Preparation method of heteroatom-doped hierarchical porous carbon supercapacitor electrode material with small mesoporous structure

By using the 'hard template + chemical activation' strategy in porous carbon materials, heteroatom doped hierarchical porous carbon supercapacitor electrode material with small mesoporous structures has been solved, and the problem of insufficient electrochemical performance of porous carbon materials in the prior art is solved. High specific capacity and excellent rate performance are achieved.

CN119049892APending Publication Date: 2024-11-29SHANGHAI JIAOTONG UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411218254.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to achieve customized pore size distribution of porous carbon materials, resulting in insufficient electrochemical performance of porous carbon electrode materials, especially in terms of rate performance and cycle stability.

Method used

Using the 'hard template + chemical activation' strategy, using chitosan, sodium lignin sulfonate, bamboo fiber and other materials, carbonization through ultrasonic treatment and high temperature under nitrogen atmosphere, forming heteroatom doped staging porous carbon with small mesoporous structure Supercapacitor electrode material.

Benefits of technology

The customized small mesoporous distribution of porous carbon materials is realized, the specific surface area, heteroatomic functional group content and electrochemical performance of the material are improved, and the high specific capacity, superior rate performance and excellent cycle stability are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005022196580000011
    Figure HDA0005022196580000011
  • Figure HDA0005022196580000012
    Figure HDA0005022196580000012
  • Figure HDA0005022196580000021
    Figure HDA0005022196580000021
Patent Text Reader

Abstract

The invention discloses a preparation method of a heteroatom-doped hierarchical porous carbon supercapacitor electrode material with a small mesoporous structure, and relates to the technical field of materials. An aerogel carbon precursor is prepared from chitosan and sodium lignin sulfonate, a sulfur source, an oxygen source and a nitrogen source cooperate with one another, more charges are transferred, good rate capability and stability can be kept under high current density and long-time electric circulation, and the material achieves excellent electrochemical performance; then adding bamboo fibers, and performing high-power ultrasonic treatment to enable the aerogel to form a mechanically stable nano network structure, so as to provide more diffusion channels for charges; then potassium hydroxide is used for activating treatment, so that the surface of the gel is rougher, a 3D porous carbon frame structure is formed, ion transmission is promoted, ions are rapidly diffused in the charging and discharging processes, and excellent rate capability, excellent cycling stability and high energy density are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material technology, and in particular to a method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material with a small mesoporous structure. Background Art

[0002] With the booming development of electric vehicles and portable consumer electronics, the demand for sustainable and renewable energy conversion and storage devices is increasing. Supercapacitors are widely regarded as one of the most promising energy storage systems (EES) due to their advantages such as high power density, long cycle life and low cost. However, the low energy density greatly limits the development and practical application of supercapacitors. Biomass-derived activated carbon has the advantages of excellent electrochemical properties, high specific surface area, high adsorption, adjustable surface chemistry, fast ion / electron transport, rich functional groups and low cost. It is a promising supercapacitor electrode material and is of great significance for the further development and application of high energy density supercapacitors.

[0003] There have been many studies on biomass-derived porous carbon electrodes for supercapacitors in existing literature and patents. CN108022762A discloses a method for preparing nitrogen-doped porous carbon supercapacitor electrode materials based on peanut shells. Using peanut shells as a precursor and sodium hydroxide as an activator, a nitrogen-doped porous carbon material with high specific surface porosity was obtained, realizing the effective utilization of waste resources. CN106542513A discloses a S-doped microporous-mesoporous-macroporous porous carbon with high specific surface area and a preparation method thereof, using lignin sulfonate as a dual source of C and S, sulfuric acid as a hydrolyzing agent, and tetraethyl orthosilicate as a mesoporous template agent. A S-doped microporous-mesoporous-macroporous porous carbon supercapacitor material with high specific surface area was obtained. The specific surface area of ​​the obtained material is 952 to 1534 m 2 ·g -1 , pore volume is 0.89~1.74cm 3 ·g -1 , the specific capacity in aqueous electrolyte can reach 318F·g -1 CN115642039A discloses a method for preparing a nitrogen-phosphorus co-doped eucalyptus bark porous carbon supercapacitor electrode material, wherein the prepared electrode material has the advantages of high specific surface area, rich heteroatom functional groups, high specific capacitance, etc.

