladding rolling is performed, the total deformation of cladding rolling does not exceed 80%, and it is divided into 6 passes, and the pressing deformation rate of each pass is 21%, 22%, 23%, 22%, 19%, 14% respectively, and the rolling direction is the same as the direction of the four-fire rolling in step 5, and a semi-finished titanium alloy plate with a thickness of 1.5mm is obtained after unpacking;
[0042] Step 8: The semi-finished titanium alloy sheet obtained in step 7 is subjected to a shape correction annealing treatment at a temperature of 550°C to 800°C for a holding time of 140 min, and then subjected to water sanding and pickling treatment to obtain a 600°C high-temperature titanium alloy sheet for superplastic forming having a thickness of 1.2 mm; the chemical composition (by weight percentage) of the titanium alloy sheet includes: Al 5.7%, Sn 3.4%, Zr 3.0%, Mo 0.5%, Si 0.33%, Ta 0.94%, Nb 0.44%, Fe 0.20%, C 0.07%, O 0.12%, and the remainder is Ti.
[0043] Figure 1 The metallographic structure diagram (200×) of the 600°C high-temperature titanium alloy sheet for superplastic forming prepared in this embodiment is shown in FIG. Figure 1 It can be seen that the metallographic structure of the 600°C high-temperature titanium alloy sheet for superplastic forming is an equiaxed structure.
[0044] After testing, the room temperature tensile strength of the 600℃ high temperature titanium alloy sheet for superplastic forming prepared in this embodiment is 1103MPa, the yield strength is 1033MPa, and the elongation is 19.5%; the 600℃ tensile strength is 720MPa, the yield strength is 581MPa, and the elongation is 19.5%. Under the conditions of 600℃ and 200MPa, it can be continuously loaded for 100h without breaking; under the conditions of 940℃ and tensile rate of 7.7×10-4 s -1 Under these conditions, the superplastic elongation of titanium alloy sheet is 641%.
[0045] Example 2
[0046] This embodiment includes the following steps:
[0047] Step 1: Apply high-temperature anti-oxidation coating GZH-4 to the entire surface of the titanium alloy slab with a specification of thickness × width × length of 130mm × 830mm × 1000mm, and put it into a roller hearth furnace for heat treatment after the surface is completely dry. When the temperature reaches the time, the heat preservation temperature T1 = (T β -10~25)℃, holding time t1=240min, after the holding heat treatment is completed, first-fire rolling is carried out, the total deformation of first-fire rolling does not exceed 70%, it is divided into 3 passes, the pressing deformation rate of each pass is 25%, 24%, 21% respectively, and the first-fire semi-finished slab with a thickness of 59mm is obtained;
[0048] Step 2: Grind the upper and lower surfaces of the semi-finished slab obtained in step 1 and cut it into pieces for the second fire. Then, apply the high-temperature anti-oxidation coating GZH-4 on the surface of the cut semi-finished slab. After the surface is completely dry, put it into a roller hearth furnace for heat insulation treatment. When the temperature reaches the time, the insulation temperature T2 = (T β -50~80)℃, holding time t2=170min, after the holding heat treatment is completed, the second-fire rolling is carried out, the total deformation of the second-fire rolling does not exceed 70%, it is divided into 4 passes, the pressing deformation rate of each pass is 25%, 27%, 25%, 20% respectively, and the rolling direction is the same as the first-fire rolling direction in step 1, and the second-fire semi-finished slab with a thickness of 19mm is obtained;
[0049] Step 3: Place the semi-finished slab obtained in step 2 into a resistance furnace for heat preservation treatment. When the temperature reaches the time, the heat preservation temperature of the heat preservation treatment is T3 = (T β +15~30)℃, insulation time t3=100min, after the insulation heat treatment is completed, put it into the quenching tank for quenching treatment, and the quenching medium is room temperature circulating water;
