Functionalized gold-silver nano-alloy wire composite photoelectric material and preparation method and application thereof

By preparing AuAg NWs and rGO-C3N4 composite materials and combining them with extended macrocyclic columnar aromatic hydrocarbon WP6[6], a high-sensitivity, wide-range, and environmentally friendly 5-HT photoelectrochemical sensor was constructed, which solved the problems of low sensitivity, poor selectivity and complicated operation of existing detection methods, and achieved efficient and stable 5-HT detection.

CN119044273AActive Publication Date: 2024-11-29NANTONG UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411105149.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-29
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

Existing 5-HT detection methods suffer from low sensitivity, poor selectivity, complex operation, expensive instruments, limited detection range, and serious environmental pollution.

Method used

Functionalized gold and silver nano-alloy wire composite optoelectronic materials were used to prepare AuAg NWs and rGO-C3N4 composite materials, combined with extended macrocyclic columnar aromatic hydrocarbon WP6[6] to form an optochemical sensor with high specific surface area and host-guest complexing ability for the detection of 5-HT.

Benefits of technology

It achieves high sensitivity (0.7640 μA cm⁻² μmol⁻¹), wide detection range (0.01–100 μmol/L), low detection limit (2 nmol/L), high stability and reproducibility (relative standard deviation of 2.8% for 5 experiments), and environmentally friendly 5-HT detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119044273A_ABST
    Figure CN119044273A_ABST
Patent Text Reader

Abstract

The invention discloses a functionalized gold and silver nano alloy wire composite photoelectric material and a preparation method and application thereof, the surface of a gold and silver nano alloy wire AuAg NWs is coated with an expanded large ring column [6] arene molecule AuAg-WP6 capable of performing subject-object complexation reaction with a serotonin molecule 5-HT, and the expanded large ring column [6] arene molecule AuAg-WP6 is loaded on a reduced graphene oxide and carbon nitride rGO-C3N4 composite material. A PEC biosensing system is designed, AuAg-coated WP6 / rGO-C3N4 is used as a sensing material, charge separation is promoted by utilizing an LSPR effect of AuAg NWs under visible light illumination, a large amount of 5-HT can be selectively adsorbed to the surface of the material by virtue of host-guest complexation of WP6, and g-C3N4 and rGO have similar pi-like conjugated structures, so that g-C3N4 and rGO are easy to bond to form an rGO-C3N4 composite material, and the material can be applied to the field of biosensing. The photogenerated holes on the rGO-C3N4 can accelerate the oxidation of serotonin molecules, the photocurrent response is further improved to detect the 5-HT, and based on the excellent photoelectrochemical properties of the composite material, the linear range is 0.01-100 [mu] M when the 5-HT is detected, and the detection limit is 2nM (S / N = 3).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photoelectrochemistry, and specifically relates to a functionalized gold-silver nano alloy wire composite photoelectric material and a preparation method and application thereof. Background Art

[0002] Serotonin, also known as 5-hydroxytryptamine, is an important neurotransmitter that acts on the central nervous system and some peripheral organs. It plays a role in regulating anxiety, mood, appetite and even sleep. Its level changes are closely related to a variety of nervous system diseases and peripheral organ diseases, including anxiety, depression, Parkinson's disease, insomnia, gastrointestinal diseases and heart diseases. 5-HT has complex connections with endocrine, diabetes and even cancer. 5-HT can be used as an important biomarker for some diseases.

[0003] The content of 5-HT in normal human urine is about 300-1650nM. Similarly, the content of 5-HT in blood is about 262-1550nM 5-HT. Commonly used 5-HT detection methods include high performance liquid chromatography, enzyme-linked immunosorbent assay, and electrochemical method. These methods require specific enzymes or special strategies to improve the selectivity of the determination method. The complex operation also limits their development. Therefore, there is an urgent need for a 5-HT detection method with high sensitivity, strong selectivity, fast and convenient. Photoelectrochemical (PEC) detection technology is an emerging bioanalysis method developed based on electrochemical detection technology. Due to the separation of excitation signal and detection signal (electricity), this detection method has a lower background signal, thereby obtaining a higher signal-to-noise ratio, and therefore has ultra-high sensitivity.

[0004] Using precious metal nanoparticles with unique LSPR effect to modify electrode materials is an effective way to enhance the PEC performance of materials. By integrating the LSPR performance of Au and the good conductivity of Ag, a layer of Au was plated on the surface of Ag NWs by ion exchange method on the previously synthesized silver nanowires (Ag NWs), and a gold-silver nanowire (AuAg NWs) composite material was successfully synthesized. This material not only has good photoelectrochemical properties, but also has excellent charge transfer ability. In PEC sensing, good specific recognition ability is indispensable. Traditional sensors based on Au or Ag are often restricted by the lack of specific recognition ability. Therefore, it is necessary to add a sensing strategy for specific recognition of 5-HT to PEC sensing. The unique size-adjustable cavity structure, host-guest complexing ability, and highly adjustable functionalized edges of water-soluble columnar aromatics provide a new method for specific recognition of target substances to build specific sensors. In addition, pillar[n]arenes with groups such as amine (-NH2) or carboxyl (-COOH) can be easily functionalized with Au or other inorganic nanomaterials, and the above groups can be designed to be specific groups that bind to target species.

[0005] Reduced graphene oxide (rGO) is a good adsorption material and electrochemically active material with the characteristics of large surface area, high conductivity, strong adsorption capacity and good visible light absorption capacity. Therefore, rGO with a large surface area can load AuAg NWs and promote charge transfer. Graphitic carbon nitride (g-C3N4) is widely used in the field of photoelectrochemistry because of its strong light absorption ability, excellent stability and easy synthesis. However, due to the small specific surface area of ​​g-C3N4 and the problem of easy recombination of photogenerated carriers, its widespread use is limited. Therefore, it is necessary to modify it with suitable materials to avoid these problems. Summary of the invention

[0006] Technical issues solved:

[0007] In order to solve the technical problems of low sensitivity, limited detection range, expensive instruments and the like in the existing detection technology, the present application provides a functionalized gold-silver nano alloy wire composite optoelectronic material and its preparation method and application.

