Electrochemical sensor based on gold nanoparticle modified iron functionalized manganese dioxide hollow micro-nest material as well as preparation method and application of electrochemical sensor

By using iron-functionalized manganese dioxide hollow micronensis material modified by gold nanoparticles in electrochemical sensors, the problem of insufficient conductivity and catalytic capabilities of traditional electrochemical sensors is solved, and high sensitivity detection and anti-interference ability of BHT is achieved. , suitable for food analysis.

CN119044271APending Publication Date: 2024-11-29GUANGXI NORMAL UNIV FOR NATITIES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411387781.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-07
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

When detecting butyl hydroxytoluene (BHT), existing electrochemical sensors have poor electrical conductivity and catalytic capabilities, resulting in insufficient detection sensitivity and accuracy, and it is difficult to effectively distinguish interfering substances.

Method used

Using iron-functionalized manganese dioxide hollow micronensis material based on gold nanoparticles, Fe-MnO2@Au NPs composite material was synthesized by hydrothermal method, and modified on glass carbon electrodes to form an electrochemical sensor, which improves the conductance. The rate and active surface area enhance the electrocatalytic performance.

Benefits of technology

It realizes sensitive detection of BHT, has low detection limit, good reusability and anti-interference ability, and is suitable for food analysis, with a detection range of 0.05~32.0μM, a good linear response, and a detection limit of 13nM.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119044271A_ABST
    Figure CN119044271A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electrochemical sensors, and provides an electrochemical sensor based on a gold nanoparticle modified iron functionalized manganese dioxide hollow micro-nest material, and a preparation method and application thereof. The preparation method comprises the following steps: preparing Fe-MnO2 hollow micronests by a hydrothermal synthesis method; growing gold nanoparticles on the surface of the Fe-MnO2 hollow micro-nest in situ by adopting a mild chemical reduction method to obtain a Fe-MnO2 (at) Au NPs composite material; the preparation method comprises the following steps: modifying an electrode with a Fe-MnO2 (at) Au NPs composite material to prepare a BHT electrochemical sensor; the obtained electrochemical sensor has excellent stability and good selectivity and can be used for sensitively detecting BHT, under the optimal condition, the prepared sensor shows a good linear relation to BHT in the concentration range of 0.05-32.0 mu M, the detection limit is 13 nM, and the electrochemical sensor has wide application prospects in the field of food monitoring and analysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochemical sensors, and in particular to an electrochemical sensor based on gold nanoparticle-modified iron-functionalized manganese dioxide hollow micro-nest material, and a preparation method and application thereof. Background Art

[0002] Butylated hydroxytoluene (BHT) is a synthetic antioxidant widely used in food-related products. It can not only improve the stability of medicinal fat-soluble vitamins, but also improve the durability of rubber elastomers and plastics. However, BHT is easily degraded into aldehyde compounds in meat and food, leading to chronic poisoning in humans, so it is very important to achieve ultrasensitive detection of BHT. To date, various traditional detection techniques, such as gas chromatography-mass spectrometry (GC-MS), high-performance thin-layer chromatography (HPTLC), gas chromatography-mass spectrometry (GC-MS) and electrochemical methods, have been used for BHT analysis. Among them, electrochemical sensors based on suitable substrate active materials have the advantages of simple device, low detection limit, high sensitivity and low cost, and have been proven to be applicable to analysis in the fields of food, environment, clinical medicine, biochemical analysis, etc. In recent years, various types of electroactive materials, such as metal-organic frameworks, metal oxides, metal nanoparticles and carbon materials, have been used in different sensors.

[0003] Noble and transition metal materials, such as Au, Pt, Ti, Fe, and Mn, show good catalytic activity in electrochemical analysis. Manganese dioxide (MnO2), as a transition metal oxide, is considered to be a potential green electrochemical material due to its environmental friendliness, rich crystal forms, and flexibility. Although MnO2 has been widely used in electrochemical sensors, the main obstacle as an electrocatalyst is its poor conductivity and catalytic ability. Many researchers have addressed this limitation by combining MnO2 with highly conductive materials such as carbon materials, polythiophenes, and metal ion doping. In addition, the electrocatalytic active sites of MnO2 are mainly concentrated on the surface, so its shape and size are important for the electrochemical performance, specific surface area, and utilization of the electrocatalyst. MnO2 has special three-dimensional structures such as nanoflowers, microspheres, and Tremella, and has excellent electrocatalytic performance. In addition, MnO2 doped with metal ions such as Zn, Ni, Mg, Fe, Co, and Cu shows excellent performance in electrochemical adsorption and supercapacitors, but there is little research on how to improve its conductivity.