[0004] Although there are many reports on biomass-derived porous carbon electrodes for supercapacitors in existing literature and patents, most of these methods fail to achieve customized pore size distribution of porous carbon materials, making it difficult to further improve the electrochemical performance of porous carbon electrode materials. In response to the above problems, this patent proposes a "hard template + chemical activation" strategy to achieve customized small mesopore distribution of porous carbon materials, while ensuring high specific capacity and achieving superior rate performance. So far, there has been no report on the use of the "hard template + chemical activation" strategy to prepare heteroatom-doped hierarchical porous carbon supercapacitor electrode materials with small mesoporous structures. Summary of the invention

[0005] The present invention overcomes the problems of insufficient rate performance of porous carbon mainly composed of micropores prepared by traditional chemical activation, and uses chitosan, sodium lignin sulfonate, and bamboo fiber as carbon sources and heteroatom sources, and adopts a "hard template + chemical activation" strategy to obtain a heteroatom-doped graded porous carbon electrode material with a small mesoporous structure. The electrode material has a high specific surface area, is rich in heteroatom functional groups, has a high specific capacitance, has good rate performance, and has excellent cycle stability.

[0006] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure, comprising the following preparation steps:

[0007] (1) Dissolve chitosan in a 2 wt % acetic acid aqueous solution, sonicate for 15 min, add sodium lignin sulfonate and ferric nitrate, stir magnetically for 12 h, add bamboo pulp solution, place in an ice water bath, sonicate for 60 min, add tert-butyl alcohol, then transfer to a polytetrafluoroethylene mold and freeze at -20 ° C for 24 h, then dry at 8 Pa and -50 ° C for 48 h to obtain an aerogel;

[0008] (2) The aerogel prepared in step (1) was transferred to a quartz tube furnace and heated at 5 °C min under a nitrogen atmosphere. -1 The temperature was raised to 700°C at a rate of 1 to 3 hours, and the obtained product was dispersed in a dilute acid solution, heated in a water bath at 60°C for 12 hours, and further vacuum filtered, and washed with deionized water until the filtrate was neutral, and dried at 80°C;

[0009] (3) In a nitrogen atmosphere, and with the aid of ultrasound, a 20 wt % potassium hydroxide aqueous solution is sprayed onto the carbonized product obtained in step (2) at 5 ° C. min. -1 The temperature is raised to 650-850°C at a rate, and activated for 0.5-2h to obtain a carbon material;

[0010] (4) washing the product of step (3) with a dilute acid solution and distilled water until neutral;

[0011] (5) The product of step (4) is dried at 80° C. for 12 to 24 hours to obtain a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure.

[0012] Furthermore, the magnetic stirring rate in step (1) is 200 to 350 rpm.

[0013] Furthermore, the output power of the ultrasound in step (1) is 1200W.

[0014] Furthermore, in step (1), the mass ratio of the chitosan, 2 wt% acetic acid aqueous solution, sodium lignin sulfonate, ferric nitrate, bamboo pulp solution and tert-butanol is 0.3:50:0.7:0:0.1:0.1 to 0.3:50:0.7:1:0.3:0.1.

[0015] Furthermore, the mass ratio of the product in step (2) to the dilute acid solution is 1:3 to 1:5.

[0016] Furthermore, the drying time in step (2) is 8 to 12 hours.

[0017] Furthermore, the mass ratio of the carbonized product in step (3) to the 20 wt % potassium hydroxide aqueous solution is 1:0.5 to 1:0.8.

[0018] Furthermore, the ultrasonic frequency in step (1) and step (3) is 20 kHz.

[0019] Furthermore, the dilute acid solution in step (2) and step (4) is a 5 mol / L hydrochloric acid solution.

[0020] Furthermore, any one of the heteroatom-doped hierarchical porous carbon supercapacitor electrode materials with a small mesoporous structure prepared can be used in the preparation of supercapacitor electrode materials.

