Semiconductor chip packaging method for controlling soldering tin climbing

By setting a silver plating layer on the bare copper frame during the semiconductor chip packaging process and monitoring the chip residence time after soldering, the problem of solder climbing is solved, and the yield and reliability of the chip packaging are improved.

CN119049989APending Publication Date: 2024-11-29华羿微电子股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411147435.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

During semiconductor chip packaging, high solder climbing leads to low yield and reliability of finished chip packaging.

Method used

Use a bare copper frame and set a silver plating layer in its adhesive sheet area. The melt adhesive sheet material forms a solder layer on the surface of the silver plating layer, and press the chip on the solder layer to monitor the chip residence time after welding, and clear after exceeding the preset time. Out of the processing track to prevent solder from reflowing.

Benefits of technology

It effectively avoids solder climbing and improves the yield and reliability of chip packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049989A_ABST
    Figure CN119049989A_ABST
Patent Text Reader

Abstract

The invention discloses a semiconductor chip packaging method for controlling soldering tin climbing, and the method comprises the steps: taking a bare copper frame as a lead frame, and arranging a silver coating in a bonding area of the bare copper frame; the packaging equipment is filled with nitrogen and hydrogen mixed gas and works in a processing track at a preset temperature, a chip bonding material is melted on the surface of the silver plating layer to form a solder layer, then a target chip is pressed on the surface of the solder layer, and a welded chip is obtained; and after the time that the welded chip stays in the processing track exceeds the preset duration, the welded chip is cleared out of the processing track. According to the invention, the defect of soldering tin climbing in the packaging process of the semiconductor chip can be effectively controlled, and the packaging yield and reliability of a chip finished product are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor chip packaging, and in particular to a semiconductor chip packaging method for controlling solder creep height. Background Art

[0002] Solder is an important connecting material for connecting the chip to the lead frame during the semiconductor chip packaging process. Solder not only fixes the chip to the frame, but also conducts electricity and dissipates heat for the chip. Lead-containing solder is the most commonly used bonding material in traditional packaging processes, and its melting point is above 200°C.

[0003] In the prior art, the core loading process of the packaging process requires melting the lead-containing solder on the copper lead frame under high temperature conditions in a track filled with nitrogen-hydrogen mixed gas, and setting the solder pattern or tin pressing pattern of the lead-containing solder and the amount of solder according to the chip size through processing equipment; then the chip is picked up by the welding head assembly of the processing equipment, and a certain pressure is applied to bond the chip to the lead frame. After cooling, the solder solidifies so that the chip and the lead frame are bonded together.

[0004] Since lead-containing solder is bonded in a molten state, there will be incomplete solder reflow after bonding, which will cause part of the solder to climb along the edge side wall of the chip after bonding, and even climb to the surface of the chip, causing a chip short circuit. If the solder climbing height is too high, it will cause chip edge collapse or even cracking due to stress in the subsequent packaging process, seriously affecting the reliability of the finished chip. Summary of the invention

[0005] The invention provides a semiconductor chip packaging method for controlling solder creepage, which solves the problem of low chip finished product packaging yield and reliability caused by solder creepage during semiconductor chip packaging.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme:

[0007] The present invention provides a semiconductor chip packaging method for controlling solder creep height, the method comprising:

[0008] A bare copper frame is used as a lead frame, and a silver-plated layer is provided on the chip bonding area of ​​the bare copper frame; the size of the silver-plated layer is larger than the size of the target chip;

[0009] In a processing track of a packaging device filled with nitrogen and hydrogen mixed gas and operating at a preset temperature, the bonding material is melted on the surface of the silver-plated layer to form a solder layer, and then the target chip is pressed on the surface of the solder layer to obtain a soldered chip;

[0010] After the welded chip stays in the processing track for a period exceeding a preset time, the welded chip is cleared out of the processing track.

[0011] In a possible implementation, the length of the silver-plated layer is 300-1000 um greater than the length of the target chip;

[0012] The width of the silver-plated layer is 300-1000 um greater than the width of the target chip.

