Air inlet channel with multilayer structure suitable for high-performance engine of aerospace vehicle and preparation method of air inlet channel
By using a multi-layer structural design of carbon fiber reinforced silicon carbide ceramic composite material, silicon oxygen/phenolic resin insulation layer and high-temperature alloy shell in the air inlet of the aerospace aircraft engine, the problem of material density and connection thermal mismatch is solved. It achieves efficient temperature bearing and sealing, and improves the reliability and working efficiency of the engine.
Patent Information
- Application Number
- CN202411329068.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-29
AI Technical Summary
The air intake material of aerospace aircraft engine is difficult to meet the comprehensive performance requirements of high temperature, ablation resistance, low density and high reliability, and the structural porosity of carbon fiber reinforced silicon carbide composite materials and thermal mismatch problems of metal parts connections lead to sealing properties. Loss affects engine working efficiency.
Multi-layer structural design using carbon fiber reinforced silicon carbide ceramic matrix composite runner, silicon oxygen/phenolic resin insulation layer and high-temperature alloy shell layer, densified molding through pioneer impregnation and cracking and chemical vapor deposition processes, combined with low pressure isotherm Chemical vapor deposition technology uses pore sealing and component surface coating deposition to form a three-stage sealing layer structure.
It significantly reduces the overall weight of the intake duct, and at the same time improves the temperature bearing capacity of its working section, solves the connection and sealing problems of CMC and metal components, ensures the sealing and reliability under high-temperature and high-speed airflow, and avoids the phenomenon of fire.
Smart Images

Figure HDA0005056281030000011 
Figure HDA0005056281030000012 
Figure HDA0005056281030000013
Abstract
Description
Technical Field
[0001] The present application relates to the field of aviation engine technology, and in particular to an air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle and a preparation method thereof. Background Art
[0002] Aerospace vehicles are one of the key weapons for rapid response and seizing air and space supremacy in the future. Aerospace vehicles have the characteristics of hypersonic speed and wide airspace flight, which puts forward stringent performance requirements on the power system and its hot end components. The air-breathing combined cycle engine is the key technology for aerospace vehicles to solve the problem of free flight across the atmosphere, and the air intake duct as the engine air intake device is the key core technology of the engine. Taking into account the requirements of the aircraft and power system for the air intake duct, it needs to meet the requirements of light weight, high compression efficiency, small internal and external resistance, and large air flow.
[0003] In view of the use requirements of the engine air intake, the molded structural materials need to be lightweight, high-strength, and have excellent comprehensive properties such as ultra-high temperature resistance (>1600K), high ablation resistance, high reliability and reusability. However, refractory alloys such as tungsten copper and molybdenum copper have high density and low strength. Even with active cooling, it is difficult to break through the temperature resistance limit of the material itself. Ceramic matrix composites (CMC) have become strategic thermal structural materials that are the focus of research in various countries due to their many advantages such as high temperature resistance, oxidation resistance, wear resistance, low density, corrosion resistance, and crack insensitivity. Carbon fiber reinforced silicon carbide composites inherit the excellent properties of carbon fiber reinforced carbon-based composites such as high specific strength, high specific touch, high thermal conductivity and low thermal expansion coefficient. Its use in thermal structural materials for aviation aircraft can maximize the reliability of the aircraft while significantly reducing the weight of the entire aircraft. However, the inherent structural porosity of CMC materials makes it difficult to meet the air tightness requirements of the inlet duct. Under the action of high-pressure heat flow, the CMC inlet duct is prone to crossfire. At the same time, there is a serious thermal mismatch problem when the CMC section is directly connected to the front and rear metal parts through high-temperature alloy bolts. The thermal expansion of the bolts is more obvious than that of the composite material. The difference in elongation in the length direction causes the bolt preload to decrease, which ultimately leads to loss of sealing, forming a weak area under the scouring of high-speed airflow and quickly causing engine failure. Summary of the invention
[0004] The purpose of the present invention is to solve the above-mentioned deficiencies of the prior art, thereby providing an air intake duct with a multi-layer structure suitable for aerospace vehicle high-performance engines and a preparation method thereof, which can effectively reduce the overall weight of the air intake duct while greatly improving the temperature bearing capacity of its working section. At the same time, it solves the connection and sealing problems between the CMC working section and the metal parts.