[0004] The present invention prepares a MnO2 hollow micronest material functionalized with transition metal iron (Fe-MnO2), which has a stable and uniform shape, greatly improves the conductivity, and exhibits the characteristics of large active surface area, low density and high porosity. We also found that it can be prepared into an electrochemical sensor for quantitative analysis of BHT, with a low detection limit, good reusability and anti-interference ability, and there is no related report at present. Summary of the invention

[0005] The purpose of the present invention is to provide an electrochemical sensor based on gold nanoparticle-modified iron-functionalized manganese dioxide hollow micronest material, a preparation method and application thereof, in view of the above-mentioned existing problems. The present invention adopts a one-pot hydrothermal method, which is simple to operate, low in cost and has a good synthesis effect. The obtained material is prepared into an electrochemical sensor for quantitative analysis of BHT, has a low detection limit, good reusability and anti-interference ability, and has potential value in the field of food analysis.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] The preparation method of the electrochemical sensor based on gold nanoparticles modified iron functionalized manganese dioxide hollow micro-nest material comprises the following steps:

[0008] (1) Preparation of Fe-MnO2 hollow micronests

[0009] Manganese sulfate monohydrate, ammonium persulfate, concentrated sulfuric acid and deionized water were mixed and stirred at room temperature to obtain a mixed solution A, and then silver nitrate and ferrous sulfate heptahydrate were added and stirred at room temperature to obtain a mixed solution B; subsequently, the mixed solution B was transferred to a high-pressure reactor and heated at 120°C for reaction for 5 to 8 hours; naturally cooled to room temperature, the obtained black precipitate was washed several times with water and ethanol respectively, and finally dried in an oven to obtain Fe-MnO2 hollow micronests;

[0010] (2) Synthesis of Fe-MnO2@Au NPs

[0011] The prepared Fe-MnO2 was dispersed in deionized water, and a Fe-MnO2 suspension was obtained by ultrasonic dispersion. Then, a chloroauric acid solution was slowly injected into the Fe-MnO2 suspension under vigorous stirring. The obtained suspension was stirred for 8 to 12 hours in the dark, and washed with ethanol to obtain a precipitate. The obtained precipitate was dispersed in deionized water again, and a sodium borohydride solution was added under vigorous stirring. The stirring was continued for 2 to 4 hours in the dark. The product was washed several times with ultrapure water and ethanol, respectively, and dried to obtain Fe-MnO2 modified with AuNPs, which was recorded as Fe-MnO2@AuNPs.

[0012] (3) Preparation of BHT sensor

[0013] The exposed glassy carbon electrode was polished and cleaned, and 3 μL of anhydrous ethanol suspension of Fe-MnO2@Au NPs with a concentration of 1 mg / mL was drop-casted on the surface of the glassy carbon electrode and dried naturally at room temperature. Subsequently, the modified electrode was rinsed with deionized water to remove the anhydrous ethanol, thereby obtaining the BHT sensor.

[0014] In the present invention, preferably, the molar volume ratio of the manganese sulfate monohydrate, ammonium persulfate, concentrated sulfuric acid and deionized water is 1 mmol: 1 mmol: 1 mL: 16-25 mL, and in the mixed solution B, the molar ratio of manganese sulfate monohydrate, silver nitrate and ferrous sulfate heptahydrate is 1: 3: 0.8.

[0015] In the present invention, preferably, the stirring time of the mixed solution A in step (1) is 50 to 70 minutes, and the stirring time of the mixed solution B is 25 to 35 minutes.

[0016] In the present invention, preferably, the molar ratio of Fe-MnO2 to chloroauric acid in the suspension is 30 mg:4-6 μmol, and the molar ratio of chloroauric acid to sodium borohydride is 1:1.

[0017] In the present invention, preferably, in step (2), the solid-liquid ratio of the Fe-MnO2 suspension is 2 mg: 1-2 mL.

[0018] In the present invention, preferably, in step (2), the rotation speed of the vigorous stirring is 1000-1500 rpm, and the chloroauric acid solution is slowly injected drop by drop.

[0019] The present invention also protects the electrochemical sensor prepared by the above preparation method.

[0020] The present invention also provides application of the electrochemical sensor prepared by the preparation method in detecting BHT.

[0021] In the present invention, further, the specific method for detecting BHT is:

[0022] (1) preparing a series of BHT standard solutions with gradient concentrations;

[0023] (2) A three-electrode system was built with the BHT sensor as the working electrode, the Ag / AgCl electrode as the reference electrode, and the Pt electrode as the auxiliary electrode. A PBS solution was used as a buffer solution, and a BHT standard solution was added to the buffer solution. BHT was detected by the current-time method to obtain a linear relationship between the cathode photocurrent and the logarithm of the concentration of the BHT standard solution;

[0024] (3) Under the same conditions as step (2), add the sample solution to be tested to the buffer solution, detect the photocurrent response of the sample solution to be tested, and use the linear relationship obtained in step (2) to obtain the concentration of BHT in the sample solution to be tested according to the measured photocurrent intensity.

[0025] In the present invention, preferably, the concentration of the PBS solution is 0.2 mol·L -1 , pH value is 5.0.