[0050] Step 4: After grinding, apply high-temperature anti-oxidation coating GZH-4 on the surface of the semi-finished slab after quenching in step 3, and put it into a roller hearth furnace for heat preservation after the surface is completely dry. When the temperature reaches the time, the insulation temperature T4 = (T β-50~80)℃, holding time t4=90min, after the holding heat treatment is completed, three-fire rolling is performed, the total deformation of the three-fire rolling does not exceed 60%, it is divided into 3 passes, the pressing deformation rate of each pass is 18%, 25%, 18% respectively, and the rolling direction is the same as the direction of the two-fire rolling in step 2, and a three-fire semi-finished slab with a thickness of 9.5mm is obtained;
[0051] Step 5: Grind the upper and lower surfaces of the three-fired semi-finished slab obtained in step 4, and then cut it into four-fired pieces. Then put the cut three-fired semi-finished slab into a roller hearth furnace for heat preservation. When the temperature reaches the time, the insulation temperature T5 = (T β -50~80)℃, holding time t5=60min, after the holding heat treatment is completed, four-fire rolling is performed, the total deformation of four-fire rolling does not exceed 60%, it is divided into 3 passes, the pressing deformation rate of each pass is 16%, 19%, 15% respectively, and the rolling direction is perpendicular to the direction of three-fire rolling in step 4, to obtain a four-fire semi-finished slab with a thickness of 5.5mm;
[0052] Step 6: Cut the four-fire semi-finished slab obtained in step 5 into pieces, and then use 4 pieces of the cut four-fire semi-finished slab as a group, and use a steel plate with a thickness of 20 mm for assembly welding to obtain a coated rolling package with a size of thickness × length × width of 58.8 mm × 1175 mm × 895 mm;
[0053] Step 7: The coated rolled package obtained in step 6 is subjected to heat preservation heat treatment. When the temperature reaches the temperature, the insulation temperature T6 = (T β -50~80)℃, holding time t6=130min, after the holding heat treatment is completed, cladding rolling is performed, the total deformation of cladding rolling does not exceed 80%, and it is divided into 6 passes, and the pressing deformation rate of each pass is 20%, 25%, 25%, 22%, 21%, 14% respectively, and the rolling direction is the same as the direction of the four-fire rolling in step 5, and a semi-finished titanium alloy plate with a thickness of 1.3mm is obtained after unpacking;
[0054] Step 8: The semi-finished titanium alloy sheet obtained in step 7 is subjected to a shape correction annealing treatment at a temperature of 550°C to 800°C for a holding time of 140 min, and then subjected to water sanding and pickling treatment to obtain a 600°C high-temperature titanium alloy sheet for superplastic forming having a thickness of 1.0 mm; the chemical composition (by weight percentage) of the titanium alloy sheet includes: Al 5.6%, Sn 3.7%, Zr 3.2%, Mo 0.75%, Si 0.5%, Ta 1.2%, Nb 0.55%, Fe 0.21%, C 0.067%, O 0.12%, and the remainder is Ti.
[0055] Figure 2The metallographic structure diagram (200×) of the 600°C high-temperature titanium alloy sheet for superplastic forming prepared in this embodiment is shown in FIG. Figure 2 It can be seen that the metallographic structure of the 600°C high-temperature titanium alloy sheet for superplastic forming is an equiaxed structure.
[0056] After testing, the room temperature tensile strength of the 600℃ high temperature titanium alloy sheet for superplastic forming prepared in this embodiment is 1231MPa, the yield strength is 1157MPa, and the elongation is 16.8%; the 600℃ tensile strength is 748MPa, the yield strength is 573MPa, and the elongation is 15.0%. Under the conditions of 600℃ and 200MPa, it can be continuously loaded for 100h without breaking; under the conditions of 930℃ and tensile rate of 1.3×10 -4 s -1 Under these conditions, the superplastic elongation of titanium alloy sheet is 846%.