[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0022] The heteroatom-doped graded porous carbon supercapacitor electrode material with a small mesoporous structure prepared by the present invention proposes a "hard template + chemical activation" strategy to achieve customized small mesopore distribution of porous carbon materials. When used for supercapacitor electrode materials, it achieves excellent rate performance while ensuring high specific capacity.

[0023] Firstly, chitosan was used as nitrogen source and sodium lignin sulfonate as carbon source and sulfur source to prepare aerogel carbon precursor. Sulfur atom doping in carbon structure played a role in changing the self-selected density, thereby promoting nitrogen-containing and oxygen-containing groups to induce more charge transfer and improve the conductivity of the material. The disulfide groups can accelerate the ion transfer rate and maintain good rate performance and stability under high current density and long-term charge and discharge cycles. The groups in the form of sulfur and oxygen structures can improve the pseudocapacitance performance of the material by enhancing wettability. The rich heteroatom functional groups cooperate with each other, and the hierarchical porous structure of the aerogel makes the material Excellent electrochemical properties are achieved; then bamboo fiber is added and treated with high-power ultrasound to cause cavitation, forming local hotspots with ultra-high temperature, ultra-high pressure, and ultra-fast heating and cooling rates, which destroy the hydrogen bonds of cellulose linear polymers and decompose them into nanofibers. The aerogel forms a mechanically stable nano-network structure, and the three-dimensional aromatic hydrocarbon structure of lignin can improve the order of the material. Even after high-temperature pyrolysis and sodium hydroxide activation, the formed porous structure remains intact and is not easy to collapse. In addition, its short-range ordered local structure is beneficial to the conductivity of graphite and provides more diffusion channels for charges.

[0024] Secondly, the carbonized aerogel is activated with potassium hydroxide to make the gel surface rougher, forming a 3D porous carbon framework structure, thereby promoting ion transport; a large number of mesopores and micropores with rich porosity and high pore volume allow ions to diffuse rapidly during charging and discharging during electrolyte storage, and while ensuring high specific capacity, achieve superior rate performance, excellent cycle stability and high energy density. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 1 is a transmission electron microscope image and an energy spectrum image of the material DHPC-0.5-750 obtained in Example 2;

[0026] Figure 2 is the X-ray diffraction pattern of all materials in the embodiments;

[0027] Figure 3 is the nitrogen adsorption-desorption isotherm diagram of all materials in the examples;

[0028] Figure 4 All materials in the examples are at 50mV·s -1 The charge and discharge curve diagram of

[0029] Figure 5 All materials in the examples are at 1A·g -1 Constant current charge and discharge diagram. DETAILED DESCRIPTION

[0030] The present invention is further described in detail below in conjunction with specific embodiments, wherein all raw material components are commercially available products well known to those skilled in the art unless otherwise specified, and the technical means used are conventional means well known to those skilled in the art unless otherwise specified.

[0031] The present invention will prepare supercapacitor electrode materials respectively, and use them for electrode preparation, and further test the electrochemical performance. The following examples all use the following method to prepare electrodes: weigh 80 mg of supercapacitor electrode material, 10 mg of acetylene black, and 10 mg of polytetrafluoroethylene binder in a 50 mL beaker, add 10 mL of anhydrous ethanol, ultrasonicate for 30 minutes, put it in a drying oven and dry it to a plasticine-like state, evenly apply the plasticine-like mixture on the nickel foam, press it with a tablet press at a pressure of 10 MPa for 1 minute, and put it in a vacuum drying oven to dry. The active material loading on the electrode is 2-3 mg cm -2 .

