Heat-resistant four-stage protective glove and preparation method thereof

Through the specific heat-resistant functional slurry and sandwich structure, the existing high-temperature resistant gloves are solved, and efficient four-level protection and cost-effective heat-resistant gloves are achieved.

CN119041208APending Publication Date: 2024-11-29NANTONG QIANGSHENG SAFETY PROTECTION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411183241.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing high-temperature resistant gloves have high prices, easy breakage, skin irritation and health risks, and it is difficult to take into account high-temperature protection in terms of cost-effectiveness and comfort and breathability.

Method used

Using specific heat-resistant slurries, including heat-resistant materials, adhesives, softeners, penetrants, defoamers and crosslinkers, the yarn fibers are impregnated and textile into a glove outer layer, combining aluminum foil and embryo cloth As an intermediate interlayer, four-level protective gloves are formed.

Benefits of technology

It achieves an efficient heat-resistant contact level of level 4, and is cost-effective, adapts to a variety of high temperature scenarios, avoiding the health risks of traditional gloves.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a heat-resistant four-stage protective glove and a preparation method thereof. A heat-resistant functional slurry used in the preparation of the glove comprises the following raw material components in parts by weight: 35-60 parts of a heat-resistant material, 50-80 parts of an adhesive, 10-20 parts of a softening agent, 0.3-1 part of a penetrant, 5-10 parts of a defoaming agent, 8-15 parts of liquid wax, 1-5 parts of a cross-linking agent and 80-120 parts of water. The specific heat-resistant functional slurry is adopted, the yarn is soaked and then woven into the glove outer layer, the gray cloth and the aluminum foil are coated with the heat-resistant functional slurry to serve as the middle interlayer, the cotton cloth serves as the glove inner layer, the heat resistance of the manufactured protective glove is excellent, and the heat-resistant contact grade measured through the EN407: 2020 method can reach the fourth grade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of security products, and in particular to a heat-resistant fourth-level protective glove and a preparation method thereof. Background Art

[0002] At present, the main types of high temperature resistant gloves on the market are: carbon fiber high temperature resistant gloves, aramid high temperature resistant gloves, asbestos high temperature resistant gloves, glass fiber high temperature resistant gloves, etc. These gloves all have certain disadvantages. Carbon fiber is expensive and easy to break, aramid fiber is expensive and not resistant to light, asbestos fiber can cause diseases such as asbestosis and pleural mesothelioma, and glass fiber has strong irritation to the skin and eyes and is prone to allergies. Developing a glove that is both resistant to ultra-high temperatures, comfortable and breathable, cost-effective, and adaptable to a variety of high temperature scenarios is an important task in the current field of hand protection. Summary of the invention

[0003] In view of the deficiencies in the prior art, the object of the present invention is to provide a heat-resistant fourth-level protective glove and a preparation method thereof.

[0004] The objective of the present invention is achieved through the following technical solutions:

[0005] In the first aspect, the present invention provides a heat-resistant functional slurry, comprising the following raw material components in parts by weight: 35-60 parts of heat-resistant material, 50-80 parts of adhesive, 10-20 parts of softener, 0.3-1 part of penetrant, 5-10 parts of defoaming agent, 8-15 parts of liquid wax, 1-5 parts of cross-linking agent, and 80-120 parts of water.

[0006] As a preferred solution, the heat-resistant material is selected from at least one of fumed silica, polyarylate and polyimide.

[0007] As a further preferred embodiment, the heat-resistant material is a combination of fumed silica and polyarylate or polyimide; more preferably, the weight ratio of the fumed silica to polyarylate or polyimide is 1:1-1.2.

[0008] As a preferred embodiment, the adhesive is selected from at least one of EVA emulsion, polyamide emulsion and polyurethane.

[0009] As a preferred embodiment, the softener is a fatty acid salt.

[0010] As a preferred embodiment, the penetrant is fatty alcohol polyoxyethylene ether.

[0011] As a preferred embodiment, the defoaming agent is silicone oil.

[0012] As a preferred embodiment, the cross-linking agent is isocyanate.