[0026] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0027] 1. The present invention synthesizes Fe-MnO2 with a three-dimensional hollow micro-nest structure by a hydrothermal method, and then in situ grows gold nanoparticles (Au NPs) on the surface of the Fe-MnO2 hollow micro-nest at room temperature by a mild chemical reduction method, thereby obtaining a Fe-MnO2@Au NPs composite material based on gold nanoparticles and iron-functionalized manganese dioxide hollow micro-nest. The doping of Fe and the addition of AuNPs promote electron transfer on the electrode surface and reduce the interface impedance of the electrode surface, while the large surface area of ​​Fe-MnO2 and the excellent conductivity of Au NPs make it have strong sensing performance, and finally Fe-MnO2@Au NPs provide a large number of active sites for electrochemical reactions, enhancing the electrocatalytic performance of the material. The obtained Fe-MnO2@Au NPs composite material modified glassy carbon electrode can obtain an electrochemical sensor based on Fe-MnO2@Au NPs, which has excellent stability and good selectivity and can be used to sensitively detect BHT. Under optimal conditions, the prepared sensor shows a good linear relationship for BHT in the concentration range of 0.05 to 32.0 μM, with a detection limit of 13 nM (S / N=3).

[0028] 2. The sensor has good reproducibility, stability, anti-interference ability and selectivity, and can be used for the detection of BHT in edible oil and margarine. Compared with other methods, the sensor has an acceptable linear response and a lower detection limit, and has broad application prospects in the field of food monitoring and analysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The SEM image of Fe-MnO2 prepared in Example 1 is shown;

[0030] Figure 2 This is the SEM image of Fe-MnO2@Au NPs prepared in Example;

[0031] Figure 3 TEM image of Fe-MnO2@Au NPs prepared in Example;

[0032] Figure 4 This is the EDS image of Fe-MnO2@Au NPs prepared in Example;

[0033] Figure 5 The X-ray diffraction test results of the synthetic materials obtained in the examples and comparative examples are shown;

[0034] Figure 6 CV graphs of Bare / GCE, MnO2 / GCE, Fe-MnO2 / GCE and Fe-MnO2@Au NPs / GCE obtained in Examples and Comparative Examples in PBS buffer containing BHT;

[0035] Figure 7 The results of the experiments on Bare / GCE, MnO2 / GCE, Fe-MnO2 / GCE and Fe-MnO2@Au NPs / GCE in 5 mM [Fe(CN)6] 3- / 4- EIS spectra in solution;

[0036] Figure 8 The electrochemical peak current response diagram of Fe-MnO2@Au NPs / GCE under different BHT concentrations (0.05-32 μM);

[0037] Fig. 9 It is the linear relationship diagram of current-BHT concentration;

[0038] Fig.10 Short-term stability test results of the sensor based on Fe-MnO2@Au NPs;

[0039] Fig.11 Selectivity test results of sensors based on Fe-MnO2@Au NPs. DETAILED DESCRIPTION

[0040] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] In the embodiments of the present invention, manganese sulfate monohydrate, ferrous sulfate heptahydrate, ammonium persulfate, silver nitrate, and gold chloride trihydrate were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., China. Sodium borohydride was produced from Jiangsu Qiangsheng Chemical Co., Ltd. Concentrated sulfuric acid was from Chengdu Kelong Chemical Co., Ltd., China, with a concentration of 98 wt%.

[0042] In the embodiment of the present invention, scanning electron microscope (SEM) and energy dispersive spectrometer (EDS) use EVO-18 microscope spectrometer (ZEISS, Oberkochen, Germany). X-ray diffractometer (Bruker, D8 Advanced, Germany) and X-ray photoelectron spectrometer (Thermo Fisher Scientific Co., Waltham, MA) are used for crystal phase and element analysis, respectively. Electrochemical measurements are carried out using an electrochemical workstation (CHI 760e, Chenhua Instrument Co., Ltd., Shanghai, China). The standard three-electrode system used is composed of a modified glassy carbon electrode (GCE, diameter = 3 mm) as a working electrode, a platinum wire, and a saturated calomel electrode as an auxiliary electrode and a reference electrode, respectively.

[0043] 1. Preparation Example

[0044] Example 1

[0045] The preparation method of the electrochemical sensor based on gold nanoparticles modified iron functionalized manganese dioxide hollow micro-nest material comprises the following steps:

[0046] (1) Preparation of Fe-MnO2 hollow micronests

[0047] 0.135 g of manganese sulfate monohydrate, 0.182 g of ammonium persulfate, 0.8 mL of concentrated sulfuric acid and 20 mL of deionized water were mixed and stirred at room temperature for 50 min to obtain a mixed solution A, and then 0.4 mL of 6 M silver nitrate solution and 0.183 g of ferrous sulfate heptahydrate were added and stirred at room temperature for 25 min to obtain a mixed solution B; subsequently, the mixed solution B was transferred to a high-pressure reactor and heated at 120 ° C for 5 h; it was naturally cooled to room temperature, and the obtained black precipitate was washed twice with water and ethanol respectively, and finally dried in an oven at 80 ° C for 6 h to obtain Fe-MnO2 hollow micronests;

