Flexible giant magneto-impedance (GMI) effect magnetic sensor and preparation method thereof
Through the design of flexible giant magnetic impedance GMI effect magnetic sensor, the Wheatstone bridge structure and multi-layer magnetic material are used to solve the sensitivity and resolution of existing magnetic field sensors in high-frequency environments, and realize the high-frequency environment. Effective magnetic field sensing and efficiency improvement.
Patent Information
- Application Number
- CN202410812856.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-22
- Publication Date
- 2024-11-29
AI Technical Summary
Existing magnetic field sensors have small magnetic field range and low resolution, and most of them are only suitable for low-frequency conditions, making it difficult to apply to high-frequency environments.
Using flexible giant magnetoresistive GMI effect magnetic sensor, Wheatstone bridge structure and multi-layer magnetic materials, including the underlying buffer layer, magnetic material layer, magnetic material isolation layer and conductive intermediate layer, prepared by photolithography and magnetron sputtering technology , uses the GMI effect to achieve high-frequency magnetic field sensing.
It improves the sensitivity and working efficiency of the magnetic sensor, can work effectively in high-frequency environments, and the output voltage is 0 when the applied magnetic field is 0, expanding the application range.
Smart Images

Figure CN119044845A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of magnetic field sensors, and in particular relates to a flexible giant magneto-impedance (GMI) effect magnetic sensor and a preparation method thereof. Background Art
[0002] With the rapid development of the Internet of Things, wearable and implantable technologies, flexible electronic products have attracted much attention.
[0003] Flexible electronic components enable electronic devices to be reshaped as needed after preparation. Flexible magnetic sensors can convert changes in magnetic properties caused by external factors into electrical signals, thereby detecting the existence, strength, direction and changes of magnetic fields. They are widely used in intelligent robots, health care, electronic skin (E-Skins), human-computer interaction and other fields. The research on flexible magnetic sensors has gradually become an important research direction worldwide.
[0004] Most of the existing magnetic field sensors are based on magnetoresistance effect. The test magnetic field range of such magnetic sensors is relatively small, about 0.1-10 2 Oe, and the resolution is relatively low, about 0.1Oe. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a flexible giant magneto-impedance (GMI) effect magnetic sensor.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a flexible giant magneto-impedance (GMI) effect magnetic sensor, comprising:
[0009] substrate;
[0010] Wheatstone bridge structure magnetic strip;
[0011] and conductive electrodes connected to a Wheatstone bridge structure;
[0012] The Wheatstone bridge structure magnetic strip is a sandwich structure, which includes a bottom buffer layer, a magnetic material layer, a magnetic material isolation layer, and an intermediate layer.
[0013] As a preferred solution of the magnetic sensor of the present invention, the material of the bottom buffer layer includes Ta, and the thickness is 5 nm.
[0014] As a preferred solution of the magnetic sensor of the present invention, the magnetic material of the magnetic material layer includes NiFe, CoFeB and FeCoSiB, and the thickness is 100 nm.
[0015] As a preferred solution of the magnetic sensor of the present invention, wherein: the magnetic material isolation material of the magnetic material isolation layer is Ti, and the thickness is 6 nm.
[0016] As a preferred solution of the magnetic sensor of the present invention, the intermediate layer is a conductive material including Cu, Au or Pt, and has a thickness of 400 nm.
[0017] As a preferred solution of the magnetic sensor of the present invention, the deposition thickness of the magnetic material is 1200-1300 nm.
[0018] Another object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a flexible giant magneto-impedance (GMI) effect magnetic sensor, comprising:
[0019] Forming a first predefined pattern on the Kapton substrate using photolithography and etching techniques;
[0020] The magnetoresistive material is deposited by magnetron sputtering thin film growth technology to form a magnetic strip with a Wheatstone bridge structure;
[0021] forming a second predefined pattern on the substrate by using photolithography and etching technology;
[0022] Growing conductive electrodes using magnetron sputtering thin film growth technology;
[0023] Use acetone ultrasonic cleaning to remove excess conductive metal film.
[0024] As a preferred solution of the method for preparing the magnetic sensor of the present invention, the method for preparing the first predefined pattern includes:
[0025] Spin coating a covering photoresist on the Kapton substrate to form a first photoresist layer;
[0026] Expose the first photoresist layer to ultraviolet light through a mask of a first predefined pattern;
[0027] The exposed first photoresist layer is developed with a developer to remove excess photoresist and leave a first predefined pattern on the Kapton substrate.