[0008] Technical solution:

[0009] To achieve the above objectives, this application is implemented through the following technical solutions:

[0010] The preparation method of the functionalized gold-silver nano alloy wire composite photoelectric material specifically comprises the following steps:

[0011] Step 1: Preparation of anionic water-soluble [2]biphenyl extended column [6]arene WP6;

[0012] The second step is to prepare a silver nanowire solution: 85-90g of polyvinyl pyrrolidone with a molecular weight of 58,000 is dissolved in 5-15mL of 1,2-propylene glycol, and the solution is transferred to a 25mL flask, heated in an oil bath at 150-170°C and continuously stirred at 450rpm for 1-2 hours; 1-2mL of sodium chloride dissolved in 1,2-propylene glycol is quickly added, and the sodium chloride concentration is 1mM. After stirring at 450rpm for 5-10 minutes, 3-5mL of 0.15M silver nitrate 1,2-propylene glycol solution is added dropwise with a syringe pump, and then heated at 450rpm for 30-60 minutes to obtain a silvery white AgNWs crude solution, the centrifuge speed is controlled to 6500-7500rpm, and the Ag NWs crude solution is centrifuged and washed with ultrapure water using a centrifuge to obtain pure Ag nanowires, and the pure Ag NWs are dispersed in 20-25mL of ultrapure water for subsequent storage and use;

[0013] Step 3: Prepare the gold-silver nanowire solution: add 2-3 mL of 20 mM sodium hydroxide aqueous solution, 100-120 μL of 25.4 mM chloroauric acid aqueous solution and 17-19 mL of ultrapure water into the reactor, and stir at 500 rpm for 1-2 hours at room temperature to obtain a mixed solution A; add 40-50 mg of PVP to 3-5 mL of ultrapure water and heat at 60°C to obtain a solution B; after 2 minutes, add 500-600 μL of 100 mM anti- Ascorbic acid AA and 500-600 μL of 200 mM sodium hydroxide were added to solution B. After stirring at 500 rpm for 5 minutes, 700-800 μL of the AgNWs solution prepared in the second step was added to solution B to obtain a mixed solution C. After rapid stirring at 800 rpm for 10 minutes, the mixed solution A was dripped into the mixed solution C drop by drop at a rate of one drop per 3 seconds until the dripping was completed. After heating and stirring at 800 rpm for 10-20 minutes, the reaction was stopped to obtain a crude AuAg NWs solution. The crude AuAg NWs solution was centrifugally washed with ultrapure water at 6500-7500 rpm to obtain pure AuAg NWs. The product was dispersed in 7-8 mL of ultrapure water for subsequent use.

[0014] Step 4: Prepare AuAg@WP6 NWs by ultrasonic method: take 0.1-0.2 mL of AuAg NWs synthesized in step 3, add 0.8-1 mL of ultrapure water, add 1-1.5 mg of WP6 and ultrasonicate for 1-2 hours to prepare AuAg@WP6 NWs;

[0015] The fifth step is to prepare reduced graphene oxide by graphene oxide: 10-20 mg of graphene oxide GO and 10-15 mL of ultrapure water are added to a flask and dispersed by ultrasonic treatment for 1-2 hours to obtain a GO dispersion, the GO dispersion is added to a reactor, and 45-50 mL of ethanol is added, the pH of the mixed solution is adjusted with a 1 M potassium hydroxide aqueous solution and the pH value is detected with a pH test paper, when the pH of the dispersion reaches 9.0-10.0, the reactor is placed in an oven and heated at 80-85°C for two hours to obtain a product rGO precipitate, the black precipitate is ultrasonically dispersed and centrifuged and washed with deionized water to obtain a pure rGO dispersion, and dispersed in 20-25 mL of ultrapure water to obtain 0.6 mg mL -1 rGO dispersion;

[0016] Step 6: Prepare reduced graphene oxide-carbon nitride rGO-C3N4 by compounding graphene-like π-conjugated structure with graphene: 5 mg of graphene-carbon nitride g-C3N4 was dissolved in 2 mL of isopropanol and stirred at 450 rpm to obtain 2.5 mg mL -1g-C3N4 suspension; 0.03mL g-C3N4 suspension and 0.5mL rGO dispersion were mixed and stirred at 450rpm to obtain rGO-C3N4 composite suspension;

[0017] In the seventh step, 10 μL of the rGO-C3N4 solution prepared in the sixth step was dropped on the surface of the glassy carbon electrode polished smooth with alumina and dried at 50°C. Then 10 μL of the AuAg@WP6 NWs solution prepared in the fourth step was dropped on the electrode surface and dried at 50°C to obtain the AuAg@WP6 / rGO-C3N4 composite photoelectric material for subsequent use.

[0018] Furthermore, the second step of preparing the silver nanowire solution is specifically as follows:

[0019] S1. Dissolve 87 g of polyvinyl pyrrolidone with a molecular weight of 58,000 in 10 mL of 1,2-propylene glycol and transfer to a 25 mL flask, heat in an oil bath at 160 °C and stir continuously at 450 rpm for 1 hour;

[0020] S2, quickly add 1 mL of sodium chloride dissolved in 1,2-propylene glycol to a sodium chloride concentration of 1 mM, stir at 450 rpm for 5 minutes, then add 4 mL of 0.15 M silver nitrate 1,2-propylene glycol solution dropwise using a syringe pump, then heat and stir at 450 rpm for 40 minutes to obtain a silvery white Ag NWs crude solution;

[0021] S3, controlling the centrifuge speed to 7000 rpm, using a centrifuge and ultrapure water to centrifuge and wash the crude Ag NWs solution to obtain pure Ag nanowires;

[0022] S4. Use 20 mL of ultrapure water to disperse the pure Ag NWs for subsequent storage and use.