[0057] Example 3
[0058] This embodiment includes the following steps:
[0059] Step 1: Apply high-temperature anti-oxidation coating GZH-4 to the entire surface of the titanium alloy slab with a specification of thickness × width × length of 130mm × 830mm × 1000mm, and put it into a roller hearth furnace for heat treatment after the surface is completely dry. When the temperature reaches the time, the heat preservation temperature T1 = (T β -10~25)℃, holding time t1=250min, after the holding heat treatment is completed, first-fire rolling is carried out, the total deformation of first-fire rolling does not exceed 70%, it is divided into 3 passes, the pressing deformation rate of each pass is 25%, 24%, 21% respectively, and the first-fire semi-finished slab with a thickness of 59mm is obtained;
[0060] Step 2: Grind the upper and lower surfaces of the semi-finished slab obtained in step 1 and cut it into pieces for the second fire. Then, apply the high-temperature anti-oxidation coating GZH-4 on the surface of the cut semi-finished slab. After the surface is completely dry, put it into a roller hearth furnace for heat insulation treatment. When the temperature reaches the time, the insulation temperature T2 = (T β -50~80)℃, holding time t2=180min, after the holding heat treatment is completed, the second-fire rolling is carried out, the total deformation of the second-fire rolling does not exceed 70%, it is divided into 4 passes, the pressing deformation rate of each pass is 25%, 27%, 25%, 21% respectively, and the rolling direction is the same as the first-fire rolling direction in step 1, and the second-fire semi-finished slab with a thickness of 19mm is obtained;
[0061] Step 3: Place the semi-finished slab obtained in step 2 into a resistance furnace for heat preservation treatment. When the temperature reaches the time, the heat preservation temperature of the heat preservation treatment is T3 = (T β+15~30)℃, insulation time t3=100min, after the insulation heat treatment is completed, put it into the quenching tank for quenching treatment, and the quenching medium is room temperature circulating water;
[0062] Step 4: After grinding, apply high-temperature anti-oxidation coating GZH-4 on the surface of the semi-finished slab after quenching in step 3, and put it into a roller hearth furnace for heat preservation after the surface is completely dry. When the temperature reaches the time, the insulation temperature T4 = (T β -50~80)℃, holding time t4=100min, after the holding heat treatment is completed, three-fire rolling is performed, the total deformation of the three-fire rolling does not exceed 60%, it is divided into 3 passes, the pressing deformation rate of each pass is 24%, 24%, 23% respectively, and the rolling direction is the same as the direction of the two-fire rolling in step 2, and a three-fire semi-finished slab with a thickness of 8.5mm is obtained;
[0063] Step 5: Grind the upper and lower surfaces of the three-fired semi-finished slab obtained in step 4, and then cut it into four-fired pieces. Then put the cut three-fired semi-finished slab into a roller hearth furnace for heat preservation. When the temperature reaches the time, the insulation temperature T5 = (T β -50~80)℃, holding time t5=50min, after the holding heat treatment is completed, four-fire rolling is performed, the total deformation of the four-fire rolling does not exceed 60%, it is divided into 3 passes, the pressing deformation rate of each pass is 18%, 14%, 17% respectively, and the rolling direction is perpendicular to the direction of the three-fire rolling in step 4, and a four-fire semi-finished slab with a thickness of 5mm is obtained;
[0064] Step 6: Cut the four-fire semi-finished slab obtained in step 5 into pieces, and then use 4 pieces of the cut four-fire semi-finished slab as a group, and use a steel plate with a thickness of 20 mm for assembly welding to obtain a coated rolling package with a size of thickness × length × width of 58.0 mm × 1155 mm × 775 mm;
[0065] Step 7: The coated rolled package obtained in step 6 is subjected to heat preservation heat treatment. When the temperature reaches the temperature, the insulation temperature T6 = (T β -50~80)℃, holding time t6=130min, after the holding heat treatment is completed, cladding rolling is performed, the total deformation of cladding rolling does not exceed 80%, and it is divided into 6 passes, and the pressing deformation rate of each pass is 22%, 25%, 24%, 24%, 23%, and 11% respectively, and the rolling direction is the same as the direction of the four-fire rolling in step 5, and a semi-finished titanium alloy plate with a thickness of 1.1mm is obtained after unpacking;
[0066] Step 8: The semi-finished titanium alloy sheet obtained in step 7 is subjected to a shape correction annealing treatment at a temperature of 550°C to 800°C for a holding time of 140 min, and then subjected to water sanding and pickling treatment to obtain a 600°C high-temperature titanium alloy sheet for superplastic forming having a thickness of 0.8 mm; the chemical composition (by weight percentage) of the titanium alloy sheet includes: Al 5.8%, Sn 3.4%, Zr 3.6%, Mo 0.8%, Si 0.5%, Ta 0.8%, Nb 0.6%, Fe 0.18%, C 0.06%, O 0.12%, and the remainder is Ti.