[0032] Example 1

[0033] The chitosan was dissolved in a 2wt% acetic acid aqueous solution, ultrasonicated for 15 minutes, sodium lignin sulfonate was added, magnetic stirring was performed at 200rpm for 12 hours, bamboo pulp solution was added, and the mixture was placed in an ice-water bath, ultrasonicated at a power of 1200W and a frequency of 20kHz for 60 minutes, tert-butanol was added, and then the mixture was transferred to a polytetrafluoroethylene mold and frozen at -20°C for 24 hours, and then dried at a vacuum degree of 8Pa and -50°C for 48 hours to obtain an aerogel; wherein the mass ratio of the chitosan, 2wt% acetic acid aqueous solution, sodium lignin sulfonate, bamboo pulp solution, and tert-butanol was 0.3:50:0.7:0.1:0.1; the aerogel was transferred to a quartz tube furnace and condensed at 5°C·min under a nitrogen atmosphere. -1 The temperature was raised to 700°C at a rate of 1:3, and the carbonized product was sprayed with a 20 wt% potassium hydroxide aqueous solution under a nitrogen atmosphere and assisted by 20 kHz ultrasound at a rate of 5°C·min·s. The obtained product was dispersed in a 5 mol / L hydrochloric acid solution, heated in a water bath at 60°C for 12 h, further vacuum filtered, washed with deionized water until the filtrate was neutral, and dried at 80°C for 8 h; wherein the mass ratio of the product to the 5 mol / L hydrochloric acid solution was 1:3; a 20 wt% potassium hydroxide aqueous solution was sprayed on the carbonized product under a nitrogen atmosphere and assisted by 20 kHz ultrasound at a rate of 5°C·min·s. -1 The temperature was raised to 750°C at a rate and activated for 0.5h to obtain a carbon material; wherein the mass ratio of the carbonized product to a 20wt% potassium hydroxide aqueous solution was 1:0.5; the mixture was washed with a 5mol / L hydrochloric acid solution and distilled water until neutral, and dried at 80°C for 12h to obtain a porous carbon material. The material obtained in this example was labeled DHPC-0-750.

[0034] The electrode was prepared by DHPC-0-750 and subjected to electrochemical test. In the three-electrode system, 6 mol / L potassium hydroxide solution was used as electrolyte, Hg / HgO was used as reference electrode, platinum sheet was used as counter electrode, and the electrode loaded with active material was used as working electrode. The electrochemical performance was tested. The specific capacitance under different current density was shown in Table 1:

[0035] Table 1

[0036] <![CDATA[Current density (A·g -1 )]]> 0.5 1 2 5 10 15 20 <![CDATA[Specific capacitance (F·g -1 )]]> 270.00 250.14 236.99 210.74 187.35 179.02 171.11

[0037] Example 2

[0038] The chitosan was dissolved in a 2wt% acetic acid aqueous solution, ultrasonicated for 15 minutes, sodium lignin sulfonate and ferric nitrate were added, magnetically stirred at 275rpm for 12 hours, bamboo pulp solution was added, placed in an ice-water bath, ultrasonicated at a power of 1200W and a frequency of 20kHz for 60 minutes, tert-butanol was added, and then transferred to a polytetrafluoroethylene mold and frozen at -20°C for 24 hours, and then dried at a vacuum degree of 8Pa and -50°C for 48 hours to obtain an aerogel; wherein the mass ratio of the chitosan, 2wt% acetic acid aqueous solution, sodium lignin sulfonate, ferric nitrate, bamboo pulp solution, and tert-butanol was 0.3:50:0.7:0.5:0.2:0.1; the aerogel was transferred to a quartz tube furnace and condensed at 5°C·min under a nitrogen atmosphere. -1 The temperature was raised to 700°C at a rate of 1:4, and the carbonized product was sprayed with a 20 wt% potassium hydroxide aqueous solution under a nitrogen atmosphere and assisted by 20 kHz ultrasound at a rate of 5°C·min·s. The obtained product was dispersed in a 5 mol / L hydrochloric acid solution, heated in a water bath at 60°C for 12 h, further vacuum filtered, washed with deionized water until the filtrate was neutral, and dried at 80°C for 10 h; wherein the mass ratio of the product to the 5 mol / L hydrochloric acid solution was 1:4; a 20 wt% potassium hydroxide aqueous solution was sprayed on the carbonized product under a nitrogen atmosphere and assisted by 20 kHz ultrasound at a rate of 5°C·min·s. -1 The temperature was raised to 750°C at a rate and activated for 1 hour to obtain a carbon material; wherein the mass ratio of the carbonized product to a 20wt% potassium hydroxide aqueous solution was 1:0.6; it was washed with a 5mol / L hydrochloric acid solution and distilled water until neutral, and dried at 80°C for 18 hours to obtain a porous carbon material. The material obtained in this example was marked as DHPC-0.5-750.

