Method for dispersing aluminum powder of anode foil slurry of high-voltage aluminum electrolytic capacitor

By adopting dissolution, ball milling and vacuum treatment methods in the anode foil slurry of aluminum electrolytic capacitors, combined with abnormal coefficient detection, the problems of aluminum powder dispersion and bonding are solved, the performance and production efficiency of the capacitor are improved, and unqualified products are reduced The emergence of

CN119049884AInactive Publication Date: 2024-11-29DONGGUAN AILLEN ELECTRONICS TECH CO LTD

Patent Information

Application Number
CN202411212323.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the preparation of existing aluminum electrolytic capacitor anode foil slurry, it is difficult to achieve uniform dispersion and bonding of aluminum powder, resulting in uneven coating, affecting the performance of the capacitor, and lacking intelligent judgment and fault handling methods, resulting in a large number of unqualified products.

Method used

A method of dispersing aluminum powder of anode foil slurry of high-voltage aluminum electrolytic capacitors is adopted, including dissolving dispersant and binder, uniform ball milling, vacuum bubble removal, combined with detection and calculation of abnormal coefficients, to ensure coating uniformity and fault judgment.

Benefits of technology

It realizes uniform dispersion and good bonding of aluminum powder, improves the capacity and mechanical properties of the anode foil, intelligently judges the coating inhomogeneity, and reduces the generation of unqualified products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049884A_ABST
    Figure CN119049884A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of aluminum electrolytic capacitors, and particularly relates to an aluminum powder dispersing method for anode foil slurry of a high-voltage aluminum electrolytic capacitor, which comprises the following steps: step 1, dissolving a dispersing agent and a binder, step 2, preparing slurry, step 3, ball-milling, and step 4, removing bubbles. The aluminum powder in the coating foil slurry obtained by the preparation method of the anode foil slurry is uniformly dispersed, the bonding performance is good, and the preparation process is simple. The slurry obtained by the aluminum powder dispersion method is uniformly coated on the front and back surfaces of an aluminum foil substrate to form slurry layers, and the slurry layers are dried to obtain the aluminum foil; the coated foil obtained through the coating process is excellent in mechanical performance, aluminum powder particles are evenly distributed, the porosity can be well improved, and the capacity of the anode foil is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum electrolytic capacitors, and in particular relates to an aluminum powder dispersion method for anode foil slurry of a high-voltage aluminum electrolytic capacitor. Background Art

[0002] Aluminum electrolytic capacitors are one of the indispensable components in modern electronic products. They have excellent performance, large capacity, low cost, easy processing, and convenient use. They are widely used in important fields such as mobile phones, televisions, household appliances, power supplies, hybrid devices, and aerospace, military, etc., and play the role of filtering, bypassing, coupling and decoupling in the circuit.

[0003] Nowadays, most of the anode foils of domestic aluminum electrolytic capacitors use traditional etched foils. However, the expansion rate of traditional etched foils has approached the theoretical limit, the growth of the specific capacity of industrially formed foils has almost stagnated, and the corrosion process will produce a large amount of acidic waste liquid containing metal ions. In recent years, additive manufacturing has been introduced to replace chemical etching. This method uses spherical aluminum powder and plain aluminum foil as the main raw materials. By stacking aluminum powder layers on aluminum foil, the surface undulations of the aluminum powder layers are relied on to increase the specific surface area of ​​the anode foil.

[0004] The technology of preparing electrolytic capacitor anode aluminum foil by coating and sintering aluminum powder slurry is in its infancy in China. Among them, the preparation process of aluminum powder slurry is to evenly mix aluminum powder, solvent, dispersant and binder in a certain proportion, and the selection of dispersant and the process design of aluminum powder slurry play a vital role in the subsequent sintering and formation. In this process, the existing technology cannot achieve the problem of ensuring that the aluminum powder is evenly dispersed in the slurry and that the dispersant can be easily removed in the subsequent sintering process; and when the aluminum foil is coated with the slurry layer, it is impossible to intelligently judge the uniformity of the slurry layer coating, which affects the use of the aluminum foil; when the aluminum foil slurry layer is unevenly coated, it is impossible to intelligently and quickly judge the cause of the uneven coating of the aluminum foil slurry layer, resulting in untimely measures and a large number of unqualified aluminum foils. Therefore, it is necessary to find a simple and efficient method that can not only make the aluminum powder dispersed evenly without being damaged, but also be well bonded to the substrate.

[0005] To this end, the present invention provides an aluminum powder dispersion method for high-voltage aluminum electrolytic capacitor anode foil slurry. Summary of the invention

[0006] In order to make up for the deficiencies of the prior art, at least one technical problem raised in the background technology is solved.