[0013] In a possible implementation, the preset duration is 300 seconds.

[0014] In a possible implementation, the preset temperature is within 380±40°C.

[0015] In a possible implementation, the packaging device is a soft solder die bonder.

[0016] In a possible implementation, the processing track includes a tin dropping area, a film pressing area, and a welding area sequentially arranged on the conveying track; the bonding material is melted on the surface of the silver-plated layer to form a solder layer, and then the target chip is pressed on the surface of the solder layer to obtain a soldered chip, which specifically includes:

[0017] When the lead frame provided with the silver-plated layer reaches the tin-dropping area, the tin solder formed by melting the adhesive material at the preset temperature is dropped onto the surface of the silver-plated layer;

[0018] When the lead frame dripped with the solder reaches the film pressing area, the solder is pressed into a preset tin pressing pattern to obtain a solder layer;

[0019] When the lead frame after obtaining the solder layer reaches the welding area, the target chip is pressed against the surface of the solder layer with a preset pressure to obtain a welded chip.

[0020] In a possible implementation, after pressing the target chip on the surface of the solder layer with a preset pressure to obtain a soldered chip, the method further includes:

[0021] The time the chip stays in the processing track after welding is monitored.

[0022] In a possible implementation, the bonding material is lead-containing solder.

[0023] In practical application, the semiconductor chip packaging method for controlling solder creep provided by the embodiment of the present invention uses a bare copper frame as a lead frame, and sets a silver-plated layer in the chip-bonding area of ​​the bare copper frame; then, in the processing track of the packaging equipment, the chip-bonding material is melted on the surface of the silver-plated layer to form a solder layer, and the target chip is pressed on the solder layer to obtain a soldered chip; the time for the chip to stay in the processing track after soldering is monitored, and after the stay time exceeds the preset time, the chip to be soldered is cleared out of the processing track; the silver-plated area can increase the fluidity of the solder melted from the chip-bonding material, so that the solder at the edge of the target area is spread out with the silver-plated layer to avoid solder creeping; during the packaging process, the time for the chip to stay in the processing track after soldering is monitored, and the chip to be soldered whose stay time exceeds the preset time is cleared out in time, thereby preventing the chip to stay in the working track for too long and the solder to reflow for a long time, resulting in solder creeping; the setting of the silver-plated layer and the monitoring of the time for the chip to stay in the processing track after soldering can effectively control the defect of solder creeping in the chip packaging process, and greatly improve the packaging yield and reliability of chip products. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the structure of a semiconductor chip having a solder creep defect after packaging in the prior art;

[0025] Figure 2 A flowchart of the steps of a semiconductor chip packaging method for controlling solder creep height provided by an embodiment of the present invention;

[0026] Figure 3 A schematic structural diagram of a lead frame provided with a silver-plated layer in a semiconductor chip packaging method for controlling solder creep height provided by an embodiment of the present invention;

[0027] Figure 4 A schematic diagram of the structure of a semiconductor chip packaged by a semiconductor chip packaging method for controlling solder creep height provided by an embodiment of the present invention;

[0028] Figure 5 A schematic structural diagram of a processing track in a semiconductor chip packaging method for controlling solder creep height provided by an embodiment of the present invention.

[0029] Reference numerals and descriptions:

[0030] 11. First frame; 12. First solder layer; 13. First chip; 21. Second frame; 211. Bare copper frame; 212. Silver-plated layer; 22. Second solder layer; 23. Second chip; 24. Processing track; 241. Conveying track; 242. Tin dropping area; 243. Laminating area; 244. Welding area. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] In the following, the terms "first" and "second" are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present disclosure, unless otherwise specified, "multiple" means two or more. In addition, the use of "based on" or "according to" means openness and inclusiveness, because the process, steps, calculations or other actions "based on" or "according to" one or more of the conditions or values ​​may be based on additional conditions or values ​​beyond the described values ​​in practice.