[0028] As a preferred solution of the method for preparing the magnetic sensor of the present invention, the method for preparing the second predefined pattern includes:
[0029] Spin-coating a covering photoresist on the Kapton substrate on which the first predefined pattern magnetic material layer is deposited to form a second photoresist layer;
[0030] Expose the second photoresist layer to ultraviolet light through a mask of a second predefined pattern;
[0031] The exposed second photoresist layer is developed using a developing solution.
[0032] Beneficial effects of the present invention:
[0033] (1) The present invention provides a flexible magnetic sensor structure based on the GMI effect and a method for preparing the same to meet the development of flexible electronic devices and solve the problem of low sensor sensitivity due to a low MR ratio.
[0034] (2) Compared with the existing technology, most of the existing magnetic field sensors are based on the anisotropic magnetoresistance (AMR) effect. Such sensors can only be used in low-frequency conditions. Magnetic sensors based on the GMI effect can be used in high-frequency working environments. At the same time, due to the application of the Wheatstone bridge, when the external magnetic field is 0, the output voltage is 0, which effectively improves the working efficiency and application range of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0036] Figure 1 This is a schematic diagram of the sensor structure in Example 1 of the present invention.
[0037] Figure 2 This is a structural diagram of the magnetic strip material of the Wheatstone bridge structure in Example 1 of the present invention.
[0038] Figure 3 This is a flow chart of the preparation of the GMI sensor in Example 1 of the present invention.
[0039] Figure 4 This is a performance test result diagram of the GMI sensor in Example 1 of the present invention.
[0040] Figure 5 1 is an equivalent circuit diagram of a full-bridge structure of a Wheatstone bridge in an embodiment of the present invention. DETAILED DESCRIPTION
[0041] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0042] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0043] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0044] The magnetic sensor based on the GMI effect of the present invention can be applied to high-frequency working environments. At the same time, due to the application of the Wheatstone bridge, when the external magnetic field is 0, the output voltage is 0, which effectively improves the working efficiency and application range of the device. The specific working principle is as follows:
[0045] Figure 5 It is an equivalent circuit of the full-bridge structure of the Wheatstone bridge, where R1, R2, R3 and R4 are four variable resistors, where R1 and R3 have the same adjustment amount, R2 and R4 have the same adjustment amount, and R1 / R3 and R2 / R4 have opposite adjustment amounts, that is, under the same conditions, if the resistance of R1 / R3 decreases by ΔR, the resistance of R2 / R4 increases by ΔR;
[0046] When the adjustment amount is 0, R1=R2=R3=R4=R 0 , then under certain conditions, if R1 / R3 decreases by ΔR, recorded as R1 / R3=R-ΔR; then R2 / R4 increases by ΔR, recorded as R2 / R4=R+ΔR;
[0047] At this time, the total resistance of the two branches is R1+R2=R3+R4=2R;
[0048] In this case, V out+ With V out- The differential output voltage value between V out It can be calculated from the above formula, which is V CC *ΔR / R 0 ;
[0049] For the magnetic field sensor using the Wheatstone bridge, when the external magnetic field is zero, the change ΔR of the four sensing units is also zero, and the differential output voltage is zero at this time.
[0050] Features of the Wheatstone bridge full-bridge structure used in the GMI sensor unit of the present invention:
[0051] ① For the changes in the GMI sensing unit caused by magnetic factors, the above principle shows that the total impedance on the entire branch is a constant, which is conducive to obtaining better linear response characteristics;
[0052] ② For the changes of GMI sensor units caused by non-magnetic factors, such as temperature, the impedance of the sensor unit changes. Since the four GMI sensor units have different sensitive directions, the changes of other characteristics are consistent. That is to say, even if the total impedance of the entire branch changes, it is still a constant, which enhances the stability of the GMI sensor to a certain extent.
[0053] ③ There are three types of Wheatstone bridge structures. The full-bridge structure is used in the present invention, and its output response is In addition, there is a half-bridge structure, that is, R1 = R3 = R 0 , R2=R4=R 0 +ΔR, where only R2 and R4 are changing, the output response is The last type is a single sensor arm, that is, R1 = R3 = R4 = R 0 , R2=R 0 +ΔR, then the output response is
[0054]
[0055] By comparing the three bridge structures, it can be seen that the output of the half-bridge structure is approximately twice that of the single sensor unit, and the output of the full-bridge structure is approximately twice that of the half-bridge structure. Therefore, the full-bridge output used in the present invention can effectively improve the sensitivity of the sensor. Note: The above description is only to illustrate the principle. The actual change value of GMI is the impedance value, not the resistance value.