[0005] An air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle, comprising a carbon fiber reinforced silicon carbide ceramic-based composite flow channel lining, a high-silicon oxide / phenolic resin thermal insulation layer and a high-temperature alloy shell layer, wherein the inner side of the high-silicon oxide / phenolic resin thermal insulation layer cooperates with the outer side of the carbon fiber reinforced silicon carbide ceramic-based composite flow channel lining, and the outer side of the high-silicon oxide / phenolic resin thermal insulation layer cooperates with the inner side of the high-temperature alloy shell layer.
[0006] The following steps are used:
[0007] S1: preparing a carbon fiber preform that is shaped like an engine intake duct;
[0008] S2: Densifying the contoured carbon fiber preform into a carbon fiber reinforced silicon carbide ceramic matrix composite material flow channel lining through precursor impregnation pyrolysis and chemical vapor deposition process;
[0009] S3: high silica fiber plain cloth prepreg is prepared on the outer surface of the carbon fiber reinforced silicon carbide ceramic matrix composite flow channel lining by continuous winding and molding curing process to obtain a high silica / phenolic resin insulation layer;
[0010] S4: A high-temperature alloy shell layer is prepared outside the high-silica / phenolic resin insulation layer using a high-temperature alloy steel sand casting molding process.
[0011] Step S2 is specifically as follows:
[0012] S21: Fiber interface coating treatment
[0013] The contoured carbon fiber preform made of 2.5D-T700 carbon fiber is placed in a high temperature resistant vacuum sintering furnace for isothermal chemical vapor deposition process to obtain a preform with a pyrolytic carbon interface layer;
[0014] S22: Precursor impregnation pyrolysis process matrix densification
[0015] The preform obtained in step S21 is densified by using a precursor impregnation cracking process, and a silicon carbide matrix is introduced to obtain C f / SiC components;
[0016] S23: Machining
[0017] The C obtained in step S22 is processed by a numerically controlled machine tool. f / Cut and grind the outer surface and end face of SiC components, and mill the inner surface of the flow channel to obtain the flow channel lining shape and surface roughness required by the design;
[0018] S24: Sealing and component surface coating deposition
[0019] The C machined in step S23 is deposited by low pressure isothermal chemical vapor deposition process. fCVI-SiC coating is introduced on the surface of / SiC components to fill the pores on the surface of the components.
[0020] Step S21 is specifically as follows:
[0021] A carbon fiber preform with a fiber volume fraction of 30% to 40% is placed in a high-temperature vacuum sintering furnace and kept at 900°C for two hours in a nitrogen atmosphere. Subsequently, deposition is performed using natural gas as the carbon source gas and nitrogen as the dilution and protective gas. The deposition temperature is 1050 to 1120°C, the deposition time is 10 to 15 hours, and the deposition pressure is 3000 to 6000Pa. The natural gas flow rate is 0.5 to 1.1 L / min, and the nitrogen flow rate is 2 to 4 L / min. After the deposition is completed, the pyrolytic carbon interface thickness should be ensured to be 500 to 1200 nm.
[0022] Step S22 is specifically as follows:
[0023] The preform processed in step S21 is fixed with a graphite mold, and a compressive force is applied in the thickness direction of the preform to obtain a preform with a high fiber volume fraction of 55% to 70%;
[0024] The preform is immersed in a 35% to 50% polycarbosilane / xylene solution under vacuum conditions and maintained under pressure for 3 hours, then cured at 270°C for 2 hours, and then pyrolyzed at 1100°C for 3 hours;
[0025] The above impregnation-curing-cracking process is repeated 3 to 4 times until the density of the preform reaches a predetermined value, and then the graphite mold is removed. The above impregnation-curing-cracking process is continued to be repeated until the preform weight gain rate is less than 1% to complete the high fiber volume fraction matrix densification process.
[0026] In step S22, the graphite mold is fastened by high-temperature alloy bolts, graphite bolts or C / C bolts, and compression force is applied using metal pressure rods, pressure strips or strapping tapes; the curing and high-temperature cracking process is carried out in a high-purity nitrogen atmosphere.
[0027] Step S24 is specifically as follows:
[0028] After the machining in step S23, f / SiC components are placed in a high-temperature furnace, trichloromethylsilane is used as silicon and carbon source gas, hydrogen is used as carrier gas and dilution gas, argon is used as protective gas, and low-pressure isothermal chemical vapor deposition is performed, the deposition temperature is 1000-1100°C, the deposition time is 30-60 hours, and the deposition pressure is 1000-1500Pa;
[0029] The flow ratio of the reaction gases is 1:30:30 for trichloromethylsilane:hydrogen:argon;
[0030] The final C f / SiC component density should be >2.0g / cm3 .