[0013] In a second aspect, the present invention provides a method for preparing a heat-resistant functional slurry, comprising the following steps:

[0014] After the water and penetrant are stirred evenly, add the heat-resistant material and stir evenly, then add the adhesive, cross-linking agent, liquid wax, softener and defoaming agent in sequence, and stir by ball milling for 3-10 hours to obtain.

[0015] In a third aspect, the present invention provides a method for preparing heat-resistant level 4 protective gloves, comprising the following steps:

[0016] A1. Dipping the yarn fiber into the heat-resistant functional slurry according to any one of claims 1 to 6, and after dipping, passing through a pressing roller, drying, and then winding into aramid-like fiber, and then weaving the aramid-like fiber into the outer layer of the glove;

[0017] A2, coating the grey cloth and the aluminum foil with the heat-resistant functional slurry according to any one of claims 1 to 6, and drying;

[0018] A3. Use cotton cloth as the inner layer of the gloves, and sequentially bond the grey cloth coated with heat-resistant functional slurry and aluminum foil to the outside of the inner layer of the gloves to form an intermediate layer. Then place the outer layer of the gloves on the outside of the intermediate layer to form a heat-resistant level 4 protective glove.

[0019] As a preferred embodiment, in step A1, the yarn fiber is selected from any one of cotton yarn, polyester, nylon, acrylic fiber, viscose fiber or any blended yarn of several thereof.

[0020] As a preferred embodiment, in step A2, the grey cloth is any one of pure cotton grey cloth, polyester grey cloth, nylon grey cloth, acrylic grey cloth, and viscose fiber grey cloth.

[0021] In a fourth aspect, the present invention provides a heat-resistant level 4 protective glove prepared according to the aforementioned method.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention adopts a specific heat-resistant functional slurry, immerses the yarn in it and then weaves it into the outer layer of the gloves, and then coats the grey cloth and aluminum foil with the heat-resistant functional slurry as the middle layer, and uses cotton cloth as the inner layer of the gloves. The protective gloves thus prepared have excellent heat resistance, and the heat-resistant contact grade measured by the EN407:2020 method can reach level four. DETAILED DESCRIPTION

[0024] Unless otherwise defined, technical terms or scientific terms used in this specification and claims shall have the ordinary meanings understood by persons with ordinary skills in the technical field to which this application belongs. All values ​​from the lowest value to the highest value listed herein refer to all values ​​obtained by incrementing the lowest value to the highest value by one unit when the difference between the lowest value and the highest value is more than two units.

[0025] The specific implementation methods of the present application will be described below. It should be noted that in the specific description of these implementation methods, in order to provide a concise description, it is impossible for this specification to provide a detailed description of all the features of the actual implementation methods. Without departing from the spirit and scope of the present application, those skilled in the art may modify and replace the implementation methods of the present application, and the resulting implementation methods are also within the scope of protection of the present application.

[0026] In a specific embodiment of the present invention, a method for preparing heat-resistant level 4 protective gloves is provided, comprising the following steps:

[0027] 1) Preparation of heat-resistant functional slurry: weigh each component by weight, stir 80-120 parts of water and 0.3-1 parts of penetrant for 4-6 minutes, add 35-60 parts of heat-resistant material, stir for 1.5-2.5 hours, then add 50-80 parts of adhesive, 1-5 parts of cross-linking agent, 8-15 parts of liquid wax, 10-20 parts of softener, 5-10 parts of defoamer in sequence, and stir by ball milling at a speed of 5-10 rpm for 3-10 hours to obtain heat-resistant functional slurry;

[0028] 2) Dipping the polyester into the heat-resistant functional slurry prepared in step 1) for 1-5 minutes, passing the dipped polyester through a pressing roller, drying, winding, and weaving it into an outer layer of the glove using a knitting machine;

[0029] 3) coating the grey cloth and the aluminum foil with the heat-resistant functional slurry prepared in step 1) respectively, to obtain the cotton grey cloth and the aluminum foil coated with the heat-resistant functional slurry;

[0030] 4) After the cotton yarn is knitted into the inner layer of the gloves, the aluminum foil coated with heat-resistant functional slurry and the grey cloth coated with heat-resistant functional slurry are sequentially bonded to the outer side of the inner layer of the gloves; and then the inner layer of the gloves is sewn together to form a heat-resistant protective glove which comprises, from inside to outside, the inner layer of the gloves, the middle layer of the aluminum foil coated with functional slurry and the grey cloth, and the outer layer of the gloves.