[0033] like Figure 1 As shown, in the prior art, lead-containing solder is melted on the surface of the first frame 11 under high temperature conditions to form a first solder layer 12, and the first chip 13 is pressed onto the first solder layer 12 for bonding. After bonding, the solder reflow after the lead-containing solder is melted is incomplete, resulting in a portion of the solder climbing up along the edge side wall of the chip to be packaged after bonding.

[0034] The first frame 11 is a copper lead frame, and the first chip 13 is a semiconductor chip to be packaged.

[0035] Solder climbing to the surface of the first chip 13 may cause a chip short circuit. If the solder climbing height is too high, the first chip 13 may break corners or even crack due to stress during the subsequent packaging process, seriously affecting the reliability of the finished chip after packaging.

[0036] In order to solve the problem of low chip packaging yield and reliability caused by solder creeping during semiconductor chip packaging, an embodiment of the present invention provides a semiconductor chip packaging method for controlling solder creeping.

[0037] like Figure 2 to Figure 4 As shown, the semiconductor chip packaging method for controlling solder creep height provided by the embodiment of the present invention includes:

[0038] Step 101 , using a bare copper frame 211 as a lead frame, and providing a silver plating layer 212 in the bonding area of ​​the bare copper frame 211 .

[0039] The bare copper frame 211 after the silver plating layer 212 is provided is referred to as a second frame 21 .

[0040] The size of the silver-plated layer 212 is larger than the size of the target chip, and the chip bonding area is a square area on the surface of the bare copper frame 211 where the semiconductor chip needs to be welded.

[0041] Furthermore, the length of the silver-plated layer is 300-1000um greater than the target chip length;

[0042] The width of the silver-plated layer is 300-1000um greater than the target chip width.

[0043] Step 102, in a processing track of a packaging device filled with nitrogen-hydrogen mixed gas and operating at a preset temperature, melt the bonding material on the surface of the silver-plated layer 212 to form a solder layer, and then press the target chip on the surface of the solder layer to obtain a soldered chip.

[0044] The solder layer in this step is the second solder layer 22 , and the target chip is the second chip 23 .

[0045] Furthermore, the bonding material is a conventional lead-containing solder, the melting point of which is above 200 degrees Celsius.

[0046] The solder after the bonding material is melted forms a second solder layer 22 on the surface of the second frame 21, and the second chip 23 is pressed on the surface of the second solder layer 22 to obtain Figure 4 Chip after soldering.

[0047] Furthermore, the preset temperature is within 380±40°C.

[0048] like Figure 1 As shown, compared with the copper first frame 11 used in the conventional packaging process, the second frame 21 after the silver-plated layer 212 is provided in the present invention has stronger wettability.

[0049] The solder has poor fluidity on the surface of the first frame 11 , and is not easy to spread around after bonding, which will cause the solder to climb up along the side of the first chip 13 to form a solder creeping phenomenon.

[0050] like Figure 4 As shown, the second frame 21 with a silver-plated layer 212 has a smooth surface and good oxidation resistance, strong solder fluidity and high wettability. After bonding, the solder spreads around, which can prevent the solder from climbing from the side of the second chip 23.

[0051] Therefore, after the surface of the bare copper frame 211 is silver-plated to form a silver-plated layer 212 , the solder can flow along the silver-plated layer 212 , effectively avoiding solder climbing due to the inability to reflow after soldering.

[0052] Among them, wettability refers to the formation of a uniform, smooth, continuous and firmly attached solder layer on the metal surface by the molten solder. The degree of wettability is mainly determined by the cleanliness of the lead frame surface and the surface tension of the solder.

[0053] Step 103: After the chip after welding stays in the processing track for a period exceeding a preset time, the chip after welding is cleared out of the processing track.

[0054] Specifically, since the chip after welding stays in the processing track due to packaging equipment debugging or equipment abnormality, the long stay time and the high temperature working environment of the processing track will cause the solder to reflux and oxidize on the second frame 21, causing solder climbing or chip cracking. Therefore, if the chip after welding stays in the processing track for a period of time exceeding the preset time, the function setting of clearing the chip after welding from the processing track can effectively avoid solder climbing caused by the chip after welding staying in the processing track for a long time.