[0031] In step S3, the winding angle of the high-silica fiber plain cloth prepreg is 10-20°, and the molding temperature is 190° C.; the thickness of the high-silica / phenolic resin insulation layer is 3-5 mm.
[0032] The high-temperature alloy shell layer is made of cast alloy steel of one of GH4169, GH2132, DD406 and GH625; the mating surfaces of the high-temperature alloy shell layer and the high-silicon / phenolic resin insulation layer are set at an assembly angle of 1 to 3 degrees.
[0033] The excellent effects of this application are:
[0034] (1) A three-layer rotating body structure is adopted, which includes an inner layer of carbon fiber reinforced silicon carbide ceramic matrix composite material (CMC), a middle high-silicon oxide thermal insulation buffer layer, and an outer high-temperature alloy shell. The CMC directly serves as a gas flow channel to withstand the erosion of high-temperature gas; the high-silicon oxide layer plays the role of secondary sealing, thermal insulation, and alleviation of thermal mismatch of heterogeneous materials; the outer high-temperature alloy is connected to the front and rear metal components, avoiding the problem of heterogeneous connection between CMC and metal. At the same time, the metal shell also plays a sealing role.
[0035] (2) Carbon fiber reinforced silicon carbide ceramic matrix composite materials are used to replace high-temperature alloy inlet linings. Their density is only 1 / 3 to 1 / 4 of that of refractory metals, while their bending strength can reach over 500 MPa, reducing the overall weight of the inlet while maintaining high strength and stability of the component. Even without active cooling, their temperature resistance reaches over 1650K. If cooling media and flow channels are added, their operating temperature can be increased to over 1850K.
[0036] (3) A layer-by-layer sealing design is adopted. The fiber volume fraction of the preform is increased by the tooling force curing-cracking method in the early stage of the inner CMC. The CVI-SiC coating is applied on the surface of the CMC component by combining low-pressure isothermal chemical vapor deposition, which reduces the component porosity and defect size and number, and improves the overall strength and density of the component; the heat-insulating high-silicon oxide layer is a high-density high-silicon oxide / phenolic composite material. Its tightly wound structure can not only directly serve as a high-temperature sealing layer, but also alleviate the thermal mismatch between the high-temperature alloy shell and the CMC component, prevent interlayer cracking under high-temperature airflow scouring and high-pressure gas directly acting on the alloy shell layer; the alloy shell layer provides the last level of sealing, and flanges and graphite packings are used to seal the integral alloy shell and the front and rear metals and the split alloy shell. The three-level sealing layer structure realizes axial high-reliability sealing, effectively preventing the inlet duct from cross-fire under high-temperature and high-speed airflow scouring. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1The present invention is a lightweight and efficient multi-layer structure suitable for the air intake of a high-performance engine of an aerospace vehicle;
[0038] Figure 2 For example 1 of the present invention, in C f / Schematic diagram of the structure of preparing a high silicon oxygen thermal insulation layer on the outer surface of the SiC flow channel lining;
[0039] Figure 3 A three-dimensional model diagram of a three-layer square straight-flow air inlet prepared in Example 1 of the present invention;
[0040] Figure 4 C prepared in Example 2 of the present invention f SEM image and EDS spectrum of the inner wall of the SiC flow channel lining after high temperature ablation test, where a) is C f / Scanning electron images of SiC inner wall, b), c), d) are C, O, Si signals respectively;
[0041] Figure 5 C of Example 2 of the present invention and Comparative Example 1 f SEM images of C / SiC composite materials, where a) is the C of implementation case 2 f Microscopic image of C / SiC composite material, b) is C of comparative example 1 f / SiC composite micrograph;
[0042] Figure 6 C prepared in Example 3 of the present invention f / Stereoscopic image of SiC composite lining;
[0043] Figure 7 C prepared in Example 3 of the present invention f / SiC composite material lined plane Figure 1 ;
[0044] Figure 8 C prepared in Example 3 of the present invention f / SiC composite material lined plane Figure 2 ;
[0045] Fig. 9 for Figure 6 AA view;
[0046] Fig.10 for Figure 6 BB direction view. DETAILED DESCRIPTION
[0047] The present invention is further described in the following specific preferred embodiments, but the protection scope of the present invention is not limited thereby.