[0007] The technical solution adopted by the present invention to solve the technical problem is: a method for dispersing aluminum powder of anode foil slurry of high-voltage aluminum electrolytic capacitor, comprising the following steps:

[0008] Step 1, dissolving the dispersant and the binder: dissolving the binder and the dispersant in an organic solvent to obtain a primary melt;

[0009] Step 2, slurry preparation: mixing the initial melt obtained in step 1 with the spherical aluminum powder, and then adding the same type of organic solvent as in step 1 to form an aluminum powder slurry;

[0010] Step 3, ball milling: placing the aluminum powder slurry obtained in step 2 in a ball milling tank, adding ball milling beads and ball milling to obtain a slurry;

[0011] Step 4, degassing: placing the slurry tank obtained in step 3 in a vacuum box for vacuum treatment to obtain a mixed aluminum powder slurry.

[0012] In step 1, the binder is one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene or phenolic resin. The dispersant is one or more of triethanolamine, polyvinyl alcohol, styrene-butadiene rubber or methyl amyl alcohol.

[0013] In the step 2, the aluminum powder slurry comprises, by mass, 35-45 parts of spherical aluminum powder, 45-55 parts of organic solvent, 1-5 parts of binder, and 1-5 parts of dispersant.

[0014] In step 2, the organic solvent is one or more of ethyl acetate, acetone, NN-dimethylacetamide, N-methylpyrrolidone or acetonitrile.

[0015] The average particle size of the spherical aluminum powder in step 2 is 3-5 μm.

[0016] In step 4, when the vacuum box is evacuated, the vacuum degree is -0.1 MPa; and the pressure holding time is 5 minutes.

[0017] The purity of the spherical aluminum powder is greater than 99.98%.

[0018] The present invention also provides a mixed aluminum powder slurry prepared according to the aluminum powder dispersion method.

[0019] The present invention also provides a method for preparing aluminum foil using the mixed aluminum powder slurry, comprising the following steps:

[0020] Step A, coating: uniformly coating the mixed aluminum powder slurry on both sides of the aluminum foil substrate to form a slurry layer; testing the slurry layer to ensure that the slurry layer is qualified;

[0021] Step B, drying: the aluminum foil with the aluminum slurry layer after coating in step A is placed in a vacuum dryer for drying to obtain a dried coated aluminum foil.

[0022] The present invention also provides an aluminum foil prepared according to the method.

[0023] The present invention also provides an application of the aluminum foil in preparing a capacitor. The capacitor is a high-voltage aluminum electrolytic capacitor.

[0024] The beneficial effects of the present invention are as follows:

[0025] 1. The aluminum powder dispersion method of the anode foil slurry of a high-voltage aluminum electrolytic capacitor described in the present invention, the aluminum powder in the coated foil slurry obtained by the preparation method of the anode foil slurry of the present invention is evenly dispersed, has good bonding performance, and has a simple preparation process. The coated foil obtained by the coating process has excellent mechanical properties and evenly distributed aluminum powder particles, which can well improve the porosity and increase the capacity of the anode foil.

[0026] 2. In the aluminum powder dispersion method of the anode foil slurry of a high-voltage aluminum electrolytic capacitor described in the present invention, when the aluminum foil is coated with a slurry layer, the thickness difference value and the regional thickness difference ratio factors are comprehensively considered to calculate the abnormal coefficient. The abnormal coefficient can be used to intelligently judge the uniformity of the slurry layer coating to avoid the uneven aluminum foil slurry layer affecting the use.

[0027] 3. The aluminum powder dispersion method for anode foil slurry of a high-voltage aluminum electrolytic capacitor described in the present invention obtains the total paint film difference and the regional over-film difference of the detection area when the aluminum foil slurry layer is unevenly coated, and compares the total paint film difference with the regional over-film difference to determine whether the detection area is a normal over-standard area or an abnormal over-standard area; by comparing the total number of all normal over-standard areas with the total number of abnormal over-standard areas, the cause of the uneven coating of the aluminum foil slurry layer is intelligently determined, and timely measures are taken to avoid the occurrence of a large number of unqualified aluminum foils. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention will be further described below in conjunction with the accompanying drawings.

[0029] Figure 1 A method flow chart of a method for dispersing aluminum powder of anode foil slurry of a high-voltage aluminum electrolytic capacitor;

[0030] Figure 2 It is a physical photo of the slurry of Example 1 and Comparative Examples 1, 4 and 7;

[0031] Figure 3 are SEM images of Example 1 at different magnifications;

[0032] Figure 4 is a planar SEM image of the coated foil of Comparative Examples 1-4;

[0033] Figure 5 This is a physical picture of the coated foil and coated aluminum foil of comparative example 1 being bent. DETAILED DESCRIPTION

[0034] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0035] like Figure 1 As shown, a method for dispersing aluminum powder for anode foil slurry of a high-voltage aluminum electrolytic capacitor, and steps for preparing aluminum foil using a mixed aluminum powder slurry prepared by the dispersion method are as follows:

[0036] Step 1, dissolving the dispersant and the binder: dissolving the binder and the dispersant in an organic solvent to obtain a primary melt;

[0037] Step 2, slurry preparation: the initial melt obtained in step 1 is mixed with the spherical aluminum powder, and then the same organic solvent as in step 1 is added, and the mixture is evenly mixed to form an aluminum powder slurry;