[0039] The electrode was prepared by DHPC-0.5-750 and subjected to electrochemical test. In the three-electrode system, 6 mol / L potassium hydroxide solution was used as electrolyte, Hg / HgO was used as reference electrode, platinum sheet was used as counter electrode, and the electrode loaded with active material was used as working electrode. The electrochemical performance was tested. The specific capacitance under different current density was shown in Table 2:

[0040] Table 2

[0041] <![CDATA[Current density (A·g -1 )]]> 0.5 1 2 5 10 15 20 <![CDATA[Specific capacitance (F·g -1 )]]> 330.82 317.89 311.42 286.73 280.55 273.19 269.88

[0042] Example 3

[0043] The chitosan was dissolved in a 2wt% acetic acid aqueous solution, ultrasonicated for 15 minutes, sodium lignin sulfonate and ferric nitrate were added, magnetically stirred at 350rpm for 12 hours, bamboo pulp solution was added, placed in an ice-water bath, ultrasonicated at a power of 1200W and a frequency of 20kHz for 60 minutes, tert-butanol was added, and then transferred to a polytetrafluoroethylene mold and frozen at -20°C for 24 hours, and then dried at a vacuum degree of 8Pa and -50°C for 48 hours to obtain an aerogel; wherein the mass ratio of the chitosan, 2wt% acetic acid aqueous solution, sodium lignin sulfonate, ferric nitrate, bamboo pulp solution, and tert-butanol was 0.3:50:0.7:1:0.3:0.1; the aerogel was transferred to a quartz tube furnace and condensed at 5°C·min under a nitrogen atmosphere. -1 The temperature was raised to 700°C at a rate of 1:5, and the carbonized product was sprayed with a 20 wt% potassium hydroxide aqueous solution under a nitrogen atmosphere and assisted by 20 kHz ultrasound at a rate of 5°C·min·s. The obtained product was dispersed in a 5 mol / L hydrochloric acid solution, heated in a water bath at 60°C for 12 h, further vacuum filtered, and washed with deionized water until the filtrate was neutral, and dried at 80°C for 12 h; wherein the mass ratio of the product to the 5 mol / L hydrochloric acid solution was 1:5; a 20 wt% potassium hydroxide aqueous solution was sprayed on the carbonized product under a nitrogen atmosphere and assisted by 20 kHz ultrasound at a rate of 5°C·min·s. -1 The temperature was raised to 750°C at a rate and activated for 2 hours to obtain a carbon material; wherein the mass ratio of the carbonized product to a 20wt% potassium hydroxide aqueous solution was 1:0.8; it was washed with a 5mol / L hydrochloric acid solution and distilled water until neutral, and dried at 80°C for 24 hours to obtain a porous carbon material. The material obtained in this example was marked as DHPC-1-750.

[0044] The electrode was prepared by DHPC-1-750 and subjected to electrochemical test. In the three-electrode system, 6 mol / L potassium hydroxide solution was used as electrolyte, Hg / HgO was used as reference electrode, platinum sheet was used as counter electrode, and the electrode loaded with active material was used as working electrode. The electrochemical performance was tested. The specific capacitance under different current density was shown in Table 3:

[0045] Table 3

[0046] <![CDATA[Current density (A·g -1 )]]> 0.5 1 2 5 10 15 20 <![CDATA[Specific capacitance (F·g -1 )]]> 231.52 220.65 211.06 188.47 172.472 165.288 159.80

