Novel electromagnetic shielding process and inductor manufactured by same

Through the combination of magnetic powder molding and electroplating technology, the problem of limited performance of inductors in the strong electromagnetic environment in the prior art is solved, and the stable operation of inductors in complex environments is achieved and the efficient electromagnetic shielding effect of inductors is achieved.

CN119049863AInactive Publication Date: 2024-11-29ZHUZHOU HONGDA MAG-ELECTRIC TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411251888.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art single shielding method in a strong electromagnetic environment cannot fully meet the needs of inductors, resulting in limited performance.

Method used

The magnetic powder molding process is used to wrap the excitation coil on the inner layer of the magnetic powder, and an electric field shielding layer of nickel and copper is formed on the surface of the inductor. Insulating paint is combined to achieve the combination of magnetic shielding and electric field shielding, ensuring that the inductor is in a complex electromagnetic environment. stable operation.

Benefits of technology

By combining magnetic shielding and electric field shielding, the inductor's anti-electromagnetic interference capability is significantly improved, the circuit reliability is improved, the external electric field and magnetic field interfere with the inductor, and the stable operation of the inductor in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049863A_ABST
    Figure CN119049863A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electronic components, and discloses a novel electromagnetic shielding process which comprises the following steps: step 1, magnetic powder compression molding: firstly, selecting a high-performance magnetic powder material, accurately placing a pre-manufactured excitation coil in a mold, integrally molding the magnetic powder and the coil through a compression molding process, and in the molding process, forming the magnetic powder and the coil into a whole; it is ensured that the coil is completely wrapped in the inner layer of the magnetic powder; and step 2, forming an electric field shielding layer: adopting an electroplating process on the surface of the inductor formed by the magnetic powder. By combining the advantages of magnetic shielding and electric field shielding, an efficient electromagnetic shielding structure is formed, stable operation of the inductor in a complex electromagnetic environment is ensured, through the design of the novel inductor, the anti-electromagnetic interference capability of a circuit can be remarkably improved, the reliability of the whole circuit is improved, and the cost is reduced. And particularly, the method has important application prospects in high-density circuit boards and high-frequency circuits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic components, in particular to a new electromagnetic shielding process and an inductor manufactured therefrom. Background Art

[0002] In modern electronic devices, the performance of inductors directly affects the overall stability and reliability of the circuit. In a complex electromagnetic environment, external electric and magnetic fields can interfere with inductors, and the magnetic field generated inside the inductor may also affect surrounding electronic components. Therefore, effective electromagnetic shielding of inductors is essential.

[0003] 1. Magnetic shielding: The main purpose of magnetic shielding is to isolate useless magnetic forces, including preventing external magnetic fields from entering the inductor and preventing the magnetic field inside the inductor from leaking out. At present, power inductors usually use two magnetic shielding methods: one is to use ferrite materials to surround the internal electrodes of the inductor, and the other is to use resin containing magnetic powder to wrap the winding.

[0004] 2. Electric field shielding: Electric field shielding is to use conductive materials to surround the inductor to prevent the external electric field from affecting the internal circuit of the inductor, or to prevent the electric field inside the inductor from leaking out and affecting the external environment. The principle of electric field shielding is based on the charge distribution characteristics of the conductor. Under the action of the external electric field, the free electrons inside the conductive material will redistribute to form charge rearrangement, thereby offsetting the external electric field and making the electric field strength inside the conductor close to zero.

[0005] Charge rearrangement: When a conductor is exposed to an external electric field, free electrons move under the action of the electric field, forming negative charges that accumulate on the side of the conductor surface facing the electric field, while positive charges accumulate on the opposite side, generating an internal opposing electric field.

[0006] Shielding effect: Due to the antagonistic electric field inside the conductor, the electric field is offset, and the circuits or components inside the conductor are protected from external electric field interference. At the same time, the internal electric field will not leak out and affect the surrounding environment. Summary of the invention

[0007] In view of the deficiencies in the prior art, the present invention provides a new electromagnetic shielding process and an inductor manufactured thereby, which solves the problem that a single shielding method cannot fully meet the demand in a strong electromagnetic environment, resulting in limited performance of the inductor.

