Method for determining furnace condition of blast furnace based on iron reduction degree determination

By sampling and separating the slag, iron and coke of the air outlet materials in the blast furnace and measuring their reduction degree, the problem of difficulty in obtaining internal information of the blast furnace is solved, and targeted adjustment of blast furnace operation is achieved, optimizing the furnace condition and reducing fuel costs.

CN119043980AActive Publication Date: 2024-11-29武汉钢铁有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411166725.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The amount of initial slag generated in the blast furnace and the reduction degree of iron at the air outlet plane are difficult to obtain, which leads to unclear reasons for the fluctuation of the furnace condition and lacks targeted adjustments, resulting in long fluctuation of the furnace condition and increased iron cost. There is a lack of effective method to analyze the internal conditions of the blast furnace. .

Method used

By inserting the sampling tube into the blast furnace after the blast furnace rest, sampling the air outlet materials and separating the slag, iron and coke in sections, measuring the weight ratio of the air outlet slag and iron reduction degree, calculating the mathematical average value to judge the blast furnace condition, and adjusting according to the results Raw fuel performance indicators and operation optimization furnace conditions.

Benefits of technology

Targeted adjustment of blast furnace operation, optimize furnace conditions, reduce fuel ratios, and improve blast furnace operation efficiency and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119043980A_ABST
    Figure CN119043980A_ABST
Patent Text Reader

Abstract

The invention discloses a method for determining blast furnace conditions based on iron reduction degree determination, and relates to the field of blast furnace ironmaking. The method for determining the furnace condition of the blast furnace based on iron reduction degree measurement comprises the following steps: sampling from the blast furnace after damping down of the blast furnace to obtain tuyere materials distributed along the radial direction of a hearth, and cooling; segmenting the tuyere material, and separating slag, iron and coke to obtain tuyere slag and tuyere iron of each section of tuyere material distributed along the radial direction of the hearth; weighing and calculating to obtain a tuyere slag weight ratio; measuring the mass of metallic iron and total iron in each section of tuyere iron in the sampling pipe, and calculating the reduction degree of each section of tuyere iron in the sampling pipe and the mathematical average value of the reduction degree of each section of tuyere iron; and judging the blast furnace condition according to the weight ratio of the tuyere slag and the mathematical average value of the reduction degree of each section of tuyere iron in the sampling pipe. According to the method for determining the blast furnace condition based on iron reduction degree determination, the blast furnace condition is determined by sampling the slag proportion of the blast furnace tuyere material and the iron reduction degree.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of blast furnace ironmaking, and in particular, to a method for judging the condition of a blast furnace based on the determination of the degree of reduction of iron. Background Art

[0002] As the main raw material for blast furnace ironmaking, coke can act as a reducing agent, provide heat, provide a carbon source and provide skeleton support. Above the blast furnace tuyere area, especially in the dripping zone, the iron ore and flux have melted. At this time, only coke is the skeleton that supports the blast furnace charge and bears the erosion of molten iron and liquid slag. Therefore, blast furnace coke requires a certain block composition and strength index in order to have good air permeability in the blast furnace. Blast furnace tuyere coke can directly reflect the material state in the blast furnace, and it is one of the hot research areas that ironmaking workers have long attached great importance to. The characteristics of blast furnace tuyere materials provide a basis for judging the working condition of the hearth and adjusting the material distribution system.

[0003] However, information such as the amount of primary slag generated inside the blast furnace and the degree of reduction of iron at the tuyere plane is usually difficult to obtain. The furnace condition can only be analyzed through indicators such as the composition of slag and iron discharged from the iron mouth, which leads to unclear mechanisms for fluctuations in furnace conditions and lacks targeted adjustments to furnace conditions, resulting in long fluctuations in furnace conditions and increased iron costs. In addition, there is little quantitative analysis of slag in blast furnace tuyere materials and a lack of calculation of the metallization rate of tuyere iron, which means that blast furnace operators lack effective means to analyze the internal conditions of the blast furnace. Summary of the invention

[0004] The purpose of the present application is to provide a method for judging the blast furnace condition based on the determination of the iron reduction degree, which judges the blast furnace condition by sampling the slag ratio and the iron reduction degree of the blast furnace tuyere material, thereby specifically adjusting the performance indicators of the raw fuel, optimizing the blast furnace operation to make the furnace condition smooth and reduce the fuel ratio.