[0048] (2) Synthesis of Fe-MnO2@Au NPs

[0049] 30 mg of the prepared Fe-MnO2 was dispersed in 20 mL of deionized water and ultrasonically dispersed for 20 min to obtain a Fe-MnO2 suspension. Then, 160 μL of 25 mM chloroauric acid solution was slowly injected dropwise into the Fe-MnO2 suspension under vigorous stirring at 1000 rpm. The resulting suspension was stirred for 8 h in the dark and washed with ethanol to obtain a precipitate. The obtained precipitate was dispersed again in 20 mL of deionized water, and 400 μL of 10 mM freshly prepared sodium borohydride solution was added under vigorous stirring at 1000 rpm. The stirring was continued for 2 h in the dark. The product was washed several times with ultrapure water and ethanol, respectively, and finally the precipitate was dried in a vacuum drying oven at 50°C to obtain a Fe-MnO2@AuNPs composite material.

[0050] (3) Preparation of BHT sensor

[0051] The exposed glassy carbon electrode was mirror-polished with alumina slurry and then rinsed with deionized water. 3 μL of anhydrous ethanol suspension of Fe-MnO2@Au NPs with a concentration of 1 mg / mL was drop-cast on the surface of the glassy carbon electrode and dried naturally at room temperature. Subsequently, the modified electrode was gently rinsed with deionized water to remove the anhydrous ethanol, thereby obtaining the BHT sensor.

[0052] Example 2

[0053] The preparation method of the electrochemical sensor based on gold nanoparticles modified iron functionalized manganese dioxide hollow micro-nest material comprises the following steps:

[0054] (1) Preparation of Fe-MnO2 hollow micronests

[0055] 0.169 g of manganese sulfate monohydrate, 0.228 g of ammonium persulfate, 1 mL of concentrated sulfuric acid and 20 mL of deionized water were mixed and stirred at room temperature for 60 min to obtain a mixed solution A, and then 0.5 mL of 6 M silver nitrate solution and 0.222 g of ferrous sulfate heptahydrate were added and stirred at room temperature for 30 min to obtain a mixed solution B; subsequently, the mixed solution B was transferred to a high-pressure reactor and heated at 120 ° C for 6 h; it was naturally cooled to room temperature, and the obtained black precipitate was washed with water and ethanol for 3 times, respectively, and finally dried in an oven at 80 ° C for 6 h to obtain Fe-MnO2 hollow micronests;

[0056] (2) Synthesis of Fe-MnO2@Au NPs

[0057] 30 mg of the prepared Fe-MnO2 was dispersed in 15 mL of deionized water and ultrasonically dispersed for 20 min to obtain a Fe-MnO2 suspension. Then, 200 μL of 25 mM chloroauric acid solution was slowly injected dropwise into the Fe-MnO2 suspension under vigorous stirring at 1200 rpm. The resulting suspension was stirred for 10 h in the dark and washed with ethanol to obtain a precipitate. The obtained precipitate was dispersed again in 20 mL of deionized water, and 500 μL of 10 mM freshly prepared sodium borohydride solution was added under vigorous stirring at 1200 rpm. The stirring was continued for 3 h in the dark. The product was washed several times with ultrapure water and ethanol respectively, and finally the precipitate was dried in a vacuum drying oven at 50°C to obtain a Fe-MnO2@AuNPs composite material.

[0058] (3) Preparation of BHT sensor

[0059] The exposed glassy carbon electrode was mirror-polished with alumina slurry and then rinsed with deionized water. 3 μL of anhydrous ethanol suspension of Fe-MnO2@Au NPs with a concentration of 1 mg / mL was drop-cast on the surface of the glassy carbon electrode and dried naturally at room temperature. Subsequently, the modified electrode was gently rinsed with deionized water to remove the anhydrous ethanol, thereby obtaining the BHT sensor.

[0060] Example 3

[0061] The preparation method of the electrochemical sensor based on gold nanoparticles modified iron-functionalized manganese dioxide hollow micro-nest material comprises the following steps:

[0062] (1) Preparation of Fe-MnO2 hollow micronests

[0063] 0.135 g of manganese sulfate monohydrate, 0.182 g of ammonium persulfate, 0.8 mL of concentrated sulfuric acid and 12.8 mL of deionized water were mixed and stirred at room temperature for 70 min to obtain a mixed solution A, and then 0.4 mL of 6 M silver nitrate solution and 0.183 g of ferrous sulfate heptahydrate were added and stirred at room temperature for 35 min to obtain a mixed solution B; subsequently, the mixed solution B was transferred to a high-pressure reactor and heated at 120 ° C for 8 h; it was naturally cooled to room temperature, and the obtained black precipitate was washed several times with water and ethanol respectively, and finally dried in an oven at 80 ° C for 6 h to obtain Fe-MnO2 hollow micronests;