[0031] In a specific embodiment, in step 1), the heat-resistant material is selected from at least one of fumed silica, polyarylate, and polyimide; the adhesive is selected from at least one of EVA emulsion, polyamide emulsion, and polyurethane; the softener is a fatty acid salt; the penetrant is a fatty alcohol polyoxyethylene ether; the defoamer is silicone oil; and the cross-linking agent is isocyanate.

[0032] In a specific embodiment, in step 2), the yarn fiber is selected from any one of cotton yarn, polyester, nylon, acrylic fiber, viscose fiber or any blended yarn of several thereof. The present invention does not make any special limitation.

[0033] In a specific embodiment, in step 2), the method of weaving the outer layer of the glove using a knitting machine is a conventional weaving method, and the present invention does not make any particular limitation.

[0034] In a specific embodiment, in step 3), the grey cloth is any one of pure cotton grey cloth, polyester grey cloth, nylon grey cloth, acrylic grey cloth, and viscose grey cloth. The present invention does not make any special limitation.

[0035] Example

[0036] The embodiments of the present application will be described in detail below. This embodiment is implemented on the premise of the technical solution of the present application, and a detailed implementation method and a specific operation process are given, but the protection scope of the present application is not limited to the following embodiments.

[0037] In the following examples, the polyester used was purchased from Zhejiang Huilong New Materials Co., Ltd., model 120DFDY, specification 120D 36F; the cotton grey cloth used was purchased from Huayi Textile Co., Ltd., specification 21 (gram weight 180g / m 2 ), width 1.5 meters; the aluminum foil used was purchased from Suzhou Field Special Textile Co., Ltd.; the cotton yarn used was purchased from Weifang Huafeng Textile Co., Ltd., model HF16, specification 21; the polyarylate used was purchased from Dongguan Linghan Times New Materials Co., Ltd., model AX-1500W; the polyimide used was purchased from Shanghai Fengguang Plastic Technology Co., Ltd., model PI emulsion; the fumed silica used was purchased from Dongguan Yisheng Chemical Co., Ltd., with a particle size of 1-5μm; the polyamide emulsion used was purchased from Jiangsu Jufeng Chemical Technology Co., Ltd., model YF-219; the polyurethane used was purchased from Jiangsu Jufeng Chemical Technology Co., Ltd. The ester was purchased from Anhui Femtosecond Chemical Co., Ltd., model FS-Y30; the EVA emulsion used was purchased from Shanghai Su'ao Chemical Co., Ltd., model 1901; the isocyanate used was purchased from Shanghai Ruidong Chemical Group Co., Ltd., model 2342342; the liquid wax used was purchased from Shanghai Aibi Chemical Reagent Co., Ltd., model 8012-95-1; the sodium fatty acid used was purchased from Guangzhou Hehui Chemical Co., Ltd.; the silicone oil used was purchased from Shandong Luderui New Materials Co., Ltd.; the penetrant used was fatty alcohol polyoxyethylene ether, purchased from Shandong Lusen Co., Ltd., model JFC-3.

[0038] The equipment used in the specific embodiments of the present invention are all conventional equipment for producing and preparing gloves, and the raw materials used are also prepared or purchased by conventional methods, and the present invention does not make any special limitations.