[0005] This application is implemented as follows:

[0006] The present application provides a method for determining the condition of a blast furnace based on the determination of the degree of reduction of iron, comprising the following steps:

[0007] After the blast furnace is shut down, the sampling tube is horizontally inserted into the blast furnace through the tuyere to the center of the furnace, and the tuyere materials distributed along the radial direction of the furnace are sampled from the blast furnace and then cooled;

[0008] The tuyere material in the sampling tube is segmented and then slag, iron and coke are separated to obtain tuyere slag and tuyere iron of each segment of tuyere material distributed along the radial direction of the furnace;

[0009] Weigh and calculate the tuyere slag weight ratio Ps;

[0010] Determine the mass of metallic iron MFe and total iron TFe in each section of tuyere iron in the sampling tube, calculate the reduction degree R of each section of tuyere iron in the sampling tube, and calculate the mathematical average of the reduction degree of each section of tuyere iron in the sampling tube.

[0011] According to the mathematical average of the tuyere slag weight ratio Ps and the reduction degree of each section of the tuyere iron in the sampling tube Determine the blast furnace condition.

[0012] In some optional implementation schemes, the tuyere sleeve of the blast furnace is first dismantled for sampling, and then a blast furnace tuyere coke sampler is used to horizontally insert the sampling tube through the tuyere into the center of the furnace.

[0013] In some optional embodiments, the sampling tube is separated into sections every 0.25-0.5 m.

[0014] In some optional implementation schemes, the tuyere material in the sampling tube is segmented and then subjected to magnetic separation to separate the slag, iron and coke.

[0015] In some optional implementation schemes, the tuyere slag weight ratio Ps is calculated according to the following formula: Ps=Ws / W; wherein Ws is the total weight of the tuyere slag in the sampling tube, and W is the total weight W of the tuyere material in the sampling tube.

[0016] In some optional embodiments, the reduction degree R of the tuyere iron is the mass ratio of metallic iron MFe to total iron TFe in the tuyere iron.

[0017] In some optional embodiments, when the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, it means that the ore is not fully reduced when it passes through the blocky zone, soft melting zone and dripping zone from top to bottom in the blast furnace and reaches the tuyere plane, resulting in low ore metallization rate and small amount of slag.

[0018] In some optional embodiments, when the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, the softening start stabilization and softening end temperature of the blast furnace sintered ore are reduced by 8-10°C.

[0019] In some optional embodiments, when the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, the distribution angle is moved toward the edge and the amount of central coke is reduced to strengthen the central airflow of the blast furnace.

[0020] In some optional embodiments, when the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, the coke thermal strength CSR is increased to more than 68%.

[0021] The beneficial effects of the present application are as follows: the method for judging the blast furnace condition based on the determination of the degree of reduction of iron provided in the present application comprises the following steps: after the blast furnace is shut down, a sampling tube is horizontally inserted into the blast furnace through the tuyere to the center of the furnace cylinder, and a tuyere material radially distributed along the furnace cylinder is sampled from the blast furnace and then cooled; the tuyere material in the sampling tube is segmented and then slag, iron and coke are separated to obtain tuyere slag and tuyere iron of each section of tuyere material radially distributed along the furnace cylinder; the tuyere slag weight ratio Ps is obtained by weighing and calculating; the mass of metallic iron MFe and total iron TFe in each section of tuyere iron in the sampling tube is determined, and the degree of reduction R of each section of tuyere iron in the sampling tube is calculated, and the mathematical average value of the degree of reduction of each section of tuyere iron in the sampling tube is calculated. According to the mathematical average of the tuyere slag weight ratio Ps and the reduction degree of each section of the tuyere iron in the sampling tube Determine the blast furnace condition. The method for determining the blast furnace condition based on the determination of the iron reduction degree provided in the present application determines the blast furnace condition by sampling the slag ratio and the iron reduction degree of the blast furnace tuyere material, thereby specifically adjusting the performance indicators of the raw fuel, optimizing the blast furnace operation to make the furnace condition smooth and reduce the fuel ratio. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 A schematic flow chart of a method for determining blast furnace conditions based on iron reduction degree measurement provided in an embodiment of the present application. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in combination with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments.

[0025] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for which protection is sought, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0026] In the description of the present application, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate the orientation or position relationship that the product of the application is usually placed in when used. They are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they should not be understood as limitations on the present application.