[0064] (2) Synthesis of Fe-MnO2@Au NPs

[0065] 30 mg of the prepared Fe-MnO2 was dispersed in 30 mL of deionized water and ultrasonically dispersed for 20 min to obtain a Fe-MnO2 suspension. Then, 240 μL of 25 mM chloroauric acid solution was slowly injected dropwise into the Fe-MnO2 suspension under vigorous stirring at 1500 rpm. The resulting suspension was stirred for 12 h in the dark and washed with ethanol to obtain a precipitate. The obtained precipitate was dispersed again in 20 mL of deionized water, and 600 μL of 10 mM freshly prepared sodium borohydride solution was added under vigorous stirring at 1500 rpm. The stirring was continued for 4 h in the dark. The product was washed 3 times with ultrapure water and ethanol respectively, and finally the precipitate was dried in a vacuum drying oven at 50°C to obtain a Fe-MnO2@AuNPs composite material.

[0066] (3) Preparation of BHT sensor

[0067] The exposed glassy carbon electrode was mirror-polished with alumina slurry and then rinsed with deionized water. 3 μL of anhydrous ethanol suspension of Fe-MnO2@Au NPs with a concentration of 1 mg / mL was drop-cast on the surface of the glassy carbon electrode and dried naturally at room temperature. Subsequently, the modified electrode was gently rinsed with deionized water to remove the anhydrous ethanol, thereby obtaining the BHT sensor.

[0068] Comparative Example 1

[0069] The MnO2 / GCE electrode was prepared, which was different from Example 2 in that ferrous sulfate heptahydrate was not added in step (1).

[0070] The details are as follows:

[0071] (1) Preparation of MnO2

[0072] 0.169 g of manganese sulfate monohydrate, 0.228 g of ammonium persulfate, 1 mL of concentrated sulfuric acid and 20 mL of deionized water were mixed and stirred at room temperature for 60 min to obtain a mixed solution A, and then 0.5 mL of 6 M silver nitrate solution was added and stirred at room temperature for 30 min to obtain a mixed solution B; subsequently, the mixed solution B was transferred to a high-pressure reactor and heated at 120°C for 6 h; the mixture was naturally cooled to room temperature, and the obtained black precipitate was washed with water and ethanol three times respectively, and finally dried in an oven at 80°C for 6 h to obtain MnO2;

[0073] (2) Preparation of MnO2 / GCE electrode

[0074] The exposed glassy carbon electrode was mirror-polished with alumina slurry and then rinsed with deionized water. 3 μL of anhydrous ethanol suspension with a concentration of 1 mg / mL MnO2 was drop-cast on the surface of the glassy carbon electrode and dried naturally at room temperature. Subsequently, the modified electrode was gently rinsed with deionized water to remove the anhydrous ethanol.

[0075] Comparative Example 2

[0076] The Fe-MnO2 / GCE electrode was prepared. The difference from Example 2 is that there is no step (2), and the GCE electrode prepared in step (1) is directly used for modification, as follows:

[0077] (1) Preparation of Fe-MnO2 hollow micronests

[0078] 0.169 g of manganese sulfate monohydrate, 0.228 g of ammonium persulfate, 1 mL of concentrated sulfuric acid and 20 mL of deionized water were mixed and stirred at room temperature for 60 min to obtain a mixed solution A, and then 0.5 mL of 6 M silver nitrate solution and 0.222 g of ferrous sulfate heptahydrate were added and stirred at room temperature for 30 min to obtain a mixed solution B; subsequently, the mixed solution B was transferred to a high-pressure reactor and heated at 120 ° C for 6 h; it was naturally cooled to room temperature, and the obtained black precipitate was washed with water and ethanol for 3 times, respectively, and finally dried in an oven at 80 ° C for 6 h to obtain Fe-MnO2 hollow micronests;

[0079] (2) Preparation of Fe-MnO2 / GCE electrode

[0080] The exposed glassy carbon electrode was mirror-polished with alumina slurry and then rinsed with deionized water. 3 μL of anhydrous ethanol suspension with a concentration of 1 mg / mL Fe-MnO2 was drop-cast on the surface of the glassy carbon electrode and dried naturally at room temperature. Subsequently, the modified electrode was gently rinsed with deionized water to remove the anhydrous ethanol.

[0081] 2. Characterization of Materials

[0082] In order to gain a deeper understanding of the chemical composition of the gold nanoparticle-modified iron-functionalized manganese dioxide hollow micronest material of the present invention, we characterized the material.

[0083] The surface morphology of Fe-MnO2 and Fe-MnO2@Au NPs was characterized by scanning electron microscopy (SEM) and transmission electron microscopy (TEM). Figure 1 The results show that the prepared Fe-MnO2 has a hollow microsphere structure with uniform size and a diameter of about 1 μm. The presence of the polymerization initiator (ammonium persulfate) forms active oxygen radicals by heating, which promotes the uniform nucleation of the hollow Fe-MnO2 microsphere structure. The Fe-MnO2@Au NPs were generated by in situ growth method without collapse, such as Figure 2 In addition, the TEM image of Fe-MnO2 is shown in Figure 3 The results show that the synthesized microspheres have a hollow structure and are composed of nanosheets.