[0023] Furthermore, the third step of preparing the gold-silver nanowire solution by the ion exchange method specifically comprises the following steps:

[0024] Step 1: Add 2 mL of 20 mM sodium hydroxide aqueous solution, 100 μL of 25.4 mM chloroauric acid aqueous solution and 17.9 mL of ultrapure water into a reaction kettle, and stir at 500 rpm for 1 hour at room temperature to obtain a mixed solution A;

[0025] Step 2: Add 40 mg of PVP to 3 mL of ultrapure water and heat at 60°C to obtain solution B;

[0026] Step 3: After 2 minutes, 500 μL of 100 mM ascorbic acid AA and 500 μL of 200 mM sodium hydroxide were added to solution B. After stirring at 500 rpm for 5 minutes, 700 μL of the AgNWs solution prepared in the second step was added to solution B to obtain a mixed solution C. After rapid stirring at 800 rpm for 10 minutes, the mixed solution A was dripped into the mixed solution C drop by drop at a speed of one drop per 3 seconds. After the dripping was completed, the mixture was heated and stirred at 800 rpm for 10 minutes, and then the reaction was stopped to obtain a crude AuAg NWs solution.

[0027] Step 4: Wash the crude AuAg NWs solution with ultrapure water by centrifugation at 7000 rpm for several times to obtain pure AuAgNWs, and disperse the product in 7 mL ultrapure water for subsequent use.

[0028] Furthermore, in the first step, anionic water-soluble [2]biphenyl extended column [6]arene WP6 is prepared, and the process route is as follows:

[0029] Furthermore, in the fourth step, 0.14 mL of the AuAgNWs synthesized in the third step was taken, 0.86 mL of ultrapure water was added, and 1.26 mg of WP6 was added and ultrasonicated for 1.5 hours to prepare AuAg@WP6 NWs.

[0030] Furthermore, the fifth step of preparing reduced graphene oxide by graphene oxide is specifically as follows:

[0031] Step a: 14 mg of graphene oxide GO and 10 mL of ultrapure water were added into a flask and dispersed by ultrasonication for 2 hours to obtain a GO dispersion;

[0032] Step b: Add the GO dispersion into the reactor, add 46 mL of ethanol, adjust the pH of the mixed solution with a 1 M potassium hydroxide aqueous solution, and detect the pH value with a pH test paper. When the pH of the dispersion reaches 9.0-10.0, place the reactor in an oven and heat at 80°C for two hours to obtain the product rGO precipitate;

[0033] Step c: Ultrasonic dispersion of the black precipitate was performed and washed with centrifugal centrifuge and deionized water to obtain a pure rGO dispersion, which was then dispersed in 23 mL of ultrapure water to obtain 0.6 mg mL -1 of rGO dispersion.

[0034] A functionalized gold-silver nano alloy wire composite photoelectric material prepared by any of the above preparation methods.

[0035] The present application also discloses the application of functionalized gold-silver nano alloy wire composite photoelectric material in a novel signal switch type photoelectrochemical PEC sensing system. 210 μL of rGO-C3N4 composite photoelectric material solution was drop-coated on the glassy carbon electrode and dried at 50 °C. Then, 10 μL of AuAg@WP6 NWs composite photoelectric material solution was drop-coated on the electrode surface and dried at 50 °C to prepare AuAg@WP6 / rGO-C3N4 / GCE nanocomposite electrode.

[0036] Furthermore, the novel signal switch type photoelectrochemical PEC sensing system uses a conventional three-electrode system to

[0037] AuAg@WP6 / rGO-C3N4 / GCE nanocomposite electrode was used as the working electrode, platinum mesh was used as the counter electrode, and saturated calomel electrode SCE was used as the reference electrode. A xenon lamp was used to simulate a visible light source to irradiate the surface of AuAg@WP6 / rGO-C3N4 / GCE, and the shading interval time was controlled as an adjustable "on-off". Then, an electrochemical workstation was used for photoelectrochemical detection in a phosphate buffer solution containing serotonin.

[0038] Principle explanation: Through the ion exchange method, a layer of Au was plated on the surface of Ag NWs to successfully synthesize the gold-silver alloy nanowire AuAg NWs composite material, and the AuAg NWs were functionalized with extended column [6] aromatic hydrocarbons to prepare AuAg@WP6. Then, reduced graphene oxide was prepared by graphene oxide, and the two were composited by graphene phase carbon nitride and graphene through a π-conjugated structure similar to that of graphene to prepare reduced graphene oxide-carbon nitride (rGO-C3N4). Finally, rGO-C3N4 with a large surface area was used to load

[0039] AuAg@WP6, preparation of AuAg@WP6 / rGO-C3N4 composite photoelectric materials.