[0048] like Figure 1In the first aspect, a high-performance engine air intake with a lightweight, high-efficiency and multi-layer structure is provided, comprising a carbon fiber reinforced silicon carbide ceramic matrix composite flow channel liner 1, a high-silicon oxygen / phenolic resin thermal insulation layer 2 and a high-temperature alloy shell layer 3, wherein the above components are axisymmetric bodies of revolution or other air intake structure components. The inner side of the high-silicon oxygen / phenolic resin thermal insulation layer 2 is matched with the outer side of the carbon fiber reinforced silicon carbide ceramic matrix composite flow channel liner 1, and the outer side of the high-silicon oxygen thermal insulation layer 2 is matched with the high-temperature alloy shell layer 3.
[0049] The preparation method of the air intake duct is carried out by the following steps:
[0050] S1: preparing a carbon fiber preform that is shaped like an engine intake duct;
[0051] S2: Densifying the contoured carbon fiber preform into a carbon fiber reinforced silicon carbide ceramic matrix composite material flow channel lining through precursor impregnation pyrolysis and chemical vapor deposition process;
[0052] S3: high silica fiber plain cloth prepreg is prepared on the outer surface of the carbon fiber reinforced silicon carbide ceramic matrix composite flow channel lining by continuous winding and molding curing process to obtain a high silica / phenolic resin insulation layer;
[0053] S4: A high-temperature alloy shell layer is prepared outside the high-silica / phenolic resin insulation layer using a high-temperature alloy steel sand casting molding process.
[0054] The contoured carbon fiber preform is made of 2.5D-T700 carbon fiber.
[0055] The specific molding steps of the carbon fiber reinforced silicon carbide ceramic matrix composite flow channel lining are as follows:
[0056] (1) Fiber interface coating treatment
[0057] Placing the contoured carbon fiber preform in a high temperature resistant vacuum sintering furnace for isothermal chemical vapor infiltration to obtain a preform with a pyrolytic carbon interface layer;
[0058] (2) Precursor impregnation and cracking process matrix densification
[0059] The preform obtained in step (1) is densified by using a precursor impregnation cracking process, and a silicon carbide matrix is introduced to obtain C f / SiC composite materials;
[0060] (3) Machining
[0061] The outer surface and end face of the component obtained in step (2) are cut and polished by a CNC machine tool to facilitate the subsequent prepreg winding process and assembly, and the inner surface of the flow channel is milled to obtain the flow channel shape and surface roughness required by the design.
[0062] (4) Sealing and component surface coating deposition
[0063] The C machined in step (3) is deposited by low pressure isothermal chemical vapor deposition process. f CVI-SiC coating is introduced on the surface of / SiC components to fill the pores on the surface of the components.
[0064] Step (1) is specifically as follows: placing a carbon fiber preform with a fiber volume fraction of 30% to 40% in a high-temperature vacuum sintering furnace, keeping it at 900°C for two hours in a nitrogen atmosphere, and then depositing it using natural gas as the carbon source gas and nitrogen as the dilution and protective gas. The deposition temperature is 1050 to 1120°C, the deposition time is 10 to 15 hours, and the deposition pressure is 3000 to 6000Pa; the natural gas flow rate is 0.5 to 1.1 L / min, and the nitrogen flow rate is 2 to 4 L / min. After the deposition is completed, the pyrolysis interface thickness should be ensured to be 500 to 1200 nm.
[0065] Step (2) is specifically as follows: fix the preform processed in step (1) with a graphite mold, apply compression force in the thickness direction of the preform to obtain a preform with a high fiber volume fraction of 55% to 70%, impregnate the preform with a 35% to 50% polycarbosilane / xylene solution under vacuum conditions and maintain the pressure for 3 hours, then cure at 270°C and pyrolyze at 1100°C for 3 hours. After completing 3 to 4 impregnation-curing-pyrolysis processes until the component density reaches a predetermined value, remove the tooling and continue to repeat the impregnation-curing-pyrolysis process until the component weight gain rate is less than 1%, completing the high fiber volume fraction matrix densification process.
[0066] In step (2), the graphite mold is fastened by high-temperature alloy bolts, graphite bolts or C / C bolts, and compression force is applied using metal pressure rods, pressure strips or strapping tapes; the curing and high-temperature cracking process is carried out in a high-purity nitrogen atmosphere.