[0084] Figure 4This is the energy dispersive spectrometer (EDS) analysis result of the prepared Fe-MnO2@Au NPs, in which the peaks of Mn, Fe, O and Au elements are obvious, indicating that the Fe-MnO2@Au NPs are successfully synthesized.

[0085] To determine the crystalline phase of the materials, the X-ray diffraction (XRD) patterns of MnO2, Fe-MnO2 and Fe-MnO2@Au NPs were studied. Figure 5 The figures in the figure are (A) XRD pattern of the synthesized material, (B) XPS analysis of Fe-MnO2@AuNPs; (C)-(F) are high-resolution scanning spectra of Fe 2p, Mn 2p, O 1s, and Au 4f, respectively. Figure 5 It can be seen that the diffraction peaks at 28.82° and 37.49° point to the (130) and (121) planes of α-MnO2, respectively, indicating that α-MnO2 has good crystallinity. Compared with α-MnO2, the characteristic diffraction peaks of Fe-MnO2 have a small angle shift, which may be due to the doping of Fe with a larger ionic radius in the α-MnO2 lattice, resulting in the expansion of the crystal structure. For the XRD spectrum of Fe-MnO2@Au NPs, the two diffraction peaks at 37.61° and 42.28° correspond to the (111) and (200) planes of Au NPs, respectively. The diffraction peak at 37.61° may be the overlapping peak of the Fe-MnO2 (121) and AuNPs (200) crystal planes.

[0086] The elemental composition and chemical state of Fe-MnO2@Au NPs were characterized by X-ray photoelectron spectroscopy (XPS). Figure 5 B) Figure 5 C, the high-resolution Fe 2p XPS spectrum has two peaks at 711.67eV and 724.71eV, which belong to the Fe 2p 3 / 2 and Fe 2p 1 / 2 In Fe 2p 1 / 2 and Fe 2p 3 / 2 There is a satellite peak of 717.80 eV between the two, indicating that the valence state of Fe-MnO2 is +3. Figure 5 D shows that the peak values ​​of Mn 2p are 641.91eV and 653.72eV, respectively, which are consistent with the peak values ​​of Mn 2p 3 / 2 and Mn 2p 1 / 2 Fit. Figure 5 In E, the high-resolution XPS pattern of O 1s conforms to Gauss's law, and the peaks at 529.55 eV and 531.36 eV correspond to Mn-O and HOH groups, respectively. In addition, the two peaks at 84.15 eV and 89.14 eV are Au 4f 7 / 2 and 4f5 / 2 , with an energy difference of 4.99 eV, indicating the growth of 0-valent Au. These results illustrate the successful synthesis of Fe-MnO2@Au NPs.

[0087] In summary, the characterization of the materials revealed the successful synthesis of Fe-MnO2@AuNPs, and the synthesized microspheres had a hollow structure composed of nanosheets.

[0088] 3. Electrochemical performance experiment

[0089] The electrochemical properties of Bare / GCE, MnO2 / GCE prepared in Comparative Example 1, Fe-MnO2 / GCE prepared in Comparative Example 2, and Fe-MnO2@Au NPs / GCE prepared in Example 2 in 0.2M PBS (pH 5.0) buffer containing 50 μM BHT were studied by cyclic voltammetry (CV). Figure 6 As shown. It can be seen that Fe-MnO2@AuNPs / GCE has a sharp oxidation peak at 0.08V, which is attributed to the synergistic effect of Fe-MnO2 and Au NPs. In the presence of the same concentration of BHT, there is no obvious peak on bare / GCE, Fe-MnO2 / GCE and MnO2 / GCE, indicating that BHT cannot be electrochemically detected on these modified electrodes.

[0090] In 5 mM [Fe(CN)6] 3- / 4- In solution, electrochemical impedance spectroscopy (EIS) was used to study the electrochemical interface characteristics of different electrodes. The diameter of the semicircular part in the high-frequency region represents the electron transfer resistance (Rct). Figure 7 The Nyquist plots of various modified electrodes and the schematic diagram of the Randel equivalent circuit applied to the EIS model are depicted.