[0055] Furthermore, the preset duration is 300 seconds.

[0056] That is, when it is detected that the welded chip stays in the processing track for more than 300 seconds, the welded chip is cleared out of the processing track. For example, the welded chip is directly pushed out of the processing track by tools such as telescopic rods and telescopic arms.

[0057] Furthermore, the packaging equipment is a soft solder die bonding machine.

[0058] Soft solder die bonder is mainly used for the placement and production of semiconductor chips for power devices / discrete devices. In the process of pasting chips and frames, this equipment usually uses soft solder to bond the chips to achieve conductive and thermal paths and reliable mechanical connections. The excellent reliability of soft solder is unmatched by other solders. In the solder die bond process of power devices, the die bonder needs to complete related processes such as heating, tinning, die bonding, and cooling for the lead frame to ensure the stability and reliability of the connection.

[0059] Furthermore, after pressing the target chip onto the surface of the solder layer at a preset pressure to obtain a soldered chip, the method further includes:

[0060] Monitor the time the chip stays in the processing track after soldering.

[0061] Specifically, the time that the chip stays in the processing track after welding can be determined by monitoring the time that each chip stays in the processing track after welding, and can also be indirectly determined by monitoring the downtime of the packaging equipment.

[0062] like Figure 5 As shown, further, the processing track 24 includes a tin dropping area 242, a film pressing area 243 and a welding area 244 which are sequentially arranged on the conveying track 241.

[0063] The bonding material is melted on the surface of the silver-plated layer to form a solder layer, and then the target chip is pressed on the surface of the solder layer to obtain a soldered chip, which specifically includes:

[0064] When the lead frame provided with the silver-plated layer reaches the tin-dropping area 242 , the tin solder formed by melting the die-bonding material at a preset temperature is dropped onto the surface of the silver-plated layer.

[0065] Among them, the preset temperature is set within 380±40°C, and the amount of solder dripped on the surface of the silver-plated layer can be adjusted through the packaging equipment according to the different target chips.

[0066] When the lead frame dripped with solder reaches the film pressing area 243, the solder is pressed into a preset solder pressing pattern to obtain a solder layer.

[0067] Among them, the type of tin pressing pattern can be adjusted through packaging equipment according to different target chips.

[0068] When the lead frame with the solder layer reaches the welding area 244, the target chip is pressed on the surface of the solder layer with a preset pressure to obtain a welded chip.

[0069] The size of the preset pressure can be adjusted through packaging equipment according to different target chips.

[0070] The embodiment of the present invention uses NT3210 chip package as the target chip, and the size of the target chip is 5660*4660um. 2 The target chip has a thickness of 100um, a package of TO-220FB-3L, a lead frame of TO-220FB-3L bare copper, and a lead frame size of 6800*5200um. 2 The bonding material is Pb92.5Sn2Ag2.5 leaded solder.

[0071] Since the size of the target chip is slightly different from that of the lead frame, and the solder fluidity of the bare copper frame is poor, solder climbing is likely to occur on the edge of the target chip after the soldering head of the packaging equipment is squeezed by the solder after bonding.

[0072] In order to solve this problem, firstly, a silver plating operation is performed on the bonding area of ​​the bare copper frame to obtain a lead frame provided with a silver-plated layer, and the size of the silver-plated layer is 6500*5200um. 2 .

[0073] Afterwards, use the soft solder die bonder as the packaging equipment, set the temperatures of the tin dropping area, die pressing area and welding area of ​​the working track of the soft solder die bonder to within 380±40℃, set the track dwell time to 300 seconds, and turn on the automatic track clearing function of the soft solder die bonder.