[0008] To achieve the above objectives, the present invention is implemented through the following technical solutions: A new electromagnetic shielding process, comprising the following steps:

[0009] Step 1. Magnetic powder molding:

[0010] First, high-performance magnetic powder materials are selected, and the pre-made excitation coil is accurately placed in the mold. The magnetic powder and the coil are formed into one piece through the compression molding process. During the molding process, it is ensured that the coil is completely covered by the inner layer of the magnetic powder.

[0011] Step 2. Formation of electric field shielding layer:

[0012] The surface of the inductor formed by magnetic powder is electroplated with a layer of nickel and copper in sequence. The two layers of metal are closely combined to form a highly efficient electric field shielding layer.

[0013] Step 3. Application of insulation layer:

[0014] In order to ensure reliable electrical isolation between the electric field shielding layer and the external circuit, a layer of insulating paint is evenly sprayed on the surface of the electroplating layer using advanced spraying technology;

[0015] Step 4. Electrode forming:

[0016] At the pin part of the inductor, the insulating paint is stripped off through a process to expose the internal excitation coil end. Then, the surface area of ​​the exposed excitation coil end is electroplated again, with a layer of copper, nickel, and tin plated in sequence to insulate the electric field shielding layer from the inductor electrode.

[0017] Preferably, the compression molding process in step 1 comprises the following specific steps:

[0018] 1) Preparation:

[0019] Clean the mold to ensure that there are no impurities and oil stains inside the mold, and check the magnetic powder and pre-made coils to ensure that their quality and size meet the requirements;

[0020] 2) Loading and mold closing:

[0021] Pour the magnetic powder evenly into the mold cavity, place the pre-made coil accurately at the predetermined position in the mold cavity, ensure that the coil is completely surrounded by the magnetic powder, and slowly close the mold;

[0022] 3) Apply pressure and heat:

[0023] The pressure is set at 180-250 MPa through the pressure equipment to gradually apply pressure to the mold and maintain it for a certain time, so that the magnetic powder can fully fill the mold cavity and tightly combine with the coil, and the magnetic powder forms a magnet. Then the heating device is started to heat the mold to 150-180°C and maintain the temperature for a certain time;

[0024] 4) Pressure-keeping and heat-insulating molding and demoulding:

[0025] After reaching the set pressure and temperature, the pressure and temperature are maintained for a period of time, and then the heating is stopped, and the mold and the molded part are gradually cooled to room temperature by natural cooling or forced cooling. When the mold and the molded part are cooled to room temperature, the mold is opened and the molded inductor blank is taken out;

[0026] 5) Post-processing:

[0027] After demoulding, the inductor blank is cleaned, trimmed and inspected as necessary to remove flash and burr defects.

[0028] Preferably, in the electroplating process of step 2, the surface of the inductor is first cleaned to remove oil, oxides and other impurities, and the surface is activated by chemical cleaning, pickling or mechanical polishing. Then, the electroplating solution is poured into a container, and the pretreated inductor is mounted on a special hanger or fixture so that the inductor contacts the electrode and is connected to a DC power supply. Under the action of the current, the metal ions undergo a reduction reaction on the surface of the inductor to form a plating layer.

[0029] Preferably, in the step 2, the thickness of the nickel plating is 10-20 μm, and the thickness of the copper plating is 20-30 μm.

[0030] Preferably, during the electroplating treatment in step 4, the thickness of the copper plating is 10 to 15 μm, the thickness of the nickel plating is 5 to 10 μm, and the thickness of the tin plating is 8 to 12 μm.

[0031] Preferably, the magnetic powder is a mixture of ferrite magnetic powder and carbonyl iron powder in a certain ratio, and the mixing ratio is 1:(0.5-2).

[0032] A new electromagnetic shielding inductor comprises an excitation coil, an insulating paint, an electric field shielding layer and a magnet.