[0091] The circuit model is composed of Z w , R ct , R s The Rct values ​​of Bare / GCE, MnO2 / GCE, Fe-MnO2 / GCE and Fe-MnO2@Au NPs / GCE were approximately 41.3Ω, 622.5Ω, 562.0Ω and 290.5Ω, respectively, accompanied by a more obvious semicircular part. Fe-MnO2@AuNPs showed a smaller Rct value than Fe-MnO2 / GCE and MnO2 / GCE. ct In addition, the apparent rate constant (k app ) quantitatively studies the reaction kinetics of the electron transfer process, and its calculation method is based on Nicholson theory

[0092]

[0093] R is the ideal gas constant (8.314 J·mol -1 ·K -1 ), T is the thermodynamic temperature (298.15K). F and C are the Faraday constants (96485C·mol -1 ) and the concentration of the redox pair (mol·L -1 ). The higher the kapp value, the faster the reaction rate on the modified electrode. app Value (2.37×10 -5 cm / s) is much higher than the k of MnO2 / GCE app Value (2.14×10 -5 cm / s), indicating that Fe doping accelerates the electron transfer rate. Compared with MnO2 / GCE and Fe-MnO2 / GCE, the k app Value (4.5×10 -5 The electron transfer rate of Au NPs on Fe-MnO2 was much higher than that of Au NPs on Fe-MnO2, which was attributed to the accelerated electron transfer rate. The results showed that Fe-MnO2@Au NPs had fast charge transfer efficiency and excellent electronic properties.

[0094] 4. Determination of BHT

[0095] The specific method for detecting BHT of the present invention is:

[0096] (1) Prepare a series of BHT standard solutions with gradient concentrations; the specific concentrations are: 0.05, 3.5, 6.0, 8.5, 10.5, 12.5, 14.0, 16.0, 18.0, 21.0, 23.0, 25.0, 26.5, 28.0, 30, 32.0 μM.

[0097] (2) A three-electrode system was built with the BHT sensor as the working electrode, the Ag / AgCl electrode as the reference electrode, and the Pt electrode as the auxiliary electrode. A 0.2 M PBS solution with a pH value of 5.0 was used as a buffer solution. A BHT standard solution was added to the buffer solution, and BHT was detected by the current-time method to obtain a linear relationship between the cathode photocurrent and the logarithm of the concentration of the BHT standard solution; Figure 8 As shown, the peak current response of Fe-MnO2@Au NPs / GCE to different concentrations of BHT. It can be seen that the reduction peak current of the sensor to BHT increases in the concentration range of 0.05 to 32 μM ( Fig. 9), and its linear regression equation is Ip(μA)=0.84C(μM)+5.85(R 2 =0.9952). The calculated LOD of Fe-MnO2@AuNPs / GCE for detecting BHT was 13nM (S / N=3).

[0098] (3) Under the same conditions as step (2), add the sample solution to be tested to the buffer solution, detect the photocurrent response of the sample solution to be tested, and use the linear relationship obtained in step (2) to obtain the concentration of BHT in the sample solution to be tested according to the measured photocurrent intensity.

[0099] V. Reproducibility, stability and interference

[0100] In order to evaluate the reproducibility of the sensor, under the same conditions, five newly modified Fe-MnO2@Au NPs / GCE working electrodes were used to detect the same concentration of BHT. The relative standard deviation (RSD) of the oxidation peak current signal was 3.71%, reflecting its good reproducibility.

[0101] The same electrode was used for 12 repeated tests in a 20 μM BHT solution, and the RSD of the response current was 2.5% ( Fig.10 ). Subsequently, the electrode was stored in a refrigerator at 4°C for 1 month, and the current was still 90.7% of the initial current value. The results showed that the sensor has good short-term and long-term stability.

[0102] Anti-interference is an important characteristic of sensors. When measuring BHT under Fe-MnO2@Au NPs / GCE, some interferences that may exist in actual samples were added. Fig. 9 As shown in the figure, in a 0.1M PBS buffer solution containing 1μM BHT, the interference of Fe-MnO2@Au NPs / GCE in the presence of p-nitrophenol (PNP), acetaminophen (PCP), o-aminophenol (OAP), acetylsalicylic acid (ASA), dopamine (DA), vitamin E (VC), vitamin A (VA), vitamin D (VD), glucose (GC), leucic acid (LA) and potassium sorbate (PS) (50 times concentration) was studied. The results show that these substances have no significant effect on the determination of rutin on Fe-MnO2@Au NPs / GCE, and the sensor has good selectivity.

[0103] 6. Sample Analysis

[0104] The applicability of the sensor in actual samples was analyzed by the standard addition method, and BHT in edible oil and margarine samples was detected. First, a bottle of ordinary edible oil purchased from the supermarket was pretreated. The steps are as follows: accurately weigh 1g of edible oil sample, add 3mL of ethanol, and mix and stir evenly. After standing and stratification, the upper liquid was transferred to the evaporator and extracted twice with 3mL of ethanol. Then the upper liquid was transferred to the evaporating dish and placed in the fume hood at room temperature until the extract was completely evaporated. 10mL of 0.2M pH=5.0 PBS buffer was added to the evaporating dish as the test solution. Margarine was treated in the same way. The test results are shown in Table 1. The results show that the sensor can detect BHT with a recovery rate of 97.4-103.93%. The relative standard deviation (RSD) of the two samples is no more than 4.34%, indicating that the sensor can be successfully used for the analysis of BHT in actual samples.