[0067] Step (4) is specifically as follows: placing the component machined in step (3) in a high temperature furnace, using trichloromethylsilane as silicon and carbon source gas, hydrogen as carrier gas and dilution gas, and argon as protective gas, to perform low-pressure isothermal chemical vapor deposition, the deposition temperature is 1000-1100° C., the deposition time is 30-60 hours, and the deposition pressure is 1000-1500 Pa;
[0068] The flow ratio of the reaction gases is 1:30:30 for trichloromethylsilane:hydrogen:argon;
[0069] The final C f / SiC component density should be >2.0g / cm 3 .
[0070] The winding angle of the high-silica fiber plain cloth prepreg is 10-20 degrees, and the molding temperature is 190 degrees Celsius; the thickness of the high-silica / phenolic resin insulation layer is 3-5 mm.
[0071] The casting alloy steel grade used for the high-temperature alloy shell layer is one of GH4169, GH2132, DD406, and GH625; the high-temperature alloy shell and the high-silicon oxygen matching surface are set with an assembly angle of 1 to 3 degrees.
[0072] Example 1
[0073] Three-layer square straight air intake, using C f / SiC lining, high silicon oxygen thermal insulation layer and GH625 nickel-based high temperature alloy shell.
[0074] The T-700 continuous carbon fiber 2.5D is used to make a preform that imitates the engine intake duct. The volume fraction of carbon fiber in the preform is 30%, and the initial density of the preform is 0.45g / cm 3 The preform has a 650*230*65mm square tubular structure. Before use, the preform is heated at 900°C for two hours in a nitrogen atmosphere for degumming treatment.
[0075] The fiber preform was placed in a high-temperature resistant vacuum sintering furnace, and the furnace temperature was raised to 1050°C under continuous vacuum conditions. Natural gas and nitrogen were then introduced with gas flow rates of 0.5L / min and 2L / min, respectively. The deposition lasted for 13 hours and the pressure in the furnace was maintained at 4500Pa. The thickness of the pyrolytic carbon interface on the prepared fiber surface was 600nm.
[0076] Then, the preform was loaded into the graphite core mold and four-sided graphite plates, fixed with C / C bolts, and tied with metal bands to compress the preform thickness to a volume fraction of 55%. The prepared preform was immersed in a 35% polycarbosilane / xylene solution under vacuum conditions of <100Pa for 3 hours, cured at 270℃ for 2 hours under high-purity nitrogen protection, and kept at 1100℃ for 3 hours to complete a round of impregnation-curing-cracking. After three times, the mold was removed and the impregnation-curing-cracking was repeated for 15 rounds to complete the densification of the SiC matrix, and the density was 2.05g / cm 3 C f / SiC components.
[0077] The three sides of the flow channel inside the component are milled to the required roughness, the bottom surface is processed through with a 0.5° slope according to the design requirements, and the end face and outer surface are polished smooth and flat.
[0078] The machined C fThe SiC flow channel lining component is placed in a high-temperature furnace, and low-pressure isothermal chemical vapor deposition is carried out using trichloromethylsilane as silicon and carbon source gas, hydrogen as carrier gas and dilution gas, and argon as protective gas. The deposition temperature is 1060°C, the infiltration time is 45 hours, and the infiltration pressure is 1000Pa; the flow ratio of the reaction gases is trichloromethylsilane: hydrogen: argon is 1:30:30.
[0079] The phenolic resin mixed with curing agent was impregnated with high silica fiber cloth and wound layer by layer at an angle of 15° on the C f / SiC flow channel lining outer surface, 190 ℃ mold curing and demoulding, to obtain a 4mm thick high silicon oxygen insulation layer structure as shown in the figure Figure 2 shown.
[0080] The alloy shell is cast using GH625 steel sand mold, and the surface is machined and polished to the design roughness. The mating surface with high silicon oxide insulation layer is machined at a 1.5° assembly angle. f The SiC flow channel lining component is inserted into the alloy shell to obtain a three-layer structure square straight flow inlet, such as Figure 3 shown.
[0081] Example 2
[0082] Three-layer square straight air intake, using C f / SiC lining, high silicon oxygen insulation layer and GH2132 high temperature alloy steel shell.
[0083] The T-700 continuous carbon fiber 2.5D is used to make a preform that imitates the engine intake duct. The volume fraction of carbon fiber in the preform is 35%, and the initial density of the preform is 0.48g / cm 3 The preform is in the shape of a 600*200*90mm square hollow tubular structure. Before use, the preform is heated at 900°C for two hours in a nitrogen atmosphere for degumming treatment.