[0027] like Figure 1 As shown, the embodiment of the present application provides a method for judging the blast furnace condition based on the determination of the reduction degree of iron, comprising the following steps:

[0028] Step 1: prepare a sampling tube that can be extended from the tuyere to the center of the furnace cylinder along the radial direction of the furnace cylinder, separate a section at intervals of 0.25-0.5m in the sampling tube, and then take samples; after the blast furnace is shut down, first remove the tuyere small sleeve of the blast furnace, and then use the blast furnace tuyere coke sampling machine to horizontally insert the sampling tube into the blast furnace through the tuyere to the center of the furnace cylinder, sample the tuyere materials distributed along the radial direction of the furnace cylinder from the blast furnace, and then cool them down. The tuyere materials include tuyere coke, tuyere slag, and tuyere iron;

[0029] Step 2: The tuyere material in the sampling tube is divided into various sections and taken out, and then the tuyere coke, tuyere slag and tuyere iron are separated by magnetic separation to obtain the tuyere slag and tuyere iron of each section distributed along the radial direction of the furnace;

[0030] Step 3, weigh the tuyere slag, tuyere iron and tuyere coke of each compartment distributed along the radial direction of the furnace and calculate the total weight W of the tuyere material sampled by the sampling tube and the total weight Ws of the tuyere slag of each compartment in the sampling tube, and further calculate the tuyere slag weight ratio Ps, Ps = Ws / W;

[0031] Step 4: After the tuyere iron of each compartment in the sampling tube is subjected to particle size screening, the tuyere iron samples of each compartment are obtained according to the particle size ratio, reduction, and weighing. The tuyere iron samples of each compartment are crushed in a crusher to less than 120 meshes, and the content of metallic iron MFe and the content of total iron TFe in the tuyere iron samples of each compartment are respectively determined, and the reduction degree R of the tuyere iron of each compartment in the sampling tube is calculated. The reduction degree R of the tuyere iron of each compartment is the mass ratio of metallic iron MFe and total iron TFe in the tuyere iron of each compartment, and the mathematical average of the reduction degree of the tuyere iron of each compartment in the sampling tube is calculated.

[0032] Step 5: According to the mathematical average of the tuyere slag weight ratio Ps and the reduction degree of each tuyere iron in the sampling tube To judge the blast furnace condition, the mathematical average of the reduction degree of each tuyere iron in the sampling tube is used. When the tuyere slag weight ratio Ps is less than 4%, it means that the ore is not fully reduced when it passes through the blocky zone, soft melting zone and dripping zone from top to bottom in the blast furnace and reaches the tuyere plane, resulting in low ore metallization rate and small amount of slag.

[0033] Step 6: According to the mathematical average of the tuyere slag weight ratio Ps and the reduction degree of each tuyere iron in the sampling tube After judging the blast furnace condition, adjust the blast furnace condition:

[0034] 6.1. When the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, the softening start stabilization and softening end temperatures of the blast furnace sintered ore are reduced to increase the blast furnace soft melting zone height by 8-10°C, thereby increasing the soft melting zone height.

[0035] 6.2. When the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, adjust the distribution system, move the distribution angle toward the edge, reduce the amount of central coke, appropriately strengthen the central airflow, maintain the uniformity of blast furnace gas flow distribution, control the blast furnace temperature at medium to upper, control the Si content of molten iron at about 0.5%, i.e. 0.48-0.52%, and appropriately increase the molten iron temperature to ensure sufficient physical heat in the furnace.

[0036] 6.3. When the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, the coke thermal strength CSR is increased to more than 68%.

[0037] The principle of the method for judging the blast furnace condition based on the determination of the degree of reduction of iron provided in the embodiment of the present application is: the blast furnace soft melting zone is composed of many solid coke layers and semi-molten ore layers bonded together. The coke ore in the blast furnace soft melting zone is alternate and clearly layered. Since the ore is in a soft melting state, the permeability is extremely poor. The coal gas mainly passes through the coke layer like a window, so it is called a "coke window". The upper edge of the blast furnace soft melting zone is the softening line, and the lower edge is the melting line. It is consistent with the soft melting temperature range of the ore. The highest part is called the top of the soft melting zone, and the lowest part is connected to the furnace wall, which is called the root of the soft melting zone. With the changes in raw material conditions and operating conditions, the shape and position of the soft melting zone change accordingly. The reactions occurring in the soft melting zone are mainly the softening of the ore and the formation of primary slag. The low melting point compounds formed by the solid phase reaction begin to soften after further heating. At the same time, the appearance of the liquid phase improves the contact conditions between the ore and the coke or flux. When the charge continues to drop and heat up, the liquid phase continues to increase, and finally softens and melts to form a flowing state. The softening of the ore to the melting flow is a link in the slag making process that has a greater impact on the blast furnace travel. The early and late formation of the initial slag and the high and low position in the blast furnace have a greater impact on the smooth travel of the blast furnace, so the blast furnace soft melting zone is also called the slag forming zone. The results of the three-dimensional dynamic simulation experiment on the morphology of the blast furnace soft melting zone in the laboratory in this application show that the use of the charging system of the development center and the center coke addition is conducive to the formation of a high-position inverted V-shaped soft melting zone, which can improve the permeability of the charge column and reduce the total pressure drop in the furnace. It is an effective means to increase the amount of coal injection, dredge the gas flow in the furnace, and promote the smooth travel of the blast furnace. Blast furnace tuyere coke can directly reflect the material status in the blast furnace. By detecting the slag proportion and iron reduction degree characteristics of the tuyere material in the blast furnace tuyere, it can provide a basis for judging the working condition of the furnace and adjusting the material distribution system, so as to adjust the performance indicators of the raw fuel in a targeted manner and optimize the blast furnace operation, so as to make the furnace condition smooth and reduce the fuel ratio.