[0040] Beneficial effects:

[0041] The present application provides a functionalized gold-silver nano alloy wire composite photoelectric material and a preparation method and application thereof, which has the following beneficial effects compared with the prior art:

[0042] 1. This application designs AuAg alloy nanowires that form localized surface plasmon resonance effects under visible light, as well as extended macrocyclic columnar [6] aromatic hydrocarbon WP6 with stronger host-guest complexing ability, and reduced graphene oxide-carbon nitride composite materials with large specific surface area, redox performance, and strong light absorption ability, which can be used for photoelectrochemical detection of serotonin (5-HT);

[0043] 2. This application solves the technical problems of the original detection technology, such as low sensitivity, limited detection range, serious environmental pollution, expensive instruments, need for specialized operators, low efficiency, slow speed, and difficult operation;

[0044] 3. The detection range of the functionalized gold-silver nano alloy wire composite photoelectric material of this application is 0.01-100 μmol / L, and the sensitivity is 0.7640 μAcm -2 μmol / L -1 , the detection limit is 2nmol / L (S / N);

[0045] 4. The expanded macrocyclic column [6] square hydrocarbon synthesized in this application has a good host-guest complexation with serotonin molecules, and the host-guest complexation constant is 13721;

[0046] 5. The detection of serotonin molecules in this application has good stability and reproducibility, and the relative standard deviation measured by 5 parallel experiments is 2.8%;

[0047] 6. The anionic water-soluble [2]biphenyl-extended column [6]arene modified with 8 ammonium salt ions, referred to as extended macrocyclic WP6, used in this application has a larger cavity volume than the traditional column [5] and column [6]arene, and it can be ionized in water to release NH4 + ions, thus carrying a negative charge, and expanding the macrocyclic WP6 molecular structure to resemble a root tube, with 4 -COONH4 groups on each side. After dissolving in water, the -COONH4 groups on both sides will form free NH4 + cation, leaving behind the negatively charged -COO - , electrostatically attracts the positively charged 5-HT molecule, enters its cavity, and undergoes a host-guest complexation reaction. Compared with the traditional WP5 and WP6, the synthesized extended macrocyclic WP6 has a larger cavity volume, so the host-guest complexation ability is stronger. In addition, -COO - The strong interaction between Au and WP6 can combine with AuAgNWs to prepare AuAg@WP6 NWs, so that the composite material can selectively recognize 5-HT while having excellent photoelectrochemical properties. However, AuAg NWs are large in size and require a material with a large surface area as a substrate material to load AuAg NWs. g-C3N4 and graphene have similar π-conjugated structures, which makes the two easy to bond. By using a suitable method to composite the two materials with rGO-C3N4, it is bound to improve the photoelectrochemical performance of the composite material while solving the problems of small specific surface area and high carrier recombination rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 : are SEM images of the present application, wherein A is a SEM image of AgNWs; B is a SEM image of AuAg NWs; C is a SEM image of rGO-C3N4; D is a SEM image of AuAg@WP6 / rGO-C3N4;

[0049] Figure 2 It is the XRD powder diffraction pattern and the external visible absorption spectrum of the present application, wherein A is the XRD powder diffraction pattern of rGO-C3N4, AuAg@WP6, and AuAg@WP6 / rGO-C3N4, and B is the ultraviolet absorption spectrum of Ag, AuAg, WP6, and AuAg@WP6;

[0050] Figure 3 2 are the time current (IT) curves and Nyquist (EIS) diagrams of the present application under visible light irradiation, wherein a is Ag / GCE, b is AuAg / GCE, c is AuAg@WP6 / GCE, and d is the time current (IT) curve of AuAg@WP6 / rGO-C3N4 / GCE in 20mL 0.1M phosphate buffer solution (pH=7.0) containing 0.02mM 5-HT under visible light irradiation as shown in Figure A; the Nyquist (EIS) diagrams of Ag / GCE (a), AuAg / GCE (b), AuAg@WP6 / GCE (c), and AuAg@WP6 / rGO-C3N4 / GCE (d) in a mixed solution of 5mM K3[Fe(CN)6] / K4[Fe(CN)6] and 0.1M KCl are shown in Figure B;

[0051] Figure 4 The differential pulse voltammetry curve (A) and the linear fitting curve of the oxidation peak current (B) of the sensor of the present application to 0.01-100 μmol / L 5-HT;

[0052] Figure 5 This is a flow chart of the synthetic method of the expanded macrocyclic column [6] aromatic hydrocarbon WP6 in this application. DETAILED DESCRIPTION

[0053] The present invention is further described below in conjunction with examples. The examples are only used to illustrate the present invention and do not constitute a limitation on the scope of the claims. Other alternative means that can be thought of by those skilled in the art are all within the scope of the claims of the present invention.

[0054] Embodiment 1:

[0055] The preparation method of the functionalized gold-silver nano alloy wire composite photoelectric material specifically comprises the following steps:

[0056] The first step is to prepare anionic water-soluble [2]biphenyl extended column [6]arene WP6:

[0057]

[0058] The second step is to prepare a silver nanowire solution: 87 g of polyvinyl pyrrolidone with a molecular weight of 58,000 is dissolved in 10 mL of 1,2-propylene glycol and transferred to a 25 mL flask, heated in a 160°C oil bath and stirred continuously at 450 rpm for 1 hour; 1 mL of sodium chloride dissolved in 1,2-propylene glycol is quickly added, and the sodium chloride concentration is 1 mM. After stirring at 450 rpm for 5 minutes, 4 mL of 0.15 M silver nitrate 1,2-propylene glycol solution is added dropwise with a syringe pump, and then heated and stirred at 450 rpm for 40 minutes to obtain a silvery white AgNWs crude solution. The centrifuge speed is controlled to 7000 rpm, and the Ag NWs crude solution is centrifuged and washed with ultrapure water using a centrifuge to obtain pure Ag nanowires, and the pure Ag NWs are dispersed in 20 mL of ultrapure water for subsequent storage and use;