[0047] Example 4

[0048] The chitosan was dissolved in a 2wt% acetic acid aqueous solution, ultrasonicated for 15 minutes, sodium lignin sulfonate and ferric nitrate were added, magnetically stirred at 275rpm for 12 hours, bamboo pulp solution was added, placed in an ice-water bath, ultrasonicated at a power of 1200W and a frequency of 20kHz for 60 minutes, tert-butanol was added, and then transferred to a polytetrafluoroethylene mold and frozen at -20°C for 24 hours, and then dried at a vacuum degree of 8Pa and -50°C for 48 hours to obtain an aerogel; wherein the mass ratio of the chitosan, 2wt% acetic acid aqueous solution, sodium lignin sulfonate, ferric nitrate, bamboo pulp solution, and tert-butanol was 0.3:50:0.7:0.5:0.2:0.1; the aerogel was transferred to a quartz tube furnace and condensed at 5°C·min under a nitrogen atmosphere. -1 The temperature was raised to 700°C at a rate of 1:4, and the carbonized product was sprayed with a 20 wt% potassium hydroxide aqueous solution under a nitrogen atmosphere and assisted by 20 kHz ultrasound at a rate of 5°C·min·s. The obtained product was dispersed in a 5 mol / L hydrochloric acid solution, heated in a water bath at 60°C for 12 h, further vacuum filtered, washed with deionized water until the filtrate was neutral, and dried at 80°C for 10 h; wherein the mass ratio of the product to the 5 mol / L hydrochloric acid solution was 1:4; a 20 wt% potassium hydroxide aqueous solution was sprayed on the carbonized product under a nitrogen atmosphere and assisted by 20 kHz ultrasound at a rate of 5°C·min·s. -1 The temperature was raised to 650°C at a rate and activated for 1 hour to obtain a carbon material; wherein the mass ratio of the carbonized product to a 20wt% potassium hydroxide aqueous solution was 1:0.6; it was washed with a 5mol / L hydrochloric acid solution and distilled water until neutral, and dried at 80°C for 18 hours to obtain a porous carbon material. The material obtained in this example was marked as DHPC-0.5-650.

[0049] The electrode was prepared by DHPC-0.5-650 and subjected to electrochemical test. In the three-electrode system, 6 mol / L potassium hydroxide solution was used as electrolyte, Hg / HgO was used as reference electrode, platinum sheet was used as counter electrode, and the electrode loaded with active material was used as working electrode. The electrochemical performance was tested. The specific capacitance under different current density was shown in Table 4:

[0050] Table 4

[0051] <![CDATA[Current density (A·g -1 )]]> 0.5 1 2 5 10 15 20 <![CDATA[Specific capacitance (F·g -1 )]]> 201.13 183.70 179.11 160.30 144.26 140.97 136.96

[0052] Example 5

[0053] The chitosan was dissolved in a 2wt% acetic acid aqueous solution, ultrasonicated for 15 minutes, sodium lignin sulfonate and ferric nitrate were added, magnetically stirred at 275rpm for 12 hours, bamboo pulp solution was added, placed in an ice-water bath, ultrasonicated at a power of 1200W and a frequency of 20kHz for 60 minutes, tert-butanol was added, and then transferred to a polytetrafluoroethylene mold and frozen at -20°C for 24 hours, and then dried at a vacuum degree of 8Pa and -50°C for 48 hours to obtain an aerogel; wherein the mass ratio of the chitosan, 2wt% acetic acid aqueous solution, sodium lignin sulfonate, ferric nitrate, bamboo pulp solution, and tert-butanol was 0.3:50:0.7:0.5:0.2:0.1; the aerogel was transferred to a quartz tube furnace and condensed at 5°C·min under a nitrogen atmosphere. -1 The temperature was raised to 700°C at a rate of 1:4, and the carbonized product was sprayed with a 20 wt% potassium hydroxide aqueous solution under a nitrogen atmosphere and assisted by 20 kHz ultrasound at a rate of 5°C·min·s. The obtained product was dispersed in a 5 mol / L hydrochloric acid solution, heated in a water bath at 60°C for 12 h, further vacuum filtered, washed with deionized water until the filtrate was neutral, and dried at 80°C for 10 h; wherein the mass ratio of the product to the 5 mol / L hydrochloric acid solution was 1:4; a 20 wt% potassium hydroxide aqueous solution was sprayed on the carbonized product under a nitrogen atmosphere and assisted by 20 kHz ultrasound at a rate of 5°C·min·s. -1 The temperature was raised to 850°C at a rate and activated for 1 hour to obtain a carbon material; wherein the mass ratio of the carbonized product to a 20wt% potassium hydroxide aqueous solution was 1:0.6; it was washed with a 5mol / L hydrochloric acid solution and distilled water until neutral, and dried at 80°C for 18 hours to obtain a porous carbon material. The material obtained in this example was marked as DHPC-0.5-850.