[0084] The fiber preform was placed in a high-temperature resistant vacuum sintering furnace, and the furnace temperature was raised to 1120°C under continuous vacuum conditions. Natural gas and nitrogen were then introduced with gas flow rates of 0.8 L / min and 3.2 L / min, respectively. The deposition lasted for 15 hours and the pressure in the furnace was maintained at 3000 Pa. The thickness of the pyrolytic carbon interface on the prepared fiber surface was 500 nm.
[0085] The preform is loaded into the graphite core mold and four-sided graphite plates, fixed with high-temperature alloy bolts, and the metal pressure rods are tied to compress the preform thickness to 60% by volume. The prepared preform is immersed in 50% polycarbosilane / xylene solution under vacuum degree <100Pa for 3 hours, cured at 270℃ for 2 hours under high-purity nitrogen protection, and kept at 1100℃ for 3 hours to complete a round of impregnation-curing-cracking. After three times, the mold is removed and the impregnation-curing-cracking is repeated for 13 rounds to complete the densification of the SiC matrix and obtain a density of 2.00g / cm 3 C f / SiC components.
[0086] The four sides of the internal flow channel of the component are milled to the required roughness, and the end faces and outer surfaces are polished smooth and flat.
[0087] The machined C f The SiC flow channel lining component is placed in a high-temperature furnace, and low-pressure isothermal chemical vapor deposition is carried out using trichloromethylsilane as silicon and carbon source gas, hydrogen as carrier gas and dilution gas, and argon as protective gas. The deposition temperature is 1000°C, the infiltration time is 30 hours, and the infiltration pressure is 1350Pa; the flow ratio of the reaction gases is trichloromethylsilane: hydrogen: argon is 1:30:30.
[0088] The phenolic resin mixed with curing agent was impregnated with high silica fiber cloth and wound layer by layer at an angle of 10° on the C f / SiC flow channel lining outer surface, 190 ℃ molding and curing followed by demolding to obtain a 3mm thick high silicon oxygen thermal insulation layer.
[0089] The alloy shell is cast using GH2132 steel sand mold, and the surface is machined and polished to the roughness required by the design. The mating surface with the high silicon oxide insulation layer is machined at a 1° assembly angle. f The / SiC flow channel lining component is inserted into the alloy shell to obtain a three-layer structure square straight flow inlet.
[0090] Figure 4 The intake duct passes the high temperature ablation test. f The electron microscope image and EDS spectrum of the inner surface of the SiC composite lining show that the surface of the composite component is covered with glassy substances. In addition to Si and C signals, O elements appear on the surface of the material, proving that the SiO2 produced during the ablation process is wrapped on the surface of the material and has a certain barrier effect on the internal material, thereby improving the stability of the material in a high-temperature ablation environment. This proves that the use of C f The feasibility of replacing high-temperature alloys with / SiC composite materials as the intake duct lining solution.
[0091] Comparative Case 1
[0092] The preform adopts the same initial volume fraction as in Example 2, and the fiber interface coating preparation process is the same as in Example 2. During the matrix densification process of the precursor impregnation and pyrolysis process, no graphite mold is used to compress the thickness of the preform in the first three rounds of impregnation-pyrolysis. After experimental comparison, it is found that compared with the existing precursor impregnation and pyrolysis process, the C prepared in Example 2 of the present invention is f The porosity of the / SiC composite material is only 1.83%, and the flexural strength is increased from 435MPa to 520.1MPa. Figure 5 a) with Figure 5 b) By comparison, it is found that the number of pores in the composite matrix prepared by the mold tooling force curing-cracking is significantly reduced, and only a small number of small-sized pores exist in the fiber bundle. It is proved that the use of tooling force curing-cracking process can effectively increase the fiber volume fraction of the preform, reduce the material porosity, and improve the mechanical strength of the material. The following table shows the case comparison.
[0093] <![CDATA[C f / SiC Comparison]]> Fiber volume fraction Material density Material porosity Bending Strength Embodiment 2 of the present invention 60% <![CDATA[2.00g / cm 3 ]]> 1.83% 520.1MPa Comparative Example 1 35% <![CDATA[1.82g / cm 3 ]]> 11.6% 435MPa
[0094] Example 3
[0095] Three-layer variable cross-section straight-flow inlet adopts C f / SiC lining, high silicon oxygen thermal insulation layer and GH4169 high temperature alloy steel shell.
[0096] The T-700 continuous carbon fiber 2.5D is used to make a preform that imitates the engine intake duct. The volume fraction of carbon fiber in the preform is 40%, and the initial density of the preform is 0.52g / cm 3 The preform has a 500*180*65mm variable cross-section hollow tubular structure. Before use, the preform is heated at 900°C for two hours in a nitrogen atmosphere for degumming treatment.