[0039] Example 1

[0040] This embodiment provides a method for preparing heat-resistant protective gloves, comprising the following steps:

[0041] 1) Preparation of heat-resistant functional slurry: Weigh each component by weight, as shown in Table 1; stir 100 parts of water and 1 part of JFC-3 (penetrant) for 5 minutes, then add 30 parts of polyarylate and 23 parts of fumed silica in sequence, stir for 2 hours, then add 70 parts of polyamide emulsion, 4 parts of isocyanate (cross-linking agent), 9 parts of liquid wax, 15 parts of sodium fatty acid (softener), 8.5 parts of silicone oil (defoaming agent) in sequence, and stir by ball milling at a speed of 5 rpm for 5 hours to obtain heat-resistant functional slurry;

[0042] 2) dipping the polyester into the heat-resistant functional slurry prepared in step 1) for 3 minutes, passing the dipped polyester through a pressing roller and drying at 150° C. for 3 minutes, winding the polyester, and knitting the outer layer of the gloves using a knitting machine;

[0043] 3) Put the cotton grey cloth (weight 180g / m 2 ) and aluminum foil are respectively coated with the functional slurry prepared in step 1) to obtain cotton grey cloth and aluminum foil coated with the functional slurry;

[0044] 4) After the cotton yarn is knitted into the inner layer of the gloves, the aluminum foil coated with the functional slurry and the pure cotton grey cloth coated with the functional slurry are sequentially bonded to the outer side of the inner layer of the gloves; and then the inner layer of the gloves is sewn together with the outer layer of the gloves to form a heat-resistant protective glove which comprises, from the inside to the outside, the inner layer of the gloves, the middle layer of the aluminum foil coated with the functional slurry and the pure cotton grey cloth composite, and the outer layer of the gloves.

[0045] Example 2

[0046] The present embodiment provides a method for preparing heat-resistant protective gloves, which is basically the same as the preparation method of Example 1, except that: in the present embodiment, the weight parts of the components used in step 1) are as shown in Table 2; 120 parts of water and 0.3 parts of JFC-3 (penetrant) are stirred for 3 minutes, and then 20 parts of polyimide and 15 parts of fumed silica are added in sequence, and after stirring for 1 hour, 80 parts of polyurethane, 5 parts of isocyanate (cross-linking agent), 15 parts of liquid wax, 10 parts of sodium fatty acid (softener), and 5 parts of silicone oil (defoaming agent) are added in sequence, and the mixture is ball-milled and stirred at a speed of 5 rpm for 3 hours to obtain a heat-resistant functional slurry.

[0047] Example 3

[0048] The present embodiment provides a method for preparing heat-resistant protective gloves, which is basically the same as the preparation method of Example 1, except that: in the present embodiment, the weight proportions of the components used in step 1) are as shown in Table 2; 80 parts of water and 0.8 parts of JFC-3 (penetrant) are stirred for 5 minutes, and then 30 parts of polyimide and 30 parts of fumed silica are added in sequence, and after stirring for 3 hours, 50 parts of EVA emulsion, 1 part of isocyanate (cross-linking agent), 8 parts of liquid wax, 20 parts of sodium fatty acid (softener), and 10 parts of silicone oil (defoaming agent) are added in sequence, and the mixture is ball-milled and stirred at a speed of 5 rpm for 10 hours to obtain a heat-resistant functional slurry.

[0049] Example 4

[0050] This embodiment provides a method for preparing heat-resistant protective gloves, which is basically the same as the preparation method of Example 3, except that: in this embodiment, step 1) uses 0 parts of polyimide and 60 parts of fumed silica.

[0051] Example 5

[0052] This embodiment provides a method for preparing heat-resistant protective gloves, which is basically the same as the preparation method of Example 3, except that: in this embodiment, step 1) uses 60 parts of polyimide and 0 parts of fumed silica.

[0053] Example 6

[0054] This embodiment provides a method for preparing heat-resistant protective gloves, which is basically the same as the preparation method of Example 3, except that: in this embodiment, step 1) uses 20 parts of polyimide and 40 parts of fumed silica.

[0055] Example 7

[0056] This embodiment provides a method for preparing heat-resistant protective gloves, which is basically the same as the preparation method of Example 3, except that: in this embodiment, step 1) uses 45 parts of polyimide and 15 parts of fumed silica.

[0057] Example 8

[0058] This embodiment provides a method for preparing heat-resistant protective gloves, which is basically the same as the preparation method of Example 3, except that: in this embodiment, step 3) is: preparing a pure cotton grey cloth (weight 180g / m 2 ) coating the functional slurry prepared in step 1) to obtain a pure cotton grey cloth coated with the functional slurry; in step 4), the step of applying the aluminum foil is correspondingly omitted, so that the middle interlayer is only the pure cotton grey cloth coated with the functional slurry.