[0038] The characteristics and performance of the method for judging the blast furnace condition based on the determination of the iron reduction degree of the present application are further described in detail below in conjunction with the examples.

[0039] Example 1

[0040] The present application provides a method for judging the blast furnace condition based on the determination of iron reduction degree, for 4000m 3 The treatment is carried out in a blast furnace, comprising the following steps:

[0041] Step 1: prepare a sampling tube that can be extended from the tuyere to the center of the furnace cylinder along the radial direction of the furnace cylinder by 6.8m, separate a section at intervals of 0.5m in the sampling tube so that the sampled material does not move in the sampling tube, and then take samples; after the blast furnace is shut down, first remove the tuyere small sleeve of the blast furnace, then use the blast furnace tuyere coke sampling machine to horizontally insert the sampling tube into the blast furnace through the tuyere to the center of the furnace cylinder, sample the tuyere materials distributed along the radial direction of the furnace cylinder from the blast furnace, and then cool them down. The tuyere materials include tuyere coke, tuyere slag, and tuyere iron;

[0042] Step 2: The tuyere material in the sampling tube is divided into various sections and taken out, and then the tuyere coke, tuyere slag and tuyere iron are separated by magnetic separation to obtain the tuyere slag and tuyere iron of each section distributed along the radial direction of the furnace;

[0043] Step 3, weigh the tuyere slag, tuyere iron and tuyere coke of each compartment distributed along the radial direction of the furnace and calculate the total weight W of the tuyere material sampled by the sampling tube to be 25 kg, calculate the total weight Ws of the tuyere slag of each compartment in the sampling tube to be 0.75 kg, and further calculate the tuyere slag weight ratio Ps, Ps = Ws / W = 3%;

[0044] Step 4: Use 3mm, 5mm, 10mm, 15mm, and 25mm round hole sieves to screen the tuyere iron in each compartment of the sampling tube, and then reduce and weigh them according to the particle size ratio to obtain the tuyere iron samples in each compartment. Grind the tuyere iron samples in each compartment to less than 120 mesh in a grinder, and respectively determine the content of metallic iron MFe and total iron TFe in the tuyere iron samples in each compartment, and calculate the reduction degree R of the tuyere iron in each compartment of the sampling tube. The reduction degree R of the tuyere iron in each compartment is the mass ratio of metallic iron MFe to total iron TFe in the tuyere iron in each compartment, and calculate the mathematical average of the reduction degree of the tuyere iron in each compartment of the sampling tube.

[0045] Step 5: According to the mathematical average of the tuyere slag weight ratio Ps and the reduction degree of each tuyere iron in the sampling tube To judge the blast furnace condition, the mathematical average of the reduction degree of each tuyere iron in the sampling tube is used. When the tuyere slag weight ratio Ps is less than 4%, it means that the ore is not fully reduced when it passes through the blocky zone, soft melting zone and dripping zone from top to bottom in the blast furnace and reaches the tuyere plane, resulting in low ore metallization rate and small amount of slag, which causes the tuyere iron to need further reduction in the lower part of the furnace hearth, resulting in increased heat consumption in the lower part of the furnace hearth, increasing the blast furnace fuel consumption ratio to 525kg / t, unstable furnace condition, coal ratio of 145kg / t, and easy furnace cooling.

[0046] Step 6: According to the mathematical average of the tuyere slag weight ratio Ps and the reduction degree of each tuyere iron in the sampling tube After judging the blast furnace condition, adjust the blast furnace condition:

[0047] 6.1. When the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, the softening start stabilization and softening end temperatures of the blast furnace sintered ore are reduced to increase the blast furnace soft melting zone height by 9°C, thereby increasing the soft melting zone height.