[0097] The fiber preform was placed in a high-temperature resistant vacuum sintering furnace, and the furnace temperature was raised to 1080°C under continuous vacuum conditions. Natural gas and nitrogen were then introduced with gas flow rates of 1.0 L / min and 4.0 L / min, respectively. The deposition lasted for 10 hours, and the pressure in the furnace was maintained at 6000 Pa. The thickness of the pyrolytic carbon interface on the prepared fiber surface was 1200 nm.
[0098] The preform is loaded into the graphite core mold and four-sided graphite plates, fixed with high-temperature alloy bolts, and tied with metal bands to compress the preform thickness to 70% by volume. The prepared preform is immersed in a 45% polycarbosilane / xylene solution under vacuum conditions of <100Pa for 3 hours, cured at 270℃ for 2 hours under high-purity nitrogen protection, and kept at 1100℃ for 3 hours to complete a round of impregnation-cracking. After three times, the mold is removed and the impregnation-cracking is repeated for 15 rounds to complete the densification of the SiC matrix, and the density is 2.18g / cm 3 C f / SiC components.
[0099] The four sides of the internal flow channel of the component are milled to the required roughness, and the end faces and outer surfaces are polished smooth and flat.
[0100] The machined C f The SiC flow channel lining component was placed in a high-temperature furnace, and trichloromethylsilane was used as the silicon and carbon source gas, hydrogen was used as the carrier gas and dilution gas, and argon was used as the protective gas for low-pressure isothermal chemical vapor deposition. The deposition temperature was 1100°C, the deposition time was 60 hours, and the deposition pressure was 1500Pa. The flow ratio of the participating reaction gases was trichloromethylsilane: hydrogen: argon was 1:30:30. After the densification, the C f / Schematic diagram of the SiC flow channel lining component structure Figure 6-10 shown.
[0101] Phenolic resin mixed with curing agent is impregnated with high silica fiber cloth and wrapped layer by layer at an angle of 20° on C f / SiC flow channel lining outer surface, 190 ℃ molding and curing followed by demolding to obtain a 5mm thick high silicon oxygen thermal insulation layer.
[0102] The split alloy housing is cast using GH4169 steel sand mold. The split flange has a reserved annular groove, and the surface is machined and polished to the roughness required by the design. The sealing graphite packing is installed in the annular groove of the flange, and the C with insulation layer is installed. f After the SiC flow channel lining component is inserted into the alloy shell, the split high-temperature alloy shell is fastened with IN-718 high-temperature alloy bolts to obtain a three-layer structure variable-section direct current air inlet.
[0103] Comparative Case 2
[0104] The rough blank of the integral air intake duct was casted with GH4169 steel sand mold, heat treated at 1180℃ for 20 hours, and machined and surface polished to obtain an integral variable cross-section direct current high-temperature alloy air intake duct component with the same size as the three-layer variable cross-section direct current air intake duct of Example 3. Compared with the air intake duct component of Comparative Example 2, the weight of the air intake duct of Example 3 is reduced by 3 / 5, and the operating temperature is increased from 1255K to 1700K, which proves that the use of C f / SiC channel lining instead of high-temperature alloy can significantly reduce the overall weight of the component. At the same time, since the composite material blocks most of the heat, the temperature resistance of the component is greatly improved.
Claims
1. An air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle, characterized in that: The invention comprises a carbon fiber reinforced silicon carbide ceramic matrix composite material flow channel lining (1), a high silica / phenolic resin thermal insulation layer (2) and a high temperature alloy shell layer (3), wherein the inner side of the high silica / phenolic resin thermal insulation layer (2) is matched with the outer side of the carbon fiber reinforced silicon carbide ceramic matrix composite material flow channel lining (1), and the outer side of the high silica / phenolic resin thermal insulation layer (2) is matched with the inner side of the high temperature alloy shell layer (3).
2. The method for preparing an air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle according to claim 1, characterized in that: The following steps are used: S1: preparing a carbon fiber preform that is shaped like an engine intake duct; S2: Densifying the contoured carbon fiber preform into a carbon fiber reinforced silicon carbide ceramic matrix composite material flow channel lining through precursor impregnation pyrolysis and chemical vapor deposition process; S3: high silica fiber plain cloth prepreg is prepared on the outer surface of the carbon fiber reinforced silicon carbide ceramic matrix composite flow channel lining by continuous winding and molding curing process to obtain a high silica / phenolic resin insulation layer; S4: A high-temperature alloy shell layer is prepared outside the high-silica / phenolic resin insulation layer using a high-temperature alloy steel sand casting molding process.