[0056] Example 1
[0057] This embodiment provides a new type of GMI sensor structure. The schematic diagram of the sensor structure is shown in Figure 1 , including a substrate 100; a Wheatstone bridge structure magnetic strip 200; and a conductive electrode 300 connected to the Wheatstone bridge structure; specifically, by introducing the Wheatstone bridge, when the external magnetic field is 0, the output voltage is 0, which effectively improves the working efficiency and application range of the device.
[0058] Furthermore, the Wheatstone bridge structure magnetic strip material structure is as follows Figure 2As shown, the Wheatstone bridge structure magnetic strip 200 is a sandwich structure, and is provided with a bottom buffer layer 201 , a magnetic material layer 202 , a magnetic material isolation layer 203 , and an intermediate layer 204 .
[0059] The material of the bottom buffer layer 201 includes Ta, with a thickness of 5nm; the magnetic material of the magnetic material layer 202 includes NiFe, CoFeB and FeCoSiB, which are divided into three layers, and each layer is 100nm thick; the magnetic material isolation material of the magnetic material isolation layer 203 is Ti, which is divided into three layers with a thickness of 6nm; the intermediate layer 204 is a conductive material, including Cu, Au or Pt, with a thickness of 400nm.
[0060] The magnetic sensor based on the GMI effect, due to the application of the Wheatstone bridge, has an output voltage of 0 when the external magnetic field is 0, which effectively improves the working efficiency and application range of the device.
[0061] Example 2
[0062] See also Figure 3 , introduces the preparation method of the GMI sensor in the present invention:
[0063] Step 1: Provide a Kapton substrate and ultrasonically clean it with acetone, alcohol and deionized water for 5 min respectively, then use N 2 Blow dry and bake in an oven at 115°C for 20 minutes.
[0064] Step 2: The photoresist model used is AR-P 3510T. After dropping the photoresist on the Kapton substrate, rotate it on a spreader at a speed of 600 r / min for 10 seconds to allow the photoresist to cover the Kapton sheet, and then rotate it at a speed of 4000 r / min for 40 seconds to make the photoresist thickness uniform.
[0065] Step 3: Place the Kapton substrate with the spin-coated photoresist into an oven and heat it at 115° C. for 20 minutes to completely cure the photoresist.
[0066] Step 4: exposing the first photoresist layer to ultraviolet light through a mask of a first predefined pattern;
[0067] The device of the present invention is prepared on a 4-inch Kapton, and the mask is a 5-inch mask with a chrome surface;
[0068] The method for preparing the sensor of the present invention, although the present solution features the design of a Wheatstone full-bridge structure, the mask pattern design and the like are not limited to the Wheatstone full-bridge structure.
[0069] Step 5: Development to remove excess photoresist and leave a first predefined pattern on the Kapton substrate.
[0070] Step 6: Using magnetron sputtering thin film growth technology, grow a magnetoresistive film layer on the treated substrate, the total thickness of the magnetoresistive film layer is 800nm, and the magnetic material is NiFe, CoFeB, FeCoSiB. The thickness of NiFe, CoFeB, FeCoSiB can be changed, and it can also be other magnetic materials, and the number and size of the magnetoresistive strips can also be changed;
[0071] The NiFe, CoFeB, and FeCoSiB involved in this embodiment are 2-inch*0.125-inch targets from Kurt J. Lesker.
[0072] Step 7: Remove the first layer of photoresist.
[0073] Step 8: After adding photoresist onto the Kapton substrate with the magnetoresistive layer, the coating machine is rotated at 600 r / min for 10 seconds to allow the photoresist to cover the Kapton sheet, and then rotated at 4000 r / min for 40 seconds to make the thickness of the photoresist uniform.
[0074] Step 9: Place the Kapton substrate with the spin-coated photoresist into an oven and heat it at 115° C. for 20 minutes to completely cure the photoresist.
[0075] Step 10: exposing the second photoresist layer to ultraviolet light through a mask of a second predefined pattern;
[0076] The photolithography machine used was a domestic URE-2000S / 25 double-sided alignment exposure machine. The photoresist used was AR-P 3510P positive photoresist. The spin coating parameters were 600r / min for 10s, then 4000r / min for 40s, and the UV exposure parameters were 6.5s.