[0038] Step 3, stirring: placing the aluminum powder slurry obtained in step 2 in a ball mill, adding ball mill beads and milling evenly to obtain a slurry;

[0039] Step 4, degassing: placing the slurry tank obtained in step 3 in a vacuum box for vacuum treatment to obtain a mixed aluminum powder slurry;

[0040] Step 5, coating, uniformly coating the mixed aluminum powder slurry obtained in step 4 on the front and back sides of the aluminum foil substrate to form a slurry layer; testing the slurry layer to ensure that the slurry layer is qualified, specifically: dividing the front and back sides of the aluminum foil substrate into a number of testing areas, and then dividing each testing area into a number of testing points, and the total number of testing points in each testing area is JD, collecting the paint film thickness value MH of each testing point, and calculating the difference between the paint film thickness data MH of each testing point and the paint film thickness threshold value YMH, and obtaining the thickness difference HCZ by the formula HCZ = |MH-YMH|; the paint film thickness threshold value YMH is an empirical value, which is set by the staff according to experience;

[0041] Compare the paint film difference HCZ at the detection point with the thickness difference threshold YHC; the thickness difference threshold YHC is an empirical value, which is set by the staff based on experience;

[0042] If the paint film difference HCZ of the detection point is greater than or equal to the thickness difference threshold YHC, it indicates that the thickness difference exceeds the standard and the slurry is unevenly applied, and the detection point is marked as an exceeding standard point; the paint film difference HCZ of all exceeding standard points is obtained and summed to obtain the thickness difference value ZHY;

[0043] The number of points exceeding the standard in the detection area is summed up, and then the ratio of the sum to the total number of detection points JD in the detection area is obtained to obtain the thickness difference ratio HB of the detection area; the thickness difference ratios HB of all detection areas are summed up to obtain the regional thickness difference ratio QCB;

[0044] The abnormal coefficient XYC is obtained by the formula XYC=ZHY×a1+QCB×a2, where a1 and a2 are preset proportional coefficients and a1+a2=1, and the abnormal coefficient XYC is compared with the preset abnormal coefficient YZX; the paint film thickness threshold YMH is an empirical value, which is set by the staff according to experience;

[0045] If the abnormal coefficient XYC ≥ the preset abnormal coefficient YZX, it indicates that the thickness distribution of the slurry layer is uneven, and a slurry layer coating unqualified signal is generated; on the contrary, if the abnormal coefficient XYC < the preset abnormal coefficient YZX, a slurry layer coating qualified signal is generated;

[0046] It should be noted that by adding the paint film difference HCZ of each exceeding point in all the test areas, the thickness difference value ZHY of the exceeding point is obtained, which can reflect the specific value of the slurry layer coating difference of the exceeding point; then the ratio of the exceeding points in each test area to the total number of test points JD in the test area is calculated to calculate the proportion of exceeding points in each area, and the proportion of exceeding points is added to obtain the regional thickness difference ratio QCB, which can reflect the degree of exceeding the standard. The abnormal coefficient XYC is calculated by the formula. The larger the abnormal coefficient XYC is, the more uneven the slurry layer coating is. When it exceeds the preset abnormal coefficient YZX, it indicates that the uneven degree of coating of the slurry layer exceeds the standard, and it is judged that the coating of the slurry layer is unqualified and needs to be processed later.

[0047] Based on the unqualified signal of slurry layer smearing, the reasons for uneven slurry layer smearing are analyzed, the paint film difference HCZ of all detection points in the detection area is obtained, and all the paint film difference HCZ of the monitoring point are summed to obtain the total paint film difference ZQH; the paint film difference HCZ of the exceeding points in the detection area is obtained and added to obtain the district excess film difference QCM, and the total paint film difference ZQH is compared with the district excess film difference QCM;

[0048] If the total paint film difference ZQH ≥ the regional excess film difference QCM, it means that the slurry layer in this area is normal and is recorded as the normal excess area;

[0049] If the total paint film difference ZQH is less than the regional excess film difference QCM, it indicates that the slurry layer in this area exceeds the standard abnormally, and it is recorded as an abnormal excess area;

[0050] Obtain the total number of all normal exceeding-standard areas and compare it with the total number of abnormal exceeding-standard areas;

[0051] If the sum of all normal exceeding-standard areas is greater than the sum of abnormal exceeding-standard areas, the coating value of the slurry layer thickness is abnormal, and the coating value needs to be reset and coated again;

[0052] On the contrary, if the sum of the number of all normal exceeding-standard areas is ≤ the sum of the number of abnormal exceeding-standard areas, it indicates that the coating equipment is damaged and needs to be repaired and the coating work should be stopped;