[0105] Table 1 Detection results of BHT in edible oil and margarine samples (n=5)

[0106] sample Addition amount (μM) Measured amount (μM) RSD(%) Spiked recovery rate (%) 5 4.87 4.34 97.40 Peanut Oil 15 15.14 3.58 100.93 25 25.88 2.42 103.52 5 4.91 4.20 98.2 Margarine 15 15.59 3.16 103.93 25 25.71 2.11 102.84

[0107] The above description is a detailed description of the preferred feasible embodiments of the present invention, but the embodiments are not intended to limit the scope of the patent application of the present invention. All equivalent changes or modified changes completed under the technical spirit suggested by the present invention should fall within the patent scope covered by the present invention.

Claims

1. A method for preparing an electrochemical sensor based on gold nanoparticles modified iron-functionalized manganese dioxide hollow micronest material, characterized in that: The following steps are involved: (1) Preparation of Fe-MnO2 hollow micronests Manganese sulfate monohydrate, ammonium persulfate, concentrated sulfuric acid and deionized water were mixed and stirred at room temperature to obtain a mixed solution A, and then silver nitrate and ferrous sulfate heptahydrate were added and stirred at room temperature to obtain a mixed solution B; subsequently, the mixed solution B was transferred to a high-pressure reactor and heated at 120°C for reaction for 5 to 8 hours; naturally cooled to room temperature, the obtained black precipitate was washed several times with water and ethanol respectively, and finally dried in an oven to obtain Fe-MnO2 hollow micronests; (2) Synthesis of Fe-MnO2@Au NPs The prepared Fe-MnO2 hollow micronests were dispersed in deionized water, and Fe-MnO2 suspension was obtained by ultrasonic dispersion. Then, chloroauric acid solution was slowly injected into the Fe-MnO2 suspension under vigorous stirring. The obtained suspension was stirred for 8 to 12 hours in the dark, and washed with ethanol to obtain a precipitate. The obtained precipitate was dispersed in deionized water again, and sodium borohydride solution was added under vigorous stirring, and stirring was continued for 2 to 4 hours in the dark. The product was washed several times with ultrapure water and ethanol, respectively, and dried to obtain Fe-MnO2 modified with AuNPs, which was recorded as Fe-MnO2@AuNPs. (3) Preparation of BHT sensor The exposed glassy carbon electrode was polished and cleaned, and 3 μL of anhydrous ethanol suspension of Fe-MnO2@Au NPs with a concentration of 1 mg / mL was drop-casted on the surface of the glassy carbon electrode and dried naturally at room temperature. Subsequently, the modified electrode was rinsed with deionized water to remove the anhydrous ethanol, thereby obtaining the BHT sensor.

2. The preparation method according to claim 1, characterized in that: The molar volume ratio of the manganese sulfate monohydrate, ammonium persulfate, concentrated sulfuric acid and deionized water is 1 mmol:1 mmol:1 mL:16-25 mL. In the mixed solution B, the molar ratio of manganese sulfate monohydrate, silver nitrate and ferrous sulfate heptahydrate is 1:3:0.

8.

3. The preparation method according to claim 1, characterized in that: The stirring time of the mixed solution A in step (1) is 50 to 70 minutes, and the stirring time of the mixed solution B is 25 to 35 minutes.

4. The preparation method according to claim 1, characterized in that: In step (2), the molar ratio of Fe-MnO2 to chloroauric acid in the suspension is 30 mg:4-6 μmol, and the molar ratio of chloroauric acid to sodium borohydride is 1:

1.

5. The preparation method according to claim 1, characterized in that: In step (2), the solid-liquid ratio of the Fe-MnO2 suspension is 2 mg: 1-2 mL.

6. The preparation method according to claim 1, characterized in that: In step (2), the rotation speed of the vigorous stirring is 1000-1500 rpm, and the chloroauric acid solution is slowly injected drop by drop.

7. An electrochemical sensor prepared according to the preparation method according to any one of claims 1 to 6.

8. Use of the electrochemical sensor prepared by the preparation method according to any one of claims 1 to 6 in detecting BHT.

9. The use according to claim 7, characterized in that: The specific method for detecting BHT is: (1) preparing a series of BHT standard solutions with gradient concentrations; (2) A three-electrode system was built with the BHT sensor as the working electrode, the Ag / AgCl electrode as the reference electrode, and the Pt electrode as the auxiliary electrode. A PBS solution was used as a buffer solution, and a BHT standard solution was added to the buffer solution. BHT was detected by the current-time method to obtain a linear relationship between the cathode photocurrent and the logarithm of the concentration of the BHT standard solution; (3) Under the same conditions as step (2), add the sample solution to be tested to the buffer solution, detect the photocurrent response of the sample solution to be tested, and use the linear relationship obtained in step (2) to obtain the concentration of BHT in the sample solution to be tested according to the measured photocurrent intensity.

10. The use according to claim 9, characterized in that: The concentration of the PBS solution is 0.2 mol·L -1 , pH value is 5.0.