3. The method for preparing an air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle according to claim 2, characterized in that: Step S2 is specifically as follows: S21: Fiber interface coating treatment The contoured carbon fiber preform made of 2.5D-T700 carbon fiber is placed in a high temperature resistant vacuum sintering furnace for isothermal chemical vapor deposition process to obtain a preform with a pyrolytic carbon interface layer; S22: Precursor impregnation pyrolysis process matrix densification The preform obtained in step S21 is densified by using a precursor impregnation cracking process, and a silicon carbide matrix is introduced to obtain C f / SiC components; S23: Machining The C obtained in step S22 is processed by a numerically controlled machine tool. f / Cut and grind the outer surface and end face of SiC components, and mill the inner surface of the flow channel to obtain the flow channel lining shape and surface roughness required by the design; S24: Sealing and component surface coating deposition The C machined in step S23 is deposited by low pressure isothermal chemical vapor deposition process. f CVI-SiC coating is introduced on the surface of / SiC components to fill the pores on the surface of the components.
4. The method for preparing an air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle according to claim 3, characterized in that: Step S21 is specifically as follows: A carbon fiber preform with a fiber volume fraction of 30% to 40% is placed in a high-temperature vacuum sintering furnace and kept at 900°C for two hours in a nitrogen atmosphere. Subsequently, deposition is performed using natural gas as the carbon source gas and nitrogen as the dilution and protective gas. The deposition temperature is 1050 to 1120°C, the deposition time is 10 to 15 hours, and the deposition pressure is 3000 to 6000Pa. The natural gas flow rate is 0.5 to 1.1 L / min, and the nitrogen flow rate is 2 to 4 L / min. After the deposition is completed, the pyrolytic carbon interface thickness should be ensured to be 500 to 1200 nm.
5. The method for preparing an air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle according to claim 3, characterized in that: Step S22 is specifically as follows: The preform processed in step S21 is fixed with a graphite mold, and a compressive force is applied in the thickness direction of the preform to obtain a preform with a high fiber volume fraction of 55% to 70%; The preform is immersed in a 35% to 50% polycarbosilane / xylene solution under vacuum conditions and maintained under pressure for 3 hours, then cured at 270°C for 2 hours, and then pyrolyzed at 1100°C for 3 hours; The above impregnation-curing-cracking process is repeated 3 to 4 times until the density of the preform reaches a predetermined value, and then the graphite mold is removed. The above impregnation-curing-cracking process is continued to be repeated until the preform weight gain rate is less than 1% to complete the high fiber volume fraction matrix densification process.
6. The method for preparing an air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle according to claim 3 or 5, characterized in that: In step S22, the graphite mold is fastened by high-temperature alloy bolts, graphite bolts or C / C bolts, and compression force is applied using metal pressure rods, pressure strips or strapping tapes; the curing and high-temperature cracking process is carried out in a high-purity nitrogen atmosphere.
7. The method for preparing an air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle according to claim 3, characterized in that: Step S24 is specifically as follows: After the machining in step S23, f / SiC components are placed in a high-temperature furnace, trichloromethylsilane is used as silicon and carbon source gas, hydrogen is used as carrier gas and dilution gas, argon is used as protective gas, and low-pressure isothermal chemical vapor deposition is performed, the deposition temperature is 1000-1100°C, the deposition time is 30-60 hours, and the deposition pressure is 1000-1500Pa; The flow ratio of the reaction gases is 1:30:30 for trichloromethylsilane:hydrogen:argon; The final C f / SiC component density should be >2.0g / cm 3 .
8. The method for preparing an air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle according to claim 2, characterized in that: In step S3, the winding angle of the high-silica fiber plain cloth prepreg is 10-20°, and the molding temperature is 190° C.; the thickness of the high-silica / phenolic resin insulation layer is 3-5 mm.
9. The method for preparing an air intake duct with a multi-layer structure suitable for a high-performance engine of an aerospace vehicle according to claim 2, characterized in that: The high-temperature alloy shell layer is made of cast alloy steel of one of GH4169, GH2132, DD406 and GH625; the mating surfaces of the high-temperature alloy shell layer and the high-silicon / phenolic resin insulation layer are set at an assembly angle of 1 to 3 degrees.