[0053] It should be noted that after obtaining the signal of unqualified slurry layer coating, the reason for uneven slurry layer coating is analyzed, and the total paint film difference ZQH is obtained by obtaining the paint film difference HCZ of all detection points in the detection area and summing them up. The paint film difference HCZ of the exceeding points in the detection area are added and summed to obtain the district exceeding film difference QCM. If the total paint film difference ZQH is less than the district exceeding film difference QCM, it indicates that the slurry layer thickness exceeds the standard and the slurry layer thickness is lower than the paint film thickness threshold YMH in the detection area. Because the area of ​​each detection area itself is not large, if the coating equipment works normally, the coating thickness will exceed the paint film thickness threshold YM. Even if it does not meet the standard of the exceeding point, it will not be too different. At this time, the calculated total paint film difference ZQH should be greater than the district exceeding film difference QCM to be correct. If the result is that the total paint film difference ZQH is less than the district exceeding film difference QCM, it indicates that the coating equipment is faulty and damaged, and the detection area is recorded as an abnormal exceeding standard area; If the total paint film difference ZQH≥the area excess film difference QCM, it indicates that the coating equipment is working normally. The abnormal thickness may be caused by the coating value setting problem. Therefore, normal coating can be achieved by resetting the coating value and coating again. The slurry layer coating in the detection area is normal and is recorded as the normal excess area. In order to avoid the influence of individual parameters, the present invention compares and judges by calculating the total number of all normal excess areas and the total number of all abnormal excess areas. If the total number of all normal excess areas is greater than the total number of abnormal excess areas, the coating value setting of the slurry layer thickness is abnormal, and the coating value needs to be reset and coated again. On the contrary, if the total number of all normal excess areas is less than the total number of abnormal excess areas, it indicates that the coating equipment is damaged and needs to be repaired and the coating work stopped, so that the judgment result of the cause of uneven slurry layer coating is more accurate and is not affected by individual extreme parameters, thereby avoiding the occurrence of a large number of unqualified aluminum foils.

[0054] Step 6, drying, placing the aluminum foil with the aluminum slurry layer after coating in step 5 in a vacuum dryer for drying to obtain a dried coated aluminum foil.

[0055] The aluminum powder slurry in step 2 is composed of 35-45 parts by mass of spherical aluminum powder, 45-55 parts by mass of organic solvent, 1-5 parts by mass of binder, and 1-5 parts by mass of dispersant.

[0056] The average particle size of the spherical aluminum powder in step 2 is 3-5 μm.

[0057] The organic solvent in step 2 is one or more of ethyl acetate, acetone, NN-dimethylacetamide, N-methylpyrrolidone or acetonitrile.

[0058] In step 1, the binder is one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene or phenolic resin; the dispersant is one or more of triethanolamine, polyvinyl alcohol, styrene-butadiene rubber or methyl amyl alcohol.

[0059] In step 4, when the vacuum box is evacuated, the vacuum degree is -0.1 MPa; and the pressure holding time is 5 minutes.

[0060] The purity of the spherical aluminum powder is greater than 99.98%.

[0061] Example 1

[0062] A method for dispersing aluminum powder of anode foil slurry of a high-voltage aluminum electrolytic capacitor comprises the following steps:

[0063] Step 1: Dissolving the dispersant and binder: Dissolve 4 parts of binder polyvinylidene fluoride (brand name: Wu Yu 1000, Dongguan Jiangyu New Materials Co., Ltd.) and 4 parts of dispersant polyvinyl alcohol (PVA-1788, Wuhan Runxingyuan Technology Co., Ltd.) in 25 parts of organic solvent (NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) according to mass parts to obtain a preliminary solution;

[0064] Step 2: Slurry preparation: Mix the initial solution with 40 parts of spherical aluminum powder with an average particle size of 3 μm, and then add 25 parts of the same type of organic solvent as in step 1 (composed of NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) to form an aluminum powder slurry; wherein the composition of the aluminum powder slurry in parts by mass is: 40 parts of spherical aluminum powder, 50 parts of organic solvent, 4 parts of binder, and 4 parts of dispersant.

[0065] Step 3: stirring: placing the aluminum powder slurry obtained in step 2 in a ball mill, adding ball mill beads and milling uniformly;

[0066] Step 4: Degassing: placing the slurry tank obtained in step 3 in a vacuum box with a vacuum degree of -0.1 MPa, and maintaining the pressure for 5 minutes to perform vacuum degassing treatment to obtain a mixed aluminum powder slurry;

[0067] Step 5: coating: the mixed aluminum powder slurry obtained in step 4 is evenly coated on the front and back sides of the aluminum foil substrate, with a coating thickness of 120 μm, to form a slurry layer; the slurry layer is tested to ensure that the slurry layer is qualified;

[0068] Step 6 Drying: The aluminum foil with the aluminum slurry layer after coating in step 5 is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil.