[0059] Step 3: Preparation of gold and silver nanowire solution: 2 mL of 20 mM sodium hydroxide aqueous solution, 100 μL of 25.4 mM chloroauric acid aqueous solution and 17.9 mL of ultrapure water were added to the reactor, and stirred at 500 rpm for 1 hour at room temperature to obtain a mixed solution A; 40 mg of PVP was added to 3 mL of ultrapure water and heated at 60 ° C to obtain a solution B; 2 minutes later, 500 μL of 100 mM ascorbic acid AA and 500 μL of 200 mM sodium hydroxide were added to the B solution, and after stirring at 500 rpm for 5 minutes, 700 μL of the AgNWs solution prepared in the second step was added to the B solution to obtain a mixed solution C; after rapid stirring at 800 rpm for 10 minutes, the mixed solution A was dripped drop by drop into the mixed solution C at a speed of one drop per 3 seconds, and continued to heat and stir at 800 rpm for 10 minutes until the dripping was completed, and then the reaction was stopped to obtain a crude AuAg NWs solution, and the AuAg was centrifuged and washed with ultrapure water at 7000 rpm. The NWs crude solution was used to obtain pure AuAgNWs, and the product was dispersed in 7 mL of ultrapure water for subsequent use;

[0060] The fourth step was to prepare AuAg@WP6 NWs by ultrasonic method: 0.14 mL of AuAg NWs synthesized in the third step was added with 0.86 mL of ultrapure water and 1.26 mg of WP6 and ultrasonicated for 1.5 h to prepare AuAg@WP6 NWs;

[0061] The fifth step is to prepare reduced graphene oxide by graphene oxide: 14 mg of graphene oxide GO and 10 mL of ultrapure water are added to a flask and dispersed by ultrasonication for 2 hours to obtain a GO dispersion, the GO dispersion is added to a reactor, and 46 mL of ethanol is added, the pH of the mixed solution is adjusted with a 1 M potassium hydroxide aqueous solution and the pH value is detected with a pH test paper, when the pH of the dispersion reaches 9.0-10.0, the reactor is placed in an oven and heated at 80 ° C for two hours to obtain a product rGO precipitate, the black precipitate is ultrasonically dispersed and centrifuged and washed with deionized water to obtain a pure rGO dispersion, which is dispersed in 23 mL of ultrapure water to obtain 0.6 mg mL -1 rGO dispersion;

[0062] Step 6: Prepare reduced graphene oxide-carbon nitride rGO-C3N4 by compounding graphene-like π-conjugated structure with graphene: 5 mg of graphene-carbon nitride g-C3N4 was dissolved in 2 mL of isopropanol and stirred at 450 rpm to obtain 2.5 mg mL -1 g-C3N4 suspension; 0.03mL g-C3N4 suspension and 0.5mL rGO dispersion were mixed and stirred at 450rpm to obtain rGO-C3N4 composite suspension;

[0063] In the seventh step, 10 μL of the rGO-C3N4 solution prepared in the sixth step was dropped on the surface of the glassy carbon electrode polished with alumina and dried at 50°C. Then, 10 μL of the AuAg@WP6 NWs solution prepared in the fourth step was dropped on the electrode surface and dried at 50°C.

[0064] After drying, AuAg@WP6 / rGO-C3N4 composite photoelectric material was obtained for subsequent use.

[0065] Example 2

[0066] An application of the composite photoelectric material AuAg@WP6 / rGO-C3N4 prepared in Example 1 in a novel signal switch type photoelectrochemical (PEC) sensing system, wherein the electrode is placed in a phosphate buffer solution containing serotonin for photoelectrochemical detection of 5-HT by the novel signal switch type photoelectrochemical PEC sensing system, wherein the novel signal switch type photoelectrochemical PEC sensing system uses a traditional three-electrode system, with the AuAg@WP6 / rGO-C3N4 electrode as the working electrode, the platinum metal mesh electrode as the counter electrode, and the saturated calomel electrode SCE as the reference electrode. Photoelectrochemical detection is performed using an electrochemical workstation, and a xenon lamp is used as a simulation power supply.

[0067] Performance Testing

[0068] 1. Morphological determination of Ag, AuAg, rGO-C3N4 and AuAg@WP6 / rGO-C3N4

[0069] like Figure 1 A shows a typical Ag nanowire image. The prepared Ag NWs have uniform size and complete morphology. Figure 1 In Figure B, it can be seen that the surface of AuAg NWs prepared by ion exchange method is smooth. Figure 1 As shown in C, rGO-C3N4 nanosheets are composed of many lamellar structures and have a large surface area, so they have enough area to load AuAg@WP6NWs. In addition, Figure 1 As shown in Figure D, AuAg@WP6 is evenly dispersed in rGO-C3N4 to form AuAg@WP6 / rGO-C3N4 composite materials.

[0070] 2. XRD powder diffraction and UV characterization of AuAg@WP6 / rGO-C3N4 composite photoelectric materials

[0071] Figure 2 Figure A is the XRD powder diffraction pattern of rGO-C3N4, AuAg@WP6 NWs and AuAg@WP6 / rGO-C3N4. It can be seen from the figure that AuAg@WP6 / rGO-C3N4 can clearly observe the (111), (200), (220), (311) and other crystal planes of typical AuAg NWs, the (002) crystal plane of rGO and the (100) and (002) crystal planes of g-C3N4. In addition, the peak at 21.59° is the amorphous diffraction peak of WP6, indicating the successful synthesis of AuAg@WP6 / rGO-C3N4 composite optoelectronic materials.

[0072] Figure 2 Figure B is the UV-visible absorption spectra of Ag, AuAg, WP6 and AuAg@WP6 NWs. Among them, the absorption peaks of Ag and WP6 are located at 370nm and 260nm, respectively, which is consistent with previous reports. After a layer of Au is replaced on the surface of Ag NWs, its UV absorption peak at 370nm red-shifts, which may be the effect of Au doping, and the composite material also has an absorption peak at 521nm, which is the plasma resonance absorption peak of gold. In the AuAg@WP6 NWs UV absorption spectrum, these positions have obvious absorption peaks, indicating that the materials are successfully combined. In addition, the monomer absorption peak of the composite material is weaker than that of the individual material. This is mainly because the strong absorption peak of WP6 near 260nm may affect other broad absorption peaks.

