Hardness accelerant for cyanide-free electrogilding

By using 2-picolinic acid, 3-picolinic acid or 4-picolinic acid as hardness accelerators in the cyano-free gold plating process, the problem of insufficient hardness and uniformity of cyano-free gold plating is solved, and the stable hardness of the gold plating layer is achieved and Fine uniformity avoids the environmental and health hazards of traditional cyanide electroplating.

CN119040976APending Publication Date: 2024-11-29CHONGQING LIDAO SURFACE TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411233513.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing cyanide-free gold plating process has shortcomings in the hardness and uniformity of the gold plating layer, which limits its application, and the traditional cyanide electroplating process poses a threat to the environment and human health.

Method used

2-picolinic acid, 3-picolinic acid or 4-picolinic acid are used as hardness accelerators for cyanide-free electroplating gold. By adding these compounds to the electroplating solution to improve the hardness and uniformity of the gold-plating layer. The process parameters include current density 0.05 ~0.8A/dm2, temperature 45°C, pH 8.5 and the ratio of the anode to cathode area is greater than 2:1.

Benefits of technology

Within the current density range of 0.05-0.8A/dm2, the hardness of the coating is stable in the range of 130-150HV, and the crystallization is fine and uniform, which significantly improves the hardness and uniformity of cyanide-free gold plating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027017930000031
    Figure BDA0005027017930000031
  • Figure BDA0005027017930000041
    Figure BDA0005027017930000041
  • Figure BDA0005027017930000071
    Figure BDA0005027017930000071
Patent Text Reader

Abstract

The invention relates to a hardness accelerator for cyanide-free electrogilding, which relates to the technical field of electroplating, and is characterized in that the accelerator is composed of one or more of 2-picolinic acid, 3-picolinic acid and 4-picolinic acid. The mass concentration of the accelerant is 0.01 g / L to 1g / L. By using the cyanide-free electrogilding hardness accelerator, the hardness of a plating layer of cyanide-free electrogilding can be stabilized within the range of 130-150 HV within the current density range of 0.05-0.8 A / dm < 2 >, and meanwhile, the plating layer is fine and uniform in crystallization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electroplating, and more particularly to a hardness accelerator for cyanide-free gold electroplating. Background Art

[0002] Electroplating gold technology has a history of more than 100 years. Most electroplating gold uses alkaline cyanide, acidic (added organic weak acid, such as citric acid) and neutral (pH 6.5-7.5) micro-cyanide plating solution, while the main process used for electroplating hard gold is the citrate micro-cyanide gold plating process. Nowadays, micro-cyanide gold plating is generally used for processes that meet the hardness requirements of the gold-plated layer, but it is well known that CN is highly toxic and will cause great harm to electroplating workers and the environment.

[0003] The cyanide-free gold plating that replaces the cyanide gold plating process technology does not meet the requirements for the hardness of the gold plating layer, which limits the use of cyanide-free gold plating. Therefore, people hope to obtain an additive to improve the hardness of the gold plating layer of the cyanide-free gold plating. Summary of the invention

[0004] The purpose of the invention is to provide a hardness accelerator for cyanide-free gold electroplating, so as to solve the problems of low hardness and uneven hardness of the current cyanide-free gold electroplating.

[0005] The above technical objectives of the present invention are achieved through the following technical solutions:

[0006] A hardness accelerator for cyanide-free gold electroplating, the accelerator is composed of one or more of 2-pyridinecarboxylic acid, 3-pyridinecarboxylic acid and 4-pyridinecarboxylic acid.

[0007] Furthermore, the accelerator is in the range of 0.01 g / L to 1 g / L in terms of mass concentration.

[0008] The invention discloses an application of a cyanide-free gold electroplating hardness accelerator in preparing a cyanide-free gold electroplating solution.

[0009] The beneficial effect of the present invention is that it can make the cyanide-free gold plating at 0.05-0.8A / dm 2 Within the current density range, the coating hardness is stable in the range of 130 to 150 HV, and the coating crystallization is fine and uniform. DETAILED DESCRIPTION

[0010] The preferred embodiments of the present invention are described in detail below, which is helpful for a better understanding of the present invention and its advantages and effects, but the embodiments are only used to illustrate the present invention rather than to limit the present invention.