[0069] Embodiment 2:

[0070] A method for dispersing aluminum powder of anode foil slurry of a high-voltage aluminum electrolytic capacitor comprises the following steps:

[0071] Step 1: Dissolving the dispersant and binder: Dissolve 3.5 parts of binder polyvinylidene fluoride (brand name: Wu Yu 1000, Dongguan Jiangyu New Materials Co., Ltd.) and 4.2 parts of dispersant polyvinyl alcohol (PVA-1788, Wuhan Runxingyuan Technology Co., Ltd.) in 26 parts of organic solvent (NN-dimethylacetamide and acetonitrile in a volume ratio of 3:1) according to mass parts to obtain a preliminary solution;

[0072] Step 2: Slurry preparation: Mix the initial solution with 42 parts of spherical aluminum powder with an average particle size of 3 μm, and then add 26 parts of the same type of organic solvent as in step 1 (composed of NN-dimethylacetamide and acetonitrile in a volume ratio of 3:1) to form an aluminum powder slurry; wherein the composition of the aluminum powder slurry in parts by mass is: 42 parts of spherical aluminum powder, 52 parts of organic solvent, 3.5 parts of binder, and 4.2 parts of dispersant.

[0073] Step 3: stirring: placing the aluminum powder slurry obtained in step 2 in a ball mill, adding ball mill beads and milling uniformly;

[0074] Step 4: Degassing: placing the slurry tank obtained in step 3 in a vacuum box with a vacuum degree of -0.1 MPa, and maintaining the pressure for 5 minutes to perform vacuum degassing treatment to obtain a mixed aluminum powder slurry;

[0075] Step 5: coating: the mixed aluminum powder slurry obtained in step 4 is evenly coated on the front and back sides of the aluminum foil substrate, with a coating thickness of 120 μm, to form a slurry layer; the slurry layer is tested to ensure that the slurry layer is qualified;

[0076] Step 6 Drying: The aluminum foil with the aluminum slurry layer after coating in step 5 is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil.

[0077] Comparative Example 1:

[0078] A method for dispersing aluminum powder of anode foil slurry of a high-voltage aluminum electrolytic capacitor comprises the following steps:

[0079] Step 1: Dissolving the dispersant and binder: Dissolve 2 parts of binder polyvinylidene fluoride (brand name: Wu Yu 1000, Dongguan Jiangyu New Materials Co., Ltd.) and 1 part of dispersant polyvinyl alcohol (PVA-1788, Wuhan Runxingyuan Technology Co., Ltd.) in 25 parts of organic solvent (NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) according to mass parts to obtain a preliminary solution;

[0080] Step 2: Slurry preparation: Mix the initial solution with 45 parts of spherical aluminum powder with an average particle size of 5 μm, and then add 25 parts of the same type of organic solvent as in step 1 (composed of NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) to form an aluminum powder slurry; wherein the composition of the aluminum powder slurry in parts by mass is: 45 parts of spherical aluminum powder, 50 parts of organic solvent, 2 parts of binder, and 1 part of dispersant.

[0081] Step 3: stirring: placing the aluminum powder slurry obtained in step 2 in a ball mill, adding ball mill beads and milling uniformly;

[0082] Step 4: Degassing: placing the slurry tank obtained in step 3 in a vacuum box with a vacuum degree of -0.1 MPa, and maintaining the pressure for 5 minutes to perform vacuum degassing treatment to obtain a mixed aluminum powder slurry;

[0083] Step 5: coating: the mixed aluminum powder slurry obtained in step 4 is evenly coated on the front and back sides of the aluminum foil substrate, with a coating thickness of 120 μm, to form a slurry layer; the slurry layer is tested to ensure that the slurry layer is qualified;

[0084] Step 6 Drying: The aluminum foil with the aluminum slurry layer after coating in step 5 is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil.

[0085] Comparative Example 2:

[0086] A method for dispersing aluminum powder of anode foil slurry of a high-voltage aluminum electrolytic capacitor comprises the following steps:

[0087] Step 1: Dissolving the dispersant and binder: Dissolve 2 parts of binder polyvinylidene fluoride (brand name: Wu Yu 1000, Dongguan Jiangyu New Materials Co., Ltd.) and 2 parts of dispersant polyvinyl alcohol (PVA-1788, Wuhan Runxingyuan Technology Co., Ltd.) in 25 parts of organic solvent (NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) according to mass parts to obtain a preliminary solution;

[0088] Step 2: Slurry preparation: Mix the initial solution with 45 parts of spherical aluminum powder with an average particle size of 5 μm, and then add 25 parts of the same type of organic solvent as in step 1 (composed of NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) to form an aluminum powder slurry; wherein the composition of the aluminum powder slurry in parts by mass is: 45 parts of spherical aluminum powder, 50 parts of organic solvent, 2 parts of binder, and 2 parts of dispersant.

[0089] Step 3: stirring: placing the aluminum powder slurry obtained in step 2 in a ball mill, adding ball mill beads and milling uniformly;

[0090] Step 4: Degassing: placing the slurry tank obtained in step 3 in a vacuum box with a vacuum degree of -0.1 MPa, and maintaining the pressure for 5 minutes to perform vacuum degassing treatment to obtain a mixed aluminum powder slurry;

[0091] Step 5: coating: the mixed aluminum powder slurry obtained in step 4 is evenly coated on the front and back sides of the aluminum foil substrate, with a coating thickness of 120 μm, to form a slurry layer; the slurry layer is tested to ensure that the slurry layer is qualified;

[0092] Step 6 Drying: The aluminum foil with the aluminum slurry layer after coating in step 5 is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil.