[0033] The present invention provides a new electromagnetic shielding process and an inductor produced therefrom. It has the following beneficial effects:

[0034] 1. The present invention combines the advantages of magnetic shielding and electric field shielding to form an efficient electromagnetic shielding structure, ensuring the stable operation of the inductor in a complex electromagnetic environment. The design of this new inductor can significantly improve the circuit's anti-electromagnetic interference capability and the reliability of the overall circuit, especially in high-density circuit boards and high-frequency circuit applications.

[0035] 2. The present invention combines magnetic shielding with electric field shielding to effectively prevent external electric and magnetic fields from interfering with the inductor, thereby ensuring the stable operation of the inductor in a complex electromagnetic environment. At the same time, it prevents the magnetic field generated inside the inductor from interfering with surrounding sensitive components, making the electric field strength inside the conductor close to zero. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A schematic diagram of a novel electromagnetic shielding inductor of the present invention;

[0037] Figure 2 The figure is a schematic diagram of a process of a new electromagnetic shielding process of the present invention. DETAILED DESCRIPTION

[0038] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example:

[0040] Please see attached Figure 1 -Attached Figure 2 , an embodiment of the present invention provides a new electromagnetic shielding process, comprising the following steps:

[0041] Step 1. Magnetic powder molding:

[0042] First, high-performance magnetic powder materials are selected, and the pre-made excitation coil is accurately placed in the mold. The magnetic powder and the coil are formed into one piece through the compression molding process. During the molding process, it is ensured that the coil is completely covered by the inner layer of the magnetic powder. The magnetic powder not only acts as a magnetic core, but also as an efficient magnetic shielding layer, which can effectively shield the external magnetic field and prevent the internal magnetic field from leaking out, thereby significantly improving the electromagnetic shielding performance of the inductor.

[0043] Step 2. Formation of electric field shielding layer:

[0044] The surface of the inductor formed by magnetic powder is electroplated with a layer of nickel and copper in turn. The two layers of metal are closely combined to form a highly efficient electric field shielding layer, which can effectively shield the interference of the external electric field and prevent the internal electric field from leaking outward, further enhancing the electromagnetic shielding effect of the inductor.

[0045] Step 3. Application of insulation layer:

[0046] In order to ensure reliable electrical isolation between the electric field shielding layer and the external circuit, a layer of insulating paint is evenly sprayed on the surface of the electroplating layer using advanced spraying technology. This insulating layer not only provides the necessary electrical isolation, but also significantly enhances the inductor's tolerance in various harsh environments, effectively preventing oxidation and corrosion, thereby extending the service life of the inductor.

[0047] Step 4. Electrode forming:

[0048] At the pin part of the inductor, the insulating paint is stripped off through a process to expose the internal excitation coil end. Then, the surface area of ​​the exposed excitation coil end is electroplated again, with a layer of copper, nickel, and tin plated in sequence. The electric field shielding layer is insulated from the inductor electrode. The electrode formed in this way not only has excellent conductive properties, but also can ensure the reliability and stability of the inductor during long-term use, providing a strong guarantee for the normal operation of electronic equipment.

[0049] The compression molding process in step 1 includes the following specific steps:

[0050] 1) Preparation:

[0051] Clean the mold to ensure that there are no impurities and oil stains in the mold to ensure the molding quality. Check the magnetic powder and pre-made coils to ensure that their quality and size meet the requirements;

[0052] 2) Loading and mold closing:

[0053] Pour the magnetic powder evenly into the mold cavity, place the pre-made coil accurately at the predetermined position in the mold cavity, ensure that the coil is completely surrounded by the magnetic powder, slowly close the mold, ensure that the upper and lower molds of the mold are accurately aligned, and the magnetic powder and coil will not be damaged during the mold closing process;

[0054] 3) Apply pressure and heat:

[0055] The pressure is set at 180-250MPa through the pressure equipment to gradually apply pressure to the mold and maintain it for a certain time, so that the magnetic powder can fully fill the mold cavity and tightly combine with the coil, and the magnetic powder forms a magnet. Then the heating device is started to heat the mold to 150-180℃ and maintain the temperature for a certain time to promote the solidification and molding of the magnetic powder;

[0056] 4) Pressure-keeping and heat-insulating molding and demoulding:

[0057] After reaching the set pressure and temperature, maintain the pressure and temperature for a period of time to ensure that the magnetic powder is fully solidified and formed, and to ensure that the performance of the product is uniform and stable. Then stop heating, and use natural cooling or forced cooling to gradually cool the mold and the molded part to room temperature. When the mold and the molded part cool to room temperature, open the mold and take out the formed inductor blank;

[0058] 5) Post-processing:

[0059] After demoulding, the inductor blanks are cleaned, trimmed and inspected as necessary to remove flash and burr defects to ensure product quality.

[0060] In the electroplating process of step 2, the surface of the inductor is first cleaned to remove oil, oxides and other impurities, and the surface is activated by chemical cleaning, pickling or mechanical polishing. Then the electroplating solution is poured into a container, and the pre-treated inductor is mounted on a special hanger or fixture so that the inductor contacts the electrode and is connected to a DC power supply. Under the action of the current, the metal ions undergo a reduction reaction on the surface of the inductor to form a coating.

[0061] In step 2, the thickness of nickel plating is 10-20 μm, and the thickness of copper plating is 20-30 μm.

[0062] During the electroplating treatment in step 4, the thickness of the copper plating is 10-15 μm, the thickness of the nickel plating is 5-10 μm, and the thickness of the tin plating is 8-12 μm.

[0063] The magnetic powder is a mixture of ferrite magnetic powder and carbonyl iron powder in a certain ratio of 1:(0.5-2). The mixed magnetic powder can effectively improve the magnetic permeability and saturation magnetic induction intensity of the inductor.

[0064] A new electromagnetic shielding inductor comprises an excitation coil, an insulating paint, an electric field shielding layer and a magnet.

[0065] The following is an introduction in conjunction with specific embodiments:

[0066] Embodiment 1:

[0067] In the compression molding process, the pressure is set at 180 MPa to gradually apply pressure to the mold, and then the heating device is started to heat the mold to 150°C.

[0068] The thickness of the nickel plating was 10 μm, and the thickness of the copper plating was 20 μm.

[0069] The thickness of the copper plating is 10 μm, the thickness of the nickel plating is 5 μm, and the thickness of the tin plating is 8 μm.

[0070] Ferrite magnetic powder and carbonyl iron powder are mixed in a certain ratio, and the mixing ratio is 1:0.5.

[0071] Embodiment 2:

[0072] In the compression molding process, the pressure is set at 180 MPa to gradually apply pressure to the mold, and then the heating device is started to heat the mold to 165°C.

[0073] The thickness of the nickel plating is 15 μm, and the thickness of the copper plating is 25 μm.

[0074] The thickness of the copper plating is 13 μm, the thickness of the nickel plating is 7 μm, and the thickness of the tin plating is 10 μm.

[0075] Ferrite magnetic powder and carbonyl iron powder are mixed in a certain proportion, and the mixing ratio is 1:1.

[0076] Embodiment three:

[0077] In the compression molding process, the pressure is set at 250 MPa to gradually apply pressure to the mold, and then the heating device is started to heat the mold to 180°C.

[0078] The thickness of the nickel plating is 20 μm, and the thickness of the copper plating is 30 μm.

[0079] The thickness of the copper plating is 15 μm, the thickness of the nickel plating is 10 μm, and the thickness of the tin plating is 12 μm.

[0080] Ferrite magnetic powder and carbonyl iron powder are mixed in a certain proportion, and the mixing ratio is 1:2.