[0067] Figure 3 The metallographic structure diagram (200×) of the 600°C high-temperature titanium alloy sheet for superplastic forming prepared in this embodiment is shown in FIG. Figure 3 It can be seen that the metallographic structure of the 600°C high-temperature titanium alloy sheet for superplastic forming is an equiaxed structure.
[0068] After testing, the room temperature tensile strength of the 600℃ high temperature titanium alloy sheet for superplastic forming prepared in this embodiment is 1224MPa, the yield strength is 1161MPa, and the elongation is 15.3%; the 600℃ tensile strength is 719MPa, the yield strength is 570MPa, and the elongation is 18.5%. Under the conditions of 600℃ and 200MPa, it can be continuously loaded for 100h without breaking; under the conditions of 930℃ and tensile rate of 7.7×10 -4 s -1 Under these conditions, the superplastic elongation of titanium alloy sheet is 821%.
[0069] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a 600°C high-temperature titanium alloy sheet for superplastic forming, characterized in that: The method comprises the following steps: Step 1: Apply high-temperature anti-oxidation coating to the entire surface of the titanium alloy slab, and after the surface is completely dry, put it into a roller hearth furnace for heat preservation and heat treatment. When the temperature reaches the time, after the heat preservation and heat treatment is completed, perform one-fire rolling to obtain a semi-finished slab of one fire; the total deformation of the one-fire rolling does not exceed 70%; Step 2, grinding the upper and lower surfaces of the semi-finished slab obtained in step 1, and then cutting it into pieces by two fires, and then brushing the surface of the cut semi-finished slab by high temperature anti-oxidation coating, putting it into a roller hearth furnace for heat preservation after the surface is completely dry, and after the temperature is reached, rolling it into two fires after the heat preservation is completed to obtain the semi-finished slab by two fires; the total deformation of the two fires rolling does not exceed 70%, and the rolling direction is the same as the direction of the one fire rolling in step 1; Step 3: Place the semi-finished slab obtained in step 2 into a resistance furnace for heat preservation treatment, and when the temperature reaches the timer, place it into a quenching tank for quenching treatment after the heat preservation treatment is completed; Step 4: grind the semi-finished slab after quenching in step 3, apply high-temperature anti-oxidation coating on the surface, put it into a roller hearth furnace for heat preservation after the surface is completely dry, and perform three-fire rolling after the heat preservation is completed to obtain a three-fire semi-finished slab; the total deformation of the three-fire rolling does not exceed 60%, and the rolling direction is the same as the direction of the two-fire rolling in step 2; Step 5, grinding the upper and lower surfaces of the three-fired semi-finished slab obtained in step 4, and then cutting it into four-fired pieces, and then putting the cut three-rolled slab into a roller hearth furnace for heat preservation and heat treatment, and when the temperature reaches the time, after the heat preservation and heat treatment is completed, four-fire rolling is performed to obtain a four-fired semi-finished slab; the total deformation of the four-fire rolling does not exceed 60%, and the rolling direction is perpendicular to the direction of the three-fire rolling in step 4; Step 6: Cut the four-fire semi-finished slab obtained in step 5 into pieces, and then use 3 to 4 pieces of the cut four-fire semi-finished slab as a group, and use steel plates to package and weld them to obtain a coated rolling package; Step 7, subjecting the clad rolling package obtained in step 6 to a heat preservation treatment, and after the temperature reaches the time, subjecting the clad rolling to the completion of the heat preservation treatment, to obtain a semi-finished titanium alloy plate; the total deformation of the clad rolling does not exceed 80%, and the rolling direction is the same as the direction of the four-fire rolling in step 5; Step 8: subjecting the semi-finished titanium alloy sheet obtained in step 7 to shape correction annealing, water sanding and pickling to obtain a 600°C high-temperature titanium alloy sheet for superplastic forming; the thickness of the titanium alloy sheet is 0.8 mm to 1.2 mm.