[0093] Comparative Example 3:

[0094] A method for dispersing aluminum powder of anode foil slurry of a high-voltage aluminum electrolytic capacitor comprises the following steps:

[0095] Step 1: Dissolving the dispersant and binder: Dissolve 6 parts of binder polyvinylidene fluoride (brand name: Wu Yu 1000, Dongguan Jiangyu New Materials Co., Ltd.) and 4 parts of dispersant polyvinyl alcohol (PVA-1788, Wuhan Runxingyuan Technology Co., Ltd.) in 24 parts of organic solvent (NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) according to mass parts to obtain a preliminary solution;

[0096] Step 2: Slurry preparation: Mix the initial solution with 45 parts of spherical aluminum powder with an average particle size of 3 μm, and then add 24 parts of the same type of organic solvent as in step 1 (composed of NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) to form an aluminum powder slurry; wherein the composition of the aluminum powder slurry in parts by mass is: 50 parts of spherical aluminum powder, 48 parts of organic solvent, 6 parts of binder, and 4 parts of dispersant.

[0097] Step 3: stirring: placing the aluminum powder slurry obtained in step 2 in a ball mill, adding ball mill beads and milling uniformly;

[0098] Step 4: Degassing: placing the slurry tank obtained in step 3 in a vacuum box with a vacuum degree of -0.1 MPa, and maintaining the pressure for 5 minutes to perform vacuum degassing treatment to obtain a mixed aluminum powder slurry;

[0099] Step 5: coating: the mixed aluminum powder slurry obtained in step 4 is evenly coated on the front and back sides of the aluminum foil substrate, with a coating thickness of 120 μm, to form a slurry layer; the slurry layer is tested to ensure that the slurry layer is qualified;

[0100] Step 6 Drying: The aluminum foil with the aluminum slurry layer after coating in step 5 is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil.

[0101] Comparative Example 4:

[0102] A method for dispersing aluminum powder of anode foil slurry of a high-voltage aluminum electrolytic capacitor comprises the following steps:

[0103] Step 1: Dissolving the dispersant and binder: Dissolve 4 parts of binder polyvinylidene fluoride (brand name: Wu Yu 1000, Dongguan Jiangyu New Materials Co., Ltd.) and 0.8 parts of dispersant polyvinyl alcohol (PVA-1788, Wuhan Runxingyuan Technology Co., Ltd.) in 23 parts of organic solvent (NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) according to mass parts to obtain a preliminary solution;

[0104] Step 2: Slurry preparation: Mix the initial solution with 40 parts of spherical aluminum powder with an average particle size of 3 μm, and then add 23 parts of the same type of organic solvent as in step 1 (composed of NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) to form an aluminum powder slurry; wherein the composition of the aluminum powder slurry in parts by mass is: 40 parts of spherical aluminum powder, 46 parts of organic solvent, 4 parts of binder, and 0.8 parts of dispersant.

[0105] Step 3: stirring: placing the aluminum powder slurry obtained in step 2 in a ball mill, adding ball mill beads and milling uniformly;

[0106] Step 4: Degassing: placing the slurry tank obtained in step 3 in a vacuum box with a vacuum degree of -0.1 MPa, and maintaining the pressure for 5 minutes to perform vacuum degassing treatment to obtain a mixed aluminum powder slurry;

[0107] Step 5: coating: the mixed aluminum powder slurry obtained in step 4 is evenly coated on the front and back sides of the aluminum foil substrate, with a coating thickness of 120 μm, to form a slurry layer; the slurry layer is tested to ensure that the slurry layer is qualified;

[0108] Step 6 Drying: The aluminum foil with the aluminum slurry layer after coating in step 5 is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil.

[0109] Comparative Example 5:

[0110] A method for dispersing aluminum powder of anode foil slurry of a high-voltage aluminum electrolytic capacitor comprises the following steps:

[0111] Step 1: Dissolving the dispersant and binder: Dissolve 2 parts of binder polyvinylidene fluoride (brand name: Wu Yu 1000, Dongguan Jiangyu New Materials Co., Ltd.) and 5 parts of dispersant polyvinyl alcohol (PVA-1788, Wuhan Runxingyuan Technology Co., Ltd.) in 25 parts of organic solvent (NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) according to mass parts to obtain a preliminary solution;

[0112] Step 2: Slurry preparation: Mix the initial solution with 45 parts of spherical aluminum powder with an average particle size of 5 μm, and then add 25 parts of the same type of organic solvent as in step 1 (composed of NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) to form an aluminum powder slurry; wherein the composition of the aluminum powder slurry in parts by mass is: 45 parts of spherical aluminum powder, 50 parts of organic solvent, 2 parts of binder, and 5 parts of dispersant.