[0077] The first predefined pattern of the magnetic material layer includes a magnetoresistive strip of a Wheatstone bridge structure, and the second predefined pattern of the conductive material layer includes conductive electrodes connected to the Wheatstone bridge structure.
[0078] Step 11: Develop to remove excess photoresist and leave a second predefined pattern on the Kapton substrate.
[0079] Step 12: Using magnetron sputtering thin film growth technology to grow a conductive metal layer on the treated substrate;
[0080] The conductive metal layer can be any one or more metal materials with good conductivity such as Ta, Cu, Au, Pt, etc. The total thickness of the conductive metal layer is generally 30nm to 100nm.
[0081] Step 13: Remove the second layer of photoresist. Meanwhile, the above preparation processes are all conventional technical means.
[0082] Example 3
[0083] GMI sensor performance test results:
[0084] A power amplifier is used to drive a pair of small electromagnets;
[0085] Use the AFG3000C arbitrary function generator to output a specific type of signal, which drives the electromagnet after passing through the power amplifier to generate a magnetic field signal with the same waveform change trend;
[0086] The E4990A impedance analyzer was used to test the relationship between the impedance of the sensor and the frequency. The results are shown in Figure 4 .
[0087] It can be seen that for the changes in the GMI sensor unit caused by non-magnetic factors, such as temperature, which causes changes in the impedance of the sensor unit, since the four GMI sensor units have different sensitive directions, the changes in other characteristics are consistent. In other words, even if the total impedance of the entire branch changes, it is still a constant, which enhances the stability of the GMI sensor to a certain extent.
[0088] Compared with the prior art, most of the existing magnetic field sensors are based on the anisotropic magnetoresistance (AMR) effect, and such sensors can only be used in low-frequency conditions. The present invention provides a magnetic sensor based on the GMI effect, which can be used in high-frequency working environments. At the same time, due to the application of the Wheatstone bridge, when the external magnetic field is 0, the output voltage is 0, which effectively improves the working efficiency and application range of the device.
[0089] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A flexible giant magneto-impedance (GMI) effect magnetic sensor. Features: include, Base (100); Wheatstone bridge structure magnetic strip (200); and a conductive electrode (300) connected to a Wheatstone bridge structure; The Wheatstone bridge structure magnetic strip (200) is a sandwich structure, comprising a bottom buffer layer (201), a magnetic material layer (202), a magnetic material isolation layer (203), and an intermediate layer (204).
2. The magnetic sensor according to claim 1, Features: The material of the bottom buffer layer (201) includes Ta and has a thickness of 5 nm.
3. The magnetic sensor according to claim 1 or 2, Features: The magnetic material of the magnetic material layer (202) includes NiFe, CoFeB and FeCoSiB, and has a thickness of 100 nm.
4. The magnetic sensor according to claim 3, Features: The magnetic material isolation material of the magnetic material isolation layer (203) is Ti, and the thickness is 6 nm.
5. The magnetic sensor according to claim 4, Features: The intermediate layer (204) is a conductive material including Cu, Au or Pt, and has a thickness of 400 nm.
6. The magnetic sensor according to claim 4, Features: The deposition thickness of the magnetic material is 1200-1300 nm.
7. A method for preparing a magnetic sensor according to any one of claims 1 to 6, Features: include, Forming a first predefined pattern on the Kapton substrate using photolithography and etching techniques; The magnetoresistive material is deposited by magnetron sputtering thin film growth technology to form a magnetic strip with a Wheatstone bridge structure; forming a second predefined pattern on the substrate by using photolithography and etching technology; Growing conductive electrodes using magnetron sputtering thin film growth technology; Use acetone ultrasonic cleaning to remove excess conductive metal film.
8. The preparation method according to claim 7, Features: The preparation method of the first predefined graph includes: Spin coating a covering photoresist on the Kapton substrate to form a first photoresist layer; Expose the first photoresist layer to ultraviolet light through a mask of a first predefined pattern; The exposed first photoresist layer is developed with a developer to remove excess photoresist and leave a first predefined pattern on the Kapton substrate.
9. The preparation method according to claim 7, Features: The preparation method of the second predefined graph includes: Spin-coating a covering photoresist on the Kapton substrate on which the first predefined pattern magnetic material layer is deposited to form a second photoresist layer; Expose the second photoresist layer to ultraviolet light through a mask of a second predefined pattern; The exposed second photoresist layer is developed using a developing solution.
Citation Information
Cited By
Giant magnetoresistance magnetic sensor and preparation method thereof
CN121692998A