[0048] 6.2. When the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, adjust the distribution system, move the distribution angle toward the edge, reduce the amount of central coke, appropriately strengthen the central airflow, maintain the uniformity of blast furnace gas flow distribution, control the blast furnace temperature at medium to upper, control the Si content of molten iron at 0.5%, and appropriately increase the molten iron temperature to ensure sufficient physical heat in the furnace.

[0049] 6.3. When the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, the coke thermal strength CSR is increased to more than 68%, and the permeability of the blast furnace charge column is maintained.

[0050] By adjusting the blast furnace conditions, the blast furnace fuel ratio was relatively reduced by about 5kg / t, and the coal ratio was stabilized at about 175kg / t.

[0051] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

Claims

1. A method for determining blast furnace conditions based on iron reduction degree determination, characterized in that: The following steps are involved: After the blast furnace is shut down, the sampling tube is horizontally inserted into the blast furnace through the tuyere to the center of the furnace, and the tuyere materials distributed along the radial direction of the furnace are sampled from the blast furnace and then cooled; The tuyere material in the sampling tube is segmented and then slag, iron and coke are separated to obtain tuyere slag and tuyere iron of each segment of tuyere material distributed along the radial direction of the furnace; Weigh and calculate the tuyere slag weight ratio Ps; Determine the mass of metallic iron MFe and total iron TFe in each section of tuyere iron in the sampling tube, calculate the reduction degree R of each section of tuyere iron in the sampling tube, and calculate the mathematical average of the reduction degree of each section of tuyere iron in the sampling tube. According to the mathematical average of the tuyere slag weight ratio Ps and the reduction degree of each section of the tuyere iron in the sampling tube Determine the blast furnace condition.

2. The method for judging blast furnace conditions based on iron reduction degree measurement according to claim 1, characterized in that: When sampling, first remove the blast furnace's tuyere sleeve, then use the blast furnace tuyere coke sampler to insert the sampling tube horizontally through the tuyere into the blast furnace to the center of the furnace cylinder.

3. The method for judging blast furnace conditions based on iron reduction degree measurement according to claim 1, characterized in that: The sampling tube is divided into sections at intervals of 0.25-0.5 m.

4. The method for judging blast furnace conditions based on iron reduction degree measurement according to claim 1, characterized in that: The tuyere material in the sampling tube is segmented and then subjected to magnetic separation to separate slag, iron and coke.

5. The method for judging blast furnace conditions based on iron reduction degree measurement according to claim 1, characterized in that: The tuyere slag weight ratio Ps is calculated according to the following formula: Ps=Ws / W; wherein Ws is the total weight of the tuyere slag in the sampling tube, and W is the total weight W of the tuyere material in the sampling tube.

6. The method for judging blast furnace conditions based on iron reduction degree measurement according to claim 1, characterized in that: The reduction degree R of the tuyere iron is the mass ratio of metallic iron MFe to total iron TFe in the tuyere iron.

7. The method for judging blast furnace conditions based on iron reduction degree measurement according to claim 1, characterized in that: When the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, it means that the ore is not fully reduced when it passes through the blocky zone, soft melting zone and dripping zone from top to bottom in the blast furnace and reaches the tuyere plane, resulting in low ore metallization rate and small amount of slag.

8. The method for judging blast furnace conditions based on iron reduction degree measurement according to claim 1, characterized in that: When the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, the softening start stabilization and softening end temperature of the blast furnace sintered ore are reduced by 8-10°C.

9. The method for judging blast furnace conditions based on iron reduction degree measurement according to claim 1, characterized in that: When the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, the distribution angle is moved toward the edge and the amount of central coke is reduced to strengthen the central airflow of the blast furnace.

10. The method for judging blast furnace conditions based on iron reduction degree measurement according to claim 1, characterized in that: When the mathematical average of the reduction degree of each section of the tuyere iron in the sampling tube is When the tuyere slag weight ratio Ps is less than 4%, the coke thermal strength CSR is increased to more than 68%.

Citation Information

Patent Citations

  • Blast furnace condition evaluation method based on blast furnace tuyere plane radial hearth temperature measurement

    CN115481350A

  • Method for measuring reduction degree of iron ore in blast furnace blocky zone

    CN115979885A

  • Blast furnace ore reducibility and coke reactivity matching method

    CN116256493A

  • Sampling device at air port of smelting reduction iron-making furnace

    CN201780218U

  • Quantification method for blast furnace slag analysis

    KR1020130023891A