[0113] Step 3: stirring: placing the aluminum powder slurry obtained in step 2 in a ball mill, adding ball mill beads and milling uniformly;

[0114] Step 4: Degassing: placing the slurry tank obtained in step 3 in a vacuum box with a vacuum degree of -0.1 MPa, and maintaining the pressure for 5 minutes to perform vacuum degassing treatment to obtain a mixed aluminum powder slurry;

[0115] Step 5: coating: the mixed aluminum powder slurry obtained in step 4 is evenly coated on the front and back sides of the aluminum foil substrate, with a coating thickness of 120 μm, to form a slurry layer; the slurry layer is tested to ensure that the slurry layer is qualified;

[0116] Step 6 Drying: The aluminum foil with the aluminum slurry layer after coating in step 5 is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil.

[0117] Comparative Example 6:

[0118] A method for dispersing aluminum powder of anode foil slurry of a high-voltage aluminum electrolytic capacitor comprises the following steps:

[0119] Step 1: Dissolving the dispersant and the binder: Dissolve 2 parts of the binder polyvinylidene fluoride (brand name: Wu Yu 1000, Dongguan Jiangyu New Materials Co., Ltd.) and 1 part of the dispersant styrene butadiene rubber in 25 parts of the organic solvent NN-dimethylacetamide according to mass fraction to obtain a preliminary solution;

[0120] Step 2: Slurry preparation: Mix the initial solution with 45 parts of spherical aluminum powder with an average particle size of 5 μm, and then add 25 parts of the same organic solvent NN-dimethylacetamide as in step 1 to form an aluminum powder slurry; wherein the aluminum powder slurry has the following composition by mass: 40 parts of spherical aluminum powder, 50 parts of organic solvent, 2 parts of binder, and 1 part of disperser.

[0121] Step 3: stirring: placing the aluminum powder slurry obtained in step 2 in a ball mill, adding ball mill beads and milling uniformly;

[0122] Step 4: Degassing: placing the slurry tank obtained in step 3 in a vacuum box with a vacuum degree of -0.1 MPa, and maintaining the pressure for 5 minutes to perform vacuum degassing treatment to obtain a mixed aluminum powder slurry;

[0123] Step 5: coating: the mixed aluminum powder slurry obtained in step 4 is evenly coated on the front and back sides of the aluminum foil substrate, with a coating thickness of 120 μm, to form a slurry layer; the slurry layer is tested to ensure that the slurry layer is qualified;

[0124] Step 6 Drying: The aluminum foil with the aluminum slurry layer after coating in step 5 is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil.

[0125] Comparative Example 7:

[0126] A method for dispersing aluminum powder of anode foil slurry of a high-voltage aluminum electrolytic capacitor comprises the following steps:

[0127] Step 1: Dissolving the dispersant and binder: Dissolve 2 parts of binder polyvinylidene fluoride (brand name: Wu Yu 1000, Dongguan Jiangyu New Materials Co., Ltd.) and 3 parts of dispersant styrene butadiene rubber in 25 parts of organic solvent (composed of NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) according to mass parts to obtain a preliminary solution;

[0128] Step 2: Slurry preparation: Mix the initial solution with 45 parts of spherical aluminum powder with an average particle size of 5 μm, and then add 25 parts of the same type of organic solvent as in step 1 (composed of NN-dimethylacetamide and acetonitrile in a volume ratio of 2:1) to form an aluminum powder slurry; wherein the composition of the aluminum powder slurry in parts by mass is: 45 parts of spherical aluminum powder, 50 parts of organic solvent, 2 parts of binder, and 3 parts of dispersant.

[0129] Step 3: stirring: placing the aluminum powder slurry obtained in step 2 in a ball mill, adding ball mill beads and milling uniformly;

[0130] Step 4: Degassing: placing the slurry tank obtained in step 3 in a vacuum box with a vacuum degree of -0.1 MPa, and maintaining the pressure for 5 minutes to perform vacuum degassing treatment to obtain a mixed aluminum powder slurry;

[0131] Step 5: coating: the mixed aluminum powder slurry obtained in step 4 is evenly coated on the front and back sides of the aluminum foil substrate, with a coating thickness of 120 μm, to form a slurry layer; the slurry layer is tested to ensure that the slurry layer is qualified;

[0132] Step 6 Drying: The aluminum foil with the aluminum slurry layer after coating in step 5 is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil.

[0133] Slurry state:

[0134] Figure 2 The actual photos of the slurries of Example 1 and Comparative Examples 1, 4 and 7 are shown, corresponding to Figure 2As shown in a, b, c, and d, the slurry without adding a dispersant in the implementation case is unevenly dispersed, and a large amount of slurry adheres to the ball milling beads, which is not conducive to the coating of the slurry. Comparative Examples 1, 4, and 7 are actual pictures of slurries with different dispersants added to the slurry. It can be seen from the figures that the slurry dispersion effect is better after adding the dispersant, and the separation effect of the slurry and the ball milling beads is better, which is conducive to the coating of the slurry on the aluminum foil.