[0074] After completing the debugging of the soft solder die bonding machine, the bonding material is melted on the surface of the silver-plated layer in the working track of the soft solder die bonding machine to form a solder layer, and then the target chip is pressed on the surface of the solder layer to obtain the soldered chip, thus realizing the bonding operation.

[0075] During the chip bonding operation, monitor the time the chip stays in the working track after welding. When the stay time exceeds 300 seconds, all chips and lead frames in the working track are cleared out of the working track.

[0076] In actual application, the semiconductor chip packaging method for controlling solder creep provided by the embodiment of the present invention uses a bare copper frame as a lead frame, and sets a silver-plated layer on the chip bonding area of ​​the bare copper frame; then, in the processing track of the packaging equipment, the chip bonding material is melted on the surface of the silver-plated layer to form a solder layer, and the target chip is pressed on the solder layer to obtain a welded chip; the time the welded chip stays in the processing track is monitored, and when the stay time exceeds a preset time, the welded chip is cleared out of the processing track.

[0077] The silver-plated area can increase the fluidity of the solder melted from the adhesive material, allowing the solder at the edge of the target area to spread along the silver-plated layer and prevent the solder from climbing.

[0078] During the packaging process, the time that the chip stays in the processing track after welding is monitored, and the chip that stays for more than the preset time is promptly cleared out, thereby preventing the chip from staying in the working track for too long after welding and causing the solder to reflux for a long time, resulting in solder climbing.

[0079] The setting of the silver plating layer and the monitoring of the time the chip stays in the processing track after welding can effectively control the defect of solder climbing during the chip packaging process, greatly improving the packaging yield and reliability of chip products.

[0080] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A semiconductor chip packaging method for controlling solder creep height, characterized in that: include: A bare copper frame is used as a lead frame, and a silver-plated layer is provided on the chip bonding area of ​​the bare copper frame; the size of the silver-plated layer is larger than the size of the target chip; In a processing track of a packaging device filled with nitrogen and hydrogen mixed gas and operating at a preset temperature, the bonding material is melted on the surface of the silver-plated layer to form a solder layer, and then the target chip is pressed on the surface of the solder layer to obtain a soldered chip; After the welded chip stays in the processing track for a period exceeding a preset time, the welded chip is cleared out of the processing track.

2. The semiconductor chip packaging method for controlling solder creep according to claim 1, characterized in that: The length of the silver-plated layer is 300-1000um greater than the length of the target chip; The width of the silver-plated layer is 300-1000 um greater than the width of the target chip.

3. The semiconductor chip packaging method for controlling solder creep height according to claim 2, characterized in that: The preset duration is 300 seconds.

4. The semiconductor chip packaging method for controlling solder creep height according to claim 1, characterized in that: The preset temperature is within 380±40°C.

5. The semiconductor chip packaging method for controlling solder creep according to claim 1, characterized in that: The packaging equipment is a soft solder die bonder.

6. The semiconductor chip packaging method for controlling solder creep according to claim 1, characterized in that: The processing track includes a tin dropping area, a film pressing area and a welding area which are sequentially arranged on the conveying track; the bonding material is melted on the surface of the silver-plated layer to form a solder layer, and then the target chip is pressed on the surface of the solder layer to obtain a soldered chip, which specifically includes: When the lead frame provided with the silver-plated layer reaches the tin-dropping area, the tin solder formed by melting the adhesive material at the preset temperature is dropped onto the surface of the silver-plated layer; When the lead frame dripped with the solder reaches the film pressing area, the solder is pressed into a preset tin pressing pattern to obtain a solder layer; When the lead frame after obtaining the solder layer reaches the welding area, the target chip is pressed against the surface of the solder layer with a preset pressure to obtain a welded chip.

7. The semiconductor chip packaging method for controlling solder creep height according to claim 6, characterized in that: After pressing the target chip on the surface of the solder layer with a preset pressure to obtain a soldered chip, the method further includes: The time the chip stays in the processing track after welding is monitored.

8. The semiconductor chip packaging method for controlling solder creep according to claim 1, characterized in that: The bonding material is lead-containing solder.