[0011] Testing methods for coating performance

[0012] 1. Appearance inspection: The appearance should be inspected visually under a natural scattered light source or white projection light without reflected light. The test piece should be placed under a 40W fluorescent lamp at a distance of 1.2 to 1.5 meters from the object, and the eyes should be observed at a distance of 35±5cm from the part. The overall appearance of the test piece should be uniform and consistent, and the coating crystals should be fine, uniform and continuous without blackening or roughness.

[0013] 2. Coating thickness detection: Use X-ray diffractometer to measure thickness.

[0014] 3. Hard plating detection: Use a digital microhardness tester to measure the hardness.

[0015] Example 1

[0016] The mass concentration ratio of each component of the cyanide-free gold plating hardness accelerator in this embodiment is as follows:

[0017] 2-Picolidinecarboxylic acid 0.05g / L

[0018] The concentration of the cyanide-free hard gold plating standard solution is as follows:

[0019] Potassium gold sulfite 18g / L

[0020] Potassium sulfite 120g / L

[0021] Cobalt sulfate 0.4g / L

[0022] Add the above-mentioned cyanide-free gold plating hardness accelerator to the cyanide-free hard gold plating standard solution. Process parameters: current density 0.05~0.8A / dm 2 , temperature 45℃, pH value 8.5, anode to cathode area ratio greater than 2:1, select 50×50×1mm copper test piece for plating, plating thickness of about 2μm, then check the appearance of the coating and test the hardness of the coating. After testing, at 0.05~0.8A / dm 2 When the current density is 1.547 W, the hardness of the coating is stable in the range of 130-150 HV, and the coating crystallization is fine and uniform. The test data results are shown in Table 1.

[0023] The cyanide-free hard gold plating standard solution (gold potassium sulfite 18g / L, potassium sulfite 120g / L, cobalt sulfate 0.4g / L) was used for electroplating experiments under the same process parameters: current density 0.05~0.8A / dm 2 , temperature 45℃, pH value 8.5, anode to cathode area ratio greater than 2:1, select 50×50×1mm copper test piece for plating, plating thickness of about 2μm; test the appearance of the coating and test the hardness of the coating. After testing, at 0.05~0.8A / dm 2 When the current density is high, the hardness of the coating fluctuates within the range of 80 to 150 HV, and the coating crystals are fine and uniform. The test data results are shown in Table 2.

[0024] Table 1 Experimental results of cyanide-free hard gold plating with hardness accelerator in Example 1

[0025] Current density Coating appearance Coating hardness 0.05 Fine crystals, uniform bright golden yellow 136 0.1 Fine crystals, uniform bright golden yellow 147 0.2 Fine crystals, uniform bright golden yellow 143 0.4 Fine crystals, uniform bright golden yellow 152 0.8 Fine crystals, uniform bright golden yellow 149

[0026] Table 2 Experimental results of cyanide-free hard gold plating standard solution

[0027]

[0028]

[0029] Example 2

[0030] The mass concentration ratio of each component of the cyanide-free gold plating hardness accelerator in this embodiment is as follows:

[0031] 3-Picolidinecarboxylic acid 0.05g / L

[0032] The concentration of the standard solution for cyanide-free hard gold plating is consistent with that in Example 1 (18 g / L potassium gold sulfite, 120 g / L potassium sulfite, and 0.4 g / L cobalt sulfate).

[0033] Add the above-mentioned cyanide-free gold plating hardness accelerator to the cyanide-free hard gold plating standard solution. Process parameters: current density 0.05~0.8A / dm 2 , temperature 45℃, pH value 8.5, anode to cathode area ratio greater than 2:1, select 50×50×1mm copper test piece for plating, plating thickness of about 2μm, then check the appearance of the coating and test the hardness of the coating. After testing, at 0.05~0.8A / dm 2 When the current density is high, the hardness of the coating is stable in the range of 130 to 150 HV, and the coating crystallization is fine and uniform. The test data results are shown in Table 3.