[0073] 3. Electrochemical Characterization

[0074] like Figure 3As shown in Figure A, the photoelectrochemical activity of Ag / GCE, AuAg / GCE, AuAg@WP6 / GCE, and AuAg@WP6 / rGO-C3N4 / GCE in 20mL 0.1M phosphate buffer solution (pH=7.0) containing 0.02mM 5-HT under visible light irradiation was investigated by the time current curve (it) in phosphate buffer solution containing 0.02mM serotonin. Under light conditions, the photocurrent density of AuAg@WP6 / rGO-C3N4 / GCE increased sharply, while under dark conditions, the photocurrent density decreased rapidly. Compared with Ag / GCE and AuAg@WP6 / GCE, AuAg@WP6 / rGO-C3N4 / GCE showed the strongest photocurrent density, which was mainly due to the synergistic effect between AuAg@WP6 and rGO-C3N4.

[0075] like Figure 3 As shown in B, the Nyquist spectrum (EIS) was measured in a solution containing 5.0mM K3[Fe(CN)6] / K4[Fe(CN)6] and 0.1M KCl. The diameter of the semicircle can evaluate the charge transfer resistance (Rct) of the electrode. The larger the diameter of the semicircle, the greater the charge transfer resistance. It can be seen from the figure: Ag / GCE>AuAg / GCE>AuAg@WP6 / GCE>AuAg@WP6 / rGO-C3N4 / GCE, and the electron transfer ability increases in turn, proving that the composite material has a higher charge transfer ability.

[0076] 4. Detection of serotonin

[0077] like Figure 4 As shown, the concentration of serotonin can be detected by monitoring the photocurrent intensity of the PEC sensor. The photocurrent response of the sensor is directly related to the concentration of serotonin. Figure 4 A shows that the photocurrent increases with increasing serotonin concentration. Figure 4 Middle B shows that the photocurrent response increases linearly with increasing serotonin concentration in the range of 0.01 μmol / L to 100 μmol / L. The calibration equation is I = 0.7640C 5-HT +3.2953, and the correlation coefficient is 0.9957. As the concentration of serotonin increases, the oxidation peak current density gradually increases. The photoelectrochemical sensor shows a better detection limit of 2nmol / L, which indicates that the proposed sensor may meet the improvement requirements of future serotonin analysis.

[0078] Embodiment 3:

[0079] The preparation method of the functionalized gold-silver nano alloy wire composite photoelectric material AuAg@WP6 / rGO-C3N4 specifically comprises the following steps:

[0080] The first step is to prepare anionic water-soluble [2]biphenyl extended column [6]arene WP6:

[0081]

[0082] The second step is to prepare a silver nanowire solution: 90 g of polyvinyl pyrrolidone with a molecular weight of 58,000 is dissolved in 15 mL of 1,2-propylene glycol and transferred to a 25 mL flask, heated in a 170 ° C oil bath and stirred continuously at 450 rpm for 2 hours; 2 mL of sodium chloride dissolved in 1,2-propylene glycol is quickly added, and the sodium chloride concentration is 1 mM. After stirring at 450 rpm for 10 minutes, 5 mL of 0.15 M silver nitrate 1,2-propylene glycol solution is added dropwise with a syringe pump, and then heated at 450 rpm and stirred for 60 minutes to obtain a silvery white AgNWs crude solution. The centrifuge speed is controlled to 7500 rpm, and the AgNWs crude solution is centrifuged and washed with ultrapure water using a centrifuge to obtain pure Ag nanowires, and the pure Ag NWs are dispersed in 25 mL of ultrapure water for subsequent storage and use;

[0083] Step 3: Preparation of gold and silver nanowire solution: 3 mL of 20 mM sodium hydroxide aqueous solution, 120 μL of 25.4 mM chloroauric acid aqueous solution and 19 mL of ultrapure water were added to the reactor, and stirred at 500 rpm for 2 hours at room temperature to obtain a mixed solution A; 50 mg of PVP was added to 5 mL of ultrapure water and heated at 60 ° C to obtain a solution B; 2 minutes later, 600 μL of 100 mM ascorbic acid AA and 600 μL of 200 mM sodium hydroxide were added to the B solution, and after stirring at 500 rpm for 5 minutes, 800 μL of the AgNWs solution prepared in the second step was added to the B solution to obtain a mixed solution C; after rapid stirring at 800 rpm for 10 minutes, the mixed solution A was dripped drop by drop into the mixed solution C at a speed of one drop per 3 seconds, and continued to heat and stir at 800 rpm for 20 minutes until the dripping was completed, and then the reaction was stopped to obtain a crude AuAg NWs solution, and the AuAg was centrifuged and washed with ultrapure water at 7500 rpm. The NWs crude solution was used to obtain pure AuAg NWs, and the product was dispersed in 8 mL of ultrapure water for subsequent use;

[0084] The fourth step was to prepare AuAg@WP6 NWs by ultrasonic method: 0.2 mL of AuAg NWs synthesized in the third step was taken, 1 mL of ultrapure water was added, and 1.5 mg of WP6 was added and ultrasonicated for 2 h to prepare AuAg@WP6 NWs;

[0085] The fifth step is to prepare reduced graphene oxide by graphene oxide: 20 mg of graphene oxide GO and 15 mL of ultrapure water are added to a flask and dispersed by ultrasonication for 2 hours to obtain a GO dispersion, the GO dispersion is added to a reactor, and 50 mL of ethanol is added, the pH of the mixed solution is adjusted with a 1 M potassium hydroxide aqueous solution and the pH value is detected with a pH test paper, when the pH of the dispersion reaches 9.0-10.0, the reactor is placed in an oven and heated at 85 ° C for two hours to obtain a product rGO precipitate, the black precipitate is ultrasonically dispersed and centrifuged and washed with deionized water to obtain a pure rGO dispersion, and dispersed in 20-25 mL of ultrapure water to obtain 0.6 mg mL -1 rGO dispersion;