[0054] The electrode was prepared by DHPC-0.5-850 and subjected to electrochemical test. In the three-electrode system, 6 mol / L potassium hydroxide solution was used as electrolyte, Hg / HgO was used as reference electrode, platinum sheet was used as counter electrode, and the electrode loaded with active material was used as working electrode. The electrochemical performance was tested. The specific capacitance under different current density was shown in Table 5:

[0055] Table 5

[0056] <![CDATA[Current density (A·g -1 )]]> 0.5 1 2 5 10 15 20 <![CDATA[Specific capacitance (F·g -1 )]]> 240.63 224.27 214.64 194.65 175.93 167.49 162.60

[0057] The present invention includes but is not limited to the above-mentioned embodiments. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material with a small mesoporous structure, It is characterized in that The method comprises the following preparation steps: (1) Dissolve chitosan in a 2 wt % acetic acid aqueous solution, sonicate for 15 min, add sodium lignin sulfonate and ferric nitrate, stir magnetically for 12 h, add bamboo pulp solution, place in an ice water bath, sonicate for 60 min, add tert-butyl alcohol, then transfer to a polytetrafluoroethylene mold and freeze at -20 ° C for 24 h, then dry at 8 Pa and -50 ° C for 48 h to obtain an aerogel; (2) The aerogel prepared in step (1) was transferred to a quartz tube furnace and heated at 5 °C min under a nitrogen atmosphere. -1 The temperature was raised to 700°C at a rate of 1 to 3 hours, and the obtained product was dispersed in a dilute acid solution, heated in a water bath at 60°C for 12 hours, and further vacuum filtered, and washed with deionized water until the filtrate was neutral, and dried at 80°C; (3) In a nitrogen atmosphere, and with the aid of ultrasound, a 20 wt % potassium hydroxide aqueous solution is sprayed onto the carbonized product obtained in step (2) at 5 ° C. min. -1 The temperature is raised to 650-850°C at a rate, and activated for 0.5-2h to obtain a carbon material; (4) washing the product of step (3) with a dilute acid solution and distilled water until neutral; (5) The product of step (4) is dried at 80° C. for 12 to 24 hours to obtain a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure.

2. The method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure according to claim 1, Features The magnetic stirring rate in step (1) is 200-350 rpm.

3. The method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure according to claim 1, Features The output power of the ultrasound in step (1) is 1200W.

4. The method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure according to claim 1, Features The mass ratio of the chitosan, 2wt% acetic acid aqueous solution, sodium lignin sulfonate, ferric nitrate, bamboo pulp solution and tert-butanol in step (1) is 0.3:50:0.7:0:0.1:0.1 to 0.3:50:0.7:1:0.3:0.

1.

5. The method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure according to claim 1, Features The mass ratio of the product in step (2) to the dilute acid solution is 1:3 to 1:

5.

6. The method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure according to claim 1, Features The drying time in step (2) is 8 to 12 hours.

7. The method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure according to claim 1, Features The mass ratio of the carbonized product in step (3) to the 20wt% potassium hydroxide aqueous solution is 1:0.5 to 1:0.

8.

8. The method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure according to claim 1, Features The ultrasonic frequency in step (1) and step (3) is 20 kHz.

9. The method for preparing a heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure according to claim 1, Features The dilute acid solution in step (2) and step (4) is a 5 mol / L hydrochloric acid solution.

10. Use of the heteroatom-doped hierarchical porous carbon supercapacitor electrode material having a small mesoporous structure prepared according to any one of claims 1 to 9 in preparing supercapacitor electrode materials.

Citation Information

Cited By

  • Lignin-cellulose-based hierarchical porous carbon, preparation method thereof and application of lignin-cellulose-based hierarchical porous carbon in supercapacitor