[0034] Table 3 Experimental results of cyanide-free hard gold plating with hardness accelerator in Example 2

[0035] Current density Coating appearance Coating hardness 0.05 Fine crystals, uniform bright golden yellow 134 0.1 Fine crystals, uniform bright golden yellow 138 0.2 Fine crystals, uniform bright golden yellow 145 0.4 Fine crystals, uniform bright golden yellow 147 0.8 Fine crystals, uniform bright golden yellow 154

[0036] Example 3

[0037] The mass concentration ratio of each component of the cyanide-free gold plating hardness accelerator in this embodiment is as follows:

[0038] 4-Picolidinecarboxylic acid 0.05g / L

[0039] The concentration of the standard solution for cyanide-free hard gold plating is consistent with that in Example 1 (18 g / L potassium gold sulfite, 120 g / L potassium sulfite, and 0.4 g / L cobalt sulfate).

[0040] Add the above-mentioned cyanide-free gold plating hardness accelerator to the cyanide-free hard gold plating standard solution. Process parameters: current density 0.05~0.8A / dm 2 , temperature 45℃, pH value 8.5, anode to cathode area ratio greater than 2:1, select 50×50×1mm copper test piece for plating, plating thickness of about 2μm, then check the appearance of the coating and test the hardness of the coating. After testing, at 0.05~0.8A / dm 2 When the current density is high, the hardness of the coating is stable in the range of 130 to 150 HV, and the coating crystallization is fine and uniform. The test data results are shown in Table 4.

[0041] Table 4 Experimental results of cyanide-free hard gold plating with hardness accelerator in Example 3

[0042] Current density Coating appearance Coating hardness 0.05 Fine crystals, uniform bright golden yellow 136 0.1 Fine crystals, uniform bright golden yellow 139 0.2 Fine crystals, uniform bright golden yellow 144 0.4 Fine crystals, uniform bright golden yellow 148 0.8 Fine crystals, uniform bright golden yellow 146

[0043] Example 4

[0044] The mass concentration ratio of each component of the cyanide-free gold plating hardness accelerator in this embodiment is as follows:

[0045] 2-Picolidinecarboxylic acid 0.05g / L

[0046] 3-Picolidinecarboxylic acid 0.1g / L

[0047] The above ingredients are mixed to obtain the cyanide-free gold plating hardness accelerator of this embodiment.

[0048] The concentration of the standard solution for cyanide-free hard gold plating is consistent with that in Example 1 (18 g / L potassium gold sulfite, 120 g / L potassium sulfite, and 0.4 g / L cobalt sulfate).

[0049] Add the above-mentioned cyanide-free gold plating hardness accelerator to the cyanide-free hard gold plating standard solution. Process parameters: current density 0.05~0.8A / dm 2 , temperature 45℃, pH value 8.5, anode to cathode area ratio greater than 2:1, select 50×50×1mm copper test piece for plating, plating thickness of about 2μm, then check the appearance of the coating and test the hardness of the coating. After testing, at 0.05~0.8A / dm 2 When the current density is high, the hardness of the coating is stable in the range of 130 to 150 HV, and the coating crystallization is fine and uniform. The test data results are shown in Table 5.

[0050] Table 5 Experimental results of cyanide-free hard gold plating plus hardness accelerator in Example 4

[0051] Current density Coating appearance Coating hardness 0.05 Fine crystals, uniform bright golden yellow 127 0.1 Fine crystals, uniform bright golden yellow 134 0.2 Fine crystals, uniform bright golden yellow 142 0.4 Fine crystals, uniform bright golden yellow 145 0.8 Fine crystals, uniform bright golden yellow 148

[0052] Example 5

[0053] The mass concentration ratio of each component of the cyanide-free gold plating hardness accelerator in this embodiment is as follows:

[0054] 2-Picolidinecarboxylic acid 0.05g / L

[0055] 4-Pyridinecarboxylic acid 0.1g / L

[0056] The above ingredients are mixed to obtain the cyanide-free gold plating hardness accelerator of this embodiment.

[0057] The concentration of the standard solution for cyanide-free hard gold plating is consistent with that in Example 1 (18 g / L potassium gold sulfite, 120 g / L potassium sulfite, and 0.4 g / L cobalt sulfate).