[0081] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A new electromagnetic shielding process, characterized in that: The following steps are involved: Step 1. Magnetic powder molding: First, high-performance magnetic powder materials are selected, and the pre-made excitation coil is placed in the mold. The magnetic powder and the coil are formed into one piece through the compression molding process. During the molding process, it is ensured that the coil is completely covered by the inner layer of the magnetic powder. Step 2. Formation of electric field shielding layer: On the surface of the inductor formed by magnetic powder, a layer of nickel and copper are plated in sequence by electroplating process. These two layers of metal are closely combined to form an electric field shielding layer. Step 3. Application of insulation layer: In order to ensure electrical isolation between the electric field shielding layer and the external circuit, a layer of insulating paint is evenly sprayed on the surface of the electroplating layer using advanced spraying technology; Step 4. Electrode forming: At the pin part of the inductor, the insulating paint is stripped off through a process to expose the internal excitation coil end. Then, the surface area of ​​the exposed excitation coil end is electroplated again, with a layer of copper, nickel, and tin plated in sequence to insulate the electric field shielding layer from the inductor electrode.

2. A new electromagnetic shielding process according to claim 1, characterized in that: The compression molding process in step 1 includes the following specific steps: 1) Preparation: Clean the mold to ensure that there are no impurities and oil stains inside the mold, and check the magnetic powder and pre-made coils to ensure that their quality and size meet the requirements; 2) Loading and mold closing: Pour the magnetic powder evenly into the mold cavity, place the pre-made coil accurately at the predetermined position in the mold cavity, ensure that the coil is completely surrounded by the magnetic powder, and slowly close the mold; 3) Apply pressure and heat: The pressure is set at 180-250 MPa through the pressure equipment to gradually apply pressure to the mold and maintain it for a certain time, so that the magnetic powder can fully fill the mold cavity and tightly combine with the coil, and the magnetic powder forms a magnet. Then the heating device is started to heat the mold to 150-180°C and maintain the temperature for a certain time; 4) Pressure and heat preservation molding and demoulding: After reaching the set pressure and temperature, the pressure and temperature are maintained for a period of time, and then the heating is stopped, and the mold and the molded part are gradually cooled to room temperature by natural cooling or forced cooling. When the mold and the molded part are cooled to room temperature, the mold is opened and the molded inductor blank is taken out; 5) Post-processing: After demoulding, the inductor blank is cleaned, trimmed and inspected as necessary to remove flash and burr defects.

3. A new electromagnetic shielding process according to claim 1, characterized in that: In the electroplating process of step 2, the surface of the inductor is first cleaned to remove oil, oxides and other impurities, and the surface is activated by chemical cleaning, pickling or mechanical polishing. Then, the electroplating solution is poured into a container, and the pre-treated inductor is mounted on a special hanger or fixture so that the inductor contacts the electrode and is connected to a DC power supply. Under the action of the current, the metal ions undergo a reduction reaction on the surface of the inductor to form a plating layer.

4. A new electromagnetic shielding process according to claim 1, characterized in that: In the step 2, the thickness of the nickel plating is 10-20 μm, and the thickness of the copper plating is 20-30 μm.

5. A new electromagnetic shielding process according to claim 1, characterized in that: During the electroplating treatment in step 4, the thickness of the copper plating is 10-15 μm, the thickness of the nickel plating is 5-10 μm, and the thickness of the tin plating is 8-12 μm.

6. A new electromagnetic shielding process according to claim 1, characterized in that: The magnetic powder is a mixture of ferrite magnetic powder and carbonyl iron powder in a certain ratio, and the mixing ratio is 1: (0.5-2).

7. A new electromagnetic shielding inductor, characterized in that: A new electromagnetic shielding process applied to any one of claims 1-6, wherein the inductor comprises: an excitation coil, an insulating paint, an electric field shielding layer and a magnet.

Citation Information

Patent Citations

  • Power inductor and manufacturing method thereof

    CN103050224A

  • Surface-mounted power inductor and preparation method thereof

    CN114360861A

  • Double-shielding inductor and preparation method and circuit thereof

    CN115188573A

  • Integral type inductor

    CN208637283U

  • Shielded-type inductor

    US20110248814A1