2. The method for preparing a 600°C high temperature titanium alloy sheet for superplastic forming according to claim 1, characterized in that: The high temperature anti-oxidation coating in step 1 is GZH-4, and the insulation temperature of the insulation heat treatment is T1=(T β -10~25)℃, holding time t1=(H1+110~140)min, H1 is the thickness of titanium alloy plate blank, unit is mm; the deformation rate of the first hot rolling is not more than 30%, and the total rolling process is not more than 4 times.
3. The method for preparing a 600°C high temperature titanium alloy sheet for superplastic forming according to claim 1, characterized in that: The high temperature anti-oxidation coating in step 2 is GZH-4, and the insulation temperature of the insulation heat treatment is T2 = (T β -50~80)℃, holding time t2=(H2+90~120)min, H2 is the thickness of the semi-finished plate after slitting, in mm; the deformation rate of the second-fire rolling pass is not more than 30%, and the total rolling process does not exceed 5 times.
4. The method for preparing a 600°C high temperature titanium alloy sheet for superplastic forming according to claim 1, characterized in that: The holding temperature T3 of the heat treatment in step 3 is (T β +15~30)℃, holding time t3=(H3+60~90)min, H3 is the thickness of the second-fired semi-finished plate blank, in mm; the medium for the quenching treatment is room temperature circulating water.
5. The method for preparing a 600°C high temperature titanium alloy sheet for superplastic forming according to claim 1, characterized in that: The high temperature anti-oxidation coating in step 4 is GZH-4; the insulation temperature of the insulation heat treatment is T4 = (T β -50~80)℃, holding time t4=(H3+60~90)min, H3 is the thickness of the semi-finished plate billet after two fires, in mm; the deformation rate of the three-fire rolling pass is not more than 25%, and the total rolling process does not exceed 5 times.
6. The method for preparing a 600°C high temperature titanium alloy sheet for superplastic forming according to claim 1, characterized in that: The holding temperature T5 of the heat treatment in step 5 is (T β -50~80)℃, holding time t5=(H4+40~60)min, H4 is the thickness of the three-fire semi-finished plate after slitting, in mm; the deformation rate of the four-fire rolling pass is not more than 25%, and the total rolling process does not exceed 5 times.
7. The method for preparing a 600°C high temperature titanium alloy sheet for superplastic forming according to claim 1, characterized in that: The thickness of the steel plate in the clad rolling package described in step six is 20 mm.
8. The method for preparing a 600°C high temperature titanium alloy sheet for superplastic forming according to claim 1, characterized in that: The holding temperature T6 of the heat treatment in step 7 is (T β -50~80)℃, holding time t6=(H5+60~90)min, H5 is the thickness of the cladding rolling material, in mm; the deformation rate of the cladding rolling pass is not more than 25%, and the total rolling process does not exceed 8 times.
9. The method for preparing a 600°C high temperature titanium alloy sheet for superplastic forming according to claim 1, characterized in that: The temperature of the shape correction annealing treatment in step eight is 550° C. to 800° C., and the holding time is 120 min to 360 min.
10. The method for preparing a 600°C high temperature titanium alloy sheet for superplastic forming according to claim 1, characterized in that: The room temperature tensile strength of the 600°C high temperature titanium alloy sheet for superplastic forming in step eight is above 1100MPa, the yield strength is above 1000MPa, and the elongation is above 10%; the 600°C tensile strength is above 600MPa, the yield strength is above 550MPa, the elongation is above 12%, the 600°C endurance strength is 200MPa, and the endurance time is above 100h; at 900°C to 950°C and a tensile rate of 10 -4 s -1 ~10 -3 s -1 Under these conditions, the superplastic elongation of titanium alloy sheet is over 500%.
Citation Information
Cited By
Hot rolling method of isotropic SP700 titanium alloy wide thin plate
CN120268797A