[0135] Shape detection:

[0136] The microscopic morphology of the coated foils in Examples 1 and 2 and Comparative Examples 1-7 was analyzed by scanning electron microscopy (SEM) to observe the dispersion uniformity of the aluminum powder in the slurry, the uniformity of the particle size, and the degree of adhesion between the aluminum powder and the substrate.

[0137] Figure 3 The SEM images of Example 1 at different magnifications are shown. It can be seen from the figure that when triethanolamine and styrene-butadiene rubber are not added as dispersants, the aluminum powder particles are deformed and the aluminum powder particles are unevenly distributed. However, the aluminum powder layer is firmly bonded to the aluminum foil substrate and is not easy to fall off.

[0138] Figure 4 The planar SEM images of the coated foils of Comparative Examples 1-4 correspond to Figure 4 a, b, c, d, and e, f, g, and h are partial enlarged views of a, b, c, and d, respectively. It can be seen from the figures that the aluminum powder is evenly dispersed using different proportions of dispersants, and can be firmly bonded to the aluminum foil substrate without falling off, which is beneficial to the sintering process.

[0139] Figure 5 It is a real picture of the coated foil and the coated aluminum foil of comparative example 1 being bent. It can be seen that the coated aluminum foil is smooth and flat, without obvious cracks and large particles. At the same time, there is no obvious material falling after the bending test, which shows that the coated aluminum foil has good mechanical stability and the slurry has good adhesion to the aluminum foil.

[0140] From the above analysis, the aluminum powder in the coated foil slurry obtained by the preparation method of the anode foil slurry of the present invention is evenly dispersed, has good bonding performance, and has a simple preparation process. The coated foil obtained by the coating process has excellent mechanical properties and evenly distributed aluminum powder particles, which can greatly improve the porosity and increase the capacity of the anode foil.

[0141] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for dispersing aluminum powder for anode foil slurry of high-voltage aluminum electrolytic capacitors, Features: The following steps are involved: Step 1, dissolving the dispersant and the binder: dissolving the binder and the dispersant in an organic solvent to obtain a primary melt; Step 2, slurry preparation: mixing the initial melt obtained in step 1 with the spherical aluminum powder, and then adding the same type of organic solvent as in step 1 to form an aluminum powder slurry; Step 3, ball milling: placing the aluminum powder slurry obtained in step 2 in a ball milling tank, adding ball milling beads and ball milling to obtain a slurry; Step 4, degassing: placing the slurry tank obtained in step 3 in a vacuum box for vacuum treatment to obtain a mixed aluminum powder slurry; In the step 1, the binder is one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene or phenolic resin; the dispersant is one or more of triethanolamine, polyvinyl alcohol, styrene-butadiene rubber or methyl amyl alcohol; In the step 2, the aluminum powder slurry comprises, by mass, 35-45 parts of spherical aluminum powder, 45-55 parts of organic solvent, 1-5 parts of binder, and 1-5 parts of dispersant.

2. The aluminum powder dispersion method according to claim 1, Features: The average particle size of the spherical aluminum powder in step 2 is 3-5 μm.

3. The aluminum powder dispersion method according to claim 1, Features: In step 2, the organic solvent is one or more of ethyl acetate, acetone, NN-dimethylacetamide, N-methylpyrrolidone or acetonitrile.

4. The aluminum powder dispersion method according to claim 1, Features: In step 4, when the vacuum box is evacuated, the vacuum degree is -0.1 MPa; and the pressure holding time is 5 minutes.

5. The aluminum powder dispersion method according to claim 1, Features: The purity of the spherical aluminum powder is greater than 99.98%.

6. A mixed aluminum powder slurry prepared by the aluminum powder dispersion method according to any one of claims 1 to 5.

7. A method for preparing aluminum foil using the mixed aluminum powder slurry according to claim 6, It is characterized in that The steps include: Step A, coating: uniformly coating the mixed aluminum powder slurry described in claim 6 on both sides of the aluminum foil substrate to form a slurry layer; testing the slurry layer to ensure that the slurry layer is qualified; Step B, drying: the aluminum foil with the aluminum slurry layer after coating in step A is placed in a vacuum dryer for drying to obtain a dried coated aluminum foil.

8. An aluminum foil prepared according to the method of claim 7.

9. Use of the aluminum foil according to claim 8 in preparing capacitors.

10. The use according to claim 10, Features: The capacitor is a high voltage aluminum electrolytic capacitor.

Citation Information

Patent Citations

  • Tape casting aluminum nitride green body manufacturing method

    CN103121238A

  • Porous alumina ceramic plate, and preparation method thereof

    CN110330358A

  • Semi-dry forming process of high-power multi-layer chip capacitor

    CN114188157A

  • Preparation method of high-specific-volume electrolytic capacitor anode foil

    CN116174724A

  • Functional nanoparticle dispersion slurry as well as preparation and application thereof

    CN116504457A

Cited By

  • Aluminum powder slurry for capacitor anode foil and preparation method thereof

    CN121483875A

  • Aluminum powder slurry for capacitor anode foil and method of preparing the same

    CN121483875B