[0086] Step 6: Prepare reduced graphene oxide-carbon nitride rGO-C3N4 by compounding graphene-like π-conjugated structure with graphene: 5 mg of graphene-carbon nitride g-C3N4 was dissolved in 2 mL of isopropanol and stirred at 450 rpm to obtain 2.5 mg mL -1 g-C3N4 suspension; 0.03mL g-C3N4 suspension and 0.5mL rGO dispersion were mixed and stirred at 450rpm to obtain rGO-C3N4 composite suspension;

[0087] In the seventh step, 10 μL of the rGO-C3N4 solution prepared in the sixth step was dropped on the surface of the glassy carbon electrode polished smooth with alumina and dried at 50°C. Then 10 μL of the AuAg@WP6 NWs solution prepared in the fourth step was dropped on the electrode surface and dried at 50°C to obtain the AuAg@WP6 / rGO-C3N4 composite photoelectric material for subsequent use.

[0088] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a functionalized gold-silver nano alloy wire composite photoelectric material, characterized in that: The specific steps are as follows: Step 1: Preparation of anionic water-soluble [2]biphenyl extended column [6]arene WP6; The second step is to prepare a silver nanowire solution: 85-90g of polyvinyl pyrrolidone with a molecular weight of 58,000 is dissolved in 5-15mL of 1,2-propylene glycol, and the solution is transferred to a 25mL flask, heated in an oil bath at 150-170°C and continuously stirred at 450rpm for 1-2 hours; 1-2mL of sodium chloride dissolved in 1,2-propylene glycol is quickly added, and the sodium chloride concentration is 1mM. After stirring at 450rpm for 5-10 minutes, 3-5mL of 0.15M silver nitrate 1,2-propylene glycol solution is added dropwise with a syringe pump, and then heated at 450rpm for 30-60 minutes to obtain a silvery white AgNWs crude solution, the centrifuge speed is controlled to 6500-7500rpm, and the Ag NWs crude solution is centrifuged and washed with ultrapure water using a centrifuge to obtain pure Ag nanowires, and the pure Ag NWs are dispersed in 20-25mL of ultrapure water for subsequent storage and use; Step 3: Prepare the gold-silver nanowire solution: add 2-3 mL of 20 mM sodium hydroxide aqueous solution, 100-120 μL of 25.4 mM chloroauric acid aqueous solution and 17-19 mL of ultrapure water into the reactor, and stir at 500 rpm for 1-2 hours at room temperature to obtain a mixed solution A; add 40-50 mg of PVP to 3-5 mL of ultrapure water and heat at 60°C to obtain a solution B; after 2 minutes, add 500-600 μL of 100 mM anti- Ascorbic acid AA and 500-600 μL of 200 mM sodium hydroxide were added to solution B. After stirring at 500 rpm for 5 minutes, 700-800 μL of the AgNWs solution prepared in the second step was added to solution B to obtain a mixed solution C. After rapid stirring at 800 rpm for 10 minutes, the mixed solution A was dripped into the mixed solution C drop by drop at a rate of one drop per 3 seconds until the dripping was completed. After heating and stirring at 800 rpm for 10-20 minutes, the reaction was stopped to obtain a crude AuAg NWs solution. The crude AuAg NWs solution was centrifugally washed with ultrapure water at 6500-7500 rpm to obtain pure AuAg NWs. The product was dispersed in 7-8 mL of ultrapure water for subsequent use. Step 4: Prepare AuAg@WP6 NWs by ultrasonic method: take 0.1-0.2 mL of AuAg NWs synthesized in step 3, add 0.8-1 mL of ultrapure water, add 1-1.5 mg of WP6 and ultrasonicate for 1-2 hours to prepare AuAg@WP6 NWs; The fifth step is to prepare reduced graphene oxide by graphene oxide: 10-20 mg of graphene oxide GO and 10-15 mL of ultrapure water are added to a flask and dispersed by ultrasonic treatment for 1-2 hours to obtain a GO dispersion, the GO dispersion is added to a reactor, and 45-50 mL of ethanol is added, the pH of the mixed solution is adjusted with a 1 M potassium hydroxide aqueous solution and the pH value is detected with a pH test paper, when the pH of the dispersion reaches 9.0-10.0, the reactor is placed in an oven and heated at 80-85°C for two hours to obtain a product rGO precipitate, the black precipitate is ultrasonically dispersed and centrifuged and washed with deionized water to obtain a pure rGO dispersion, and dispersed in 20-25 mL of ultrapure water to obtain 0.6 mg mL -1 rGO dispersion; Step 6: Prepare reduced graphene oxide-carbon nitride rGO-C3N4 by compounding graphene-like π-conjugated structure with graphene: 5 mg of graphene-carbon nitride g-C3N4 was dissolved in 2 mL of isopropanol and stirred at 450 rpm to obtain 2.5 mg mL -1 g-C3N4 suspension; 0.03mL g-C3N4 suspension and 0.5mL rGO dispersion were mixed and stirred at 450rpm to obtain rGO-C3N4 composite suspension; In the seventh step, 10 μL of the rGO-C3N4 solution prepared in the sixth step was dropped on the surface of the glassy carbon electrode polished smooth with alumina and dried at 50°C. Then 10 μL of the AuAg@WP6 NWs solution prepared in the fourth step was dropped on the electrode surface and dried at 50°C to obtain the AuAg@WP6 / rGO-C3N4 composite photoelectric material for subsequent use.