[0058] Add the above-mentioned cyanide-free gold plating hardness accelerator to the cyanide-free hard gold plating standard solution. Process parameters: current density 0.05~0.8A / dm 2 , temperature 45℃, pH value 8.5, anode to cathode area ratio greater than 2:1, select 50×50×1mm copper test piece for plating, plating thickness of about 2μm, then check the appearance of the coating and test the hardness of the coating. After testing, at 0.05~0.8A / dm 2 When the current density is high, the hardness of the coating is stable in the range of 130 to 150 HV, and the coating crystallization is fine and uniform. The test data results are shown in Table 5.

[0059] Table 5 Experimental results of cyanide-free hard gold plating plus hardness accelerator in Example 4

[0060] Current density Coating appearance Coating hardness 0.05 Fine crystals, uniform bright golden yellow 129 0.1 Fine crystals, uniform bright golden yellow 132 0.2 Fine crystals, uniform bright golden yellow 141 0.4 Fine crystals, uniform bright golden yellow 146 0.8 Fine crystals, uniform bright golden yellow 148

[0061] Example 6

[0062] The mass concentration ratio of each component of the cyanide-free gold plating hardness accelerator in this embodiment is as follows:

[0063] 3-Picolidinecarboxylic acid 0.05g / L

[0064] 4-Pyridinecarboxylic acid 0.1g / L

[0065] The above ingredients are mixed to obtain the cyanide-free gold plating hardness accelerator of this embodiment.

[0066] The concentration of the standard solution for cyanide-free hard gold plating is consistent with that in Example 1 (18 g / L potassium gold sulfite, 120 g / L potassium sulfite, and 0.4 g / L cobalt sulfate).

[0067] Add the above-mentioned cyanide-free gold plating hardness accelerator to the cyanide-free hard gold plating standard solution. Process parameters: current density 0.05~0.8A / dm 2, temperature 45℃, pH value 8.5, anode to cathode area ratio greater than 2:1, select 50×50×1mm copper test piece for plating, plating thickness of about 2μm, then check the appearance of the coating and test the hardness of the coating. After testing, at 0.05~0.8A / dm 2 When the current density is high, the hardness of the coating is stable in the range of 130 to 150 HV, and the coating crystallization is fine and uniform. The test data results are shown in Table 5.

[0068] Table 5 Experimental results of cyanide-free hard gold plating plus hardness accelerator in Example 4

[0069]

[0070]

[0071] Example 7

[0072] The mass concentration ratio of each component of the cyanide-free gold plating hardness accelerator in this embodiment is as follows:

[0073] 2-Picolidinecarboxylic acid 0.05g / L

[0074] 3-Picolidinecarboxylic acid 0.1g / L

[0075] 4-Pyridinecarboxylic acid 0.1g / L

[0076] The above ingredients are mixed to obtain the cyanide-free gold plating hardness accelerator of this embodiment.

[0077] The concentration of the standard solution for cyanide-free hard gold plating is consistent with that in Example 1 (18 g / L potassium gold sulfite, 120 g / L potassium sulfite, and 0.4 g / L cobalt sulfate).

[0078] Add the above-mentioned cyanide-free gold plating hardness accelerator to the cyanide-free hard gold plating standard solution. Process parameters: current density 0.05~0.8A / dm 2 , temperature 45℃, pH value 8.5, anode to cathode area ratio greater than 2:1, select 50×50×1mm copper test piece for plating, plating thickness of about 2μm, then check the appearance of the coating and test the hardness of the coating. After testing, at 0.05~0.8A / dm 2 When the current density is 2.5, the hardness of the coating is stable in the range of 130-150HV, and the coating crystallization is fine and uniform. The test data results are shown in Table 6.

[0079] Table 6 Experimental results of cyanide-free hard gold plating with hardness accelerator in Example 5

[0080]

[0081]

[0082] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A hardness accelerator for cyanide-free gold electroplating, characterized in that: The accelerator is composed of one or more of 2-pyridinecarboxylic acid, 3-pyridinecarboxylic acid and 4-pyridinecarboxylic acid.

2. A hardness accelerator for cyanide-free gold electroplating according to claim 1, characterized in that: Calculated by mass concentration, the accelerator is 0.01g / L to 1g / L.

3. Use of the hardness accelerator for cyanide-free gold electroplating according to any one of claims 1 to 2 in preparing a cyanide-free gold electroplating solution.