[0059] Example 9

[0060] This embodiment provides a method for preparing heat-resistant protective gloves, which is basically the same as the preparation method of Example 3, except that: in this embodiment, step 3) is: preparing a pure cotton grey cloth (weight 180g / m 2 ) coating the functional slurry prepared in step 1) to obtain a pure cotton grey cloth coated with the functional slurry; step 4) is: after knitting the cotton yarn into the inner layer of the gloves, bonding aluminum foil and the pure cotton grey cloth coated with the functional slurry on the outer side of the inner layer of the gloves in sequence; and then sewing it with the outer layer of the gloves to form a heat-resistant protective glove which is composed of the inner layer of the gloves, the aluminum foil and the pure cotton grey cloth coated with the functional slurry, and the outer layer of the gloves in sequence from the inside to the outside.

[0061] Performance Testing

[0062] The heat-resistant protective gloves prepared in each embodiment and comparative example were subjected to a heat resistance test, specifically, the heat-resistant contact performance test was conducted using the EN407:2020 method. The test results are shown in Table 1 below.

[0063] Table 1

[0064] Heat resistance contact grade Example 1 4 Example 2 4 Example 3 4 Example 4 3 Example 5 2 Example 6 2 Example 7 3 Example 8 1 Example 9 2

[0065] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A heat-resistant functional slurry, characterized in that: The invention comprises the following raw material components in parts by weight: 35-60 parts of heat-resistant material, 50-80 parts of adhesive, 10-20 parts of softener, 0.3-1 parts of penetrant, 5-10 parts of defoamer, 8-15 parts of liquid wax, 1-5 parts of cross-linking agent and 80-120 parts of water.

2. The heat-resistant functional slurry according to claim 1, characterized in that: The heat-resistant material is selected from at least one of fumed silica, polyarylate and polyimide.

3. The heat-resistant functional slurry according to claim 1, characterized in that: The adhesive is selected from at least one of EVA emulsion, polyamide emulsion and polyurethane.

4. The heat-resistant functional slurry according to claim 1, characterized in that: The softener is a fatty acid salt; The penetrant is fatty alcohol polyoxyethylene ether.

5. The heat-resistant functional slurry according to claim 1, characterized in that: The defoamer is silicone oil; The cross-linking agent is isocyanate.

6. A method for preparing the heat-resistant functional slurry according to any one of claims 1 to 5, characterized in that: The following steps are involved: After the water and penetrant are stirred evenly, add the heat-resistant material and stir evenly, then add the adhesive, cross-linking agent, liquid wax, softener and defoaming agent in sequence, and stir by ball milling for 3-10 hours to obtain.

7. A method for preparing heat-resistant level 4 protective gloves, characterized in that: The following steps are involved: A1. Dipping the yarn fiber into the heat-resistant functional slurry according to any one of claims 1 to 6, and after dipping, passing through a pressing roller, drying, and then winding into aramid-like fiber, and then weaving the aramid-like fiber into the outer layer of the glove; A2, coating the grey cloth and the aluminum foil with the heat-resistant functional slurry according to any one of claims 1 to 6, and drying; A3. Use cotton cloth as the inner layer of the gloves, and sequentially bond the grey cloth coated with heat-resistant functional slurry and aluminum foil to the outside of the inner layer of the gloves to form an intermediate layer. Then place the outer layer of the gloves on the outside of the intermediate layer to form a heat-resistant level 4 protective glove.

8. The method for preparing heat-resistant level 4 protective gloves according to claim 7, characterized in that: In step A1, the yarn fiber is selected from any one of cotton yarn, polyester, nylon, acrylic fiber, viscose fiber or any blended yarn of several thereof.

9. The method for preparing heat-resistant level 4 protective gloves according to claim 7, characterized in that: In step A2, the grey cloth is any one of pure cotton grey cloth, polyester grey cloth, nylon grey cloth, acrylic grey cloth, and viscose fiber grey cloth.

10. A heat-resistant level 4 protective glove prepared according to the method according to any one of claims 7 to 9.