2. The method for preparing the functionalized gold-silver nano alloy wire composite photoelectric material according to claim 1, characterized in that: The second step of preparing the silver nanowire solution is specifically as follows: S1. Dissolve 87 g of polyvinyl pyrrolidone with a molecular weight of 58,000 in 10 mL of 1,2-propylene glycol and transfer to a 25 mL flask, heat in an oil bath at 160 °C and stir continuously at 450 rpm for 1 hour; S2, quickly add 1 mL of sodium chloride dissolved in 1,2-propylene glycol to a sodium chloride concentration of 1 mM, stir at 450 rpm for 5 minutes, then add 4 mL of 0.15 M silver nitrate 1,2-propylene glycol solution dropwise using a syringe pump, then heat and stir at 450 rpm for 40 minutes to obtain a silvery white Ag NWs crude solution; S3, controlling the centrifuge speed to 7000 rpm, using a centrifuge and ultrapure water to centrifuge and wash the crude Ag NWs solution to obtain pure Ag nanowires; S4. Use 20 mL of ultrapure water to disperse the pure Ag NWs for subsequent storage and use.

3. The method for preparing the functionalized gold-silver nano alloy wire composite photoelectric material according to claim 1, characterized in that: The third step of preparing the gold-silver nanowire solution by ion exchange method specifically comprises the following steps: Step 1: Add 2 mL of 20 mM sodium hydroxide aqueous solution, 100 μL of 25.4 mM chloroauric acid aqueous solution and 17.9 mL of ultrapure water into a reaction kettle, and stir at 500 rpm for 1 hour at room temperature to obtain a mixed solution A; Step 2: Add 40 mg of PVP to 3 mL of ultrapure water and heat at 60°C to obtain solution B; Step 3: After 2 minutes, 500 μL of 100 mM ascorbic acid AA and 500 μL of 200 mM sodium hydroxide were added to solution B. After stirring at 500 rpm for 5 minutes, 700 μL of the AgNWs solution prepared in the second step was added to solution B to obtain a mixed solution C. After rapid stirring at 800 rpm for 10 minutes, the mixed solution A was dripped into the mixed solution C drop by drop at a speed of one drop per 3 seconds. After the dripping was completed, the mixture was heated and stirred at 800 rpm for 10 minutes, and then the reaction was stopped to obtain a crude AuAg NWs solution. Step 4: Wash the crude AuAg NWs solution with ultrapure water by centrifugation at 7000 rpm for several times to obtain pure AuAg NWs, and disperse the product in 7 mL ultrapure water for subsequent use.

4. The method for preparing the functionalized gold-silver nano alloy wire composite photoelectric material according to claim 1, characterized in that: In the first step, anionic water-soluble [2]biphenyl extended column [6]arene WP6 is prepared, and the process route is as follows:

5. The method for preparing the functionalized gold-silver nano alloy wire composite photoelectric material according to claim 1, characterized in that: In the fourth step, 0.14 mL of AuAgNWs synthesized in the third step was taken, 0.86 mL of ultrapure water was added, and 1.26 mg of WP6 was added for ultrasonication for 1.5 hours to prepare AuAg@WP6 NWs.

6. The method for preparing the functionalized gold-silver nano alloy wire composite photoelectric material according to claim 1, characterized in that: The fifth step of preparing reduced graphene oxide by graphene oxide is specifically as follows: Step a: 14 mg of graphene oxide GO and 10 mL of ultrapure water were added into a flask and dispersed by ultrasonication for 2 hours to obtain a GO dispersion; Step b: Add the GO dispersion into the reactor, add 46 mL of ethanol, adjust the pH of the mixed solution with a 1 M potassium hydroxide aqueous solution, and detect the pH value with a pH test paper. When the pH of the dispersion reaches 9.0-10.0, place the reactor in an oven and heat at 80°C for two hours to obtain the product rGO precipitate; Step c: Ultrasonic dispersion of black precipitate was performed and washed with centrifugal centrifuge and deionized water to obtain pure rGO dispersion, which was then dispersed in 23 mL of ultrapure water to obtain 0.6 mg mL -1 of rGO dispersion.

7. A functionalized gold-silver nano alloy wire composite optoelectronic material prepared by the preparation method according to any one of claims 1 to 6.

8. An application of the composite photoelectric material according to claim 7 in a novel signal switch type photoelectrochemical (PEC) sensing system, characterized in that: The surface area is 0.07 cm 2 10 μL rGO-C3N4 composite photoelectric material solution was drop-coated on the glassy carbon electrode and dried at 50 °C. Then, 10 μL AuAg@WP6 NWs composite photoelectric material solution was drop-coated on the electrode surface and dried at 50 °C to prepare AuAg@WP6 / rGO-C3N4 / GCE nanocomposite electrode.

9. An application of the composite photoelectric material according to claim 8 in a novel signal switch type photoelectrochemical (PEC) sensing system, characterized in that: The new signal switch type photoelectrochemical PEC sensing system uses the traditional three-electrode system to AuAg@WP6 / rGO-C3N4 / GCE nanocomposite electrode was used as the working electrode, platinum mesh was used as the counter electrode, and saturated calomel electrode SCE was used as the reference electrode. A xenon lamp was used to simulate a visible light source to irradiate the surface of AuAg@WP6 / rGO-C3N4 / GCE, and the shading interval time was controlled as an adjustable "on-off". Then, an electrochemical workstation was used for photoelectrochemical detection in a phosphate buffer solution containing serotonin.

Citation Information

Patent Citations

  • Preparation method of nitrogen-doped reduced graphene-AuAg double-metal nano compound and application of nitrogen-doped reduced graphene-AuAg double-metal nano compound to electrochemical detection of daunorubicin hydrochloride

    CN105606676A

  • Graphene-loaded multi-metal nanowire aerogel composite material and preparation method thereof

    CN110639516A

  • AuAg-coated WP5 / RGO-C3N4 composite material as well as preparation method and application thereof

    CN114235917A

  • Ion selective electrode using light responsive calix arene derivative

    JP1994201639A

  • Reduced graphene oxide-silver nanocomposite films for temperature sensor application