Negative electrode interface coating process for solid-state battery
By adopting a specific proportion of electrolyte powder and hydrophilic modified conductive powder coating coating coating coating coating coating coating coating coating coating coating coating coating porosity problems are solved, significantly improving the retention rate and service life of the battery, and enhancing the Battery safety and stability.
Patent Information
- Application Number
- CN202411392539.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-29
AI Technical Summary
The metal lithium negative electrode material in solid-state batteries is prone to form lithium dendrites, resulting in safety hazards and shortened service life. Although aluminum is incorporated into solid electrolytes, it improves performance but increases the porosity of the coating and reduces density, which in turn affects the number of cycles of the battery.
A negative electrode interface coating process for solid-state batteries is adopted. By mixing electrolyte powder, hydrophilic modified conductive powder and binder in a specific proportion, a coating slurry is formed, and rolled on a metal lithium sheet is prepared after drying. The negative electrode is obtained, and the electrolyte powder is Li7-3xLa3Zr2AlxO12. The hydrophilic modified conductive powder is coated with a dense and uniform polymer through the surface of the nanocarbon black to enhance its hydrophilicity and dispersion.
The battery's cycling capacity retention rate is significantly improved for 50-week and 100-week cycles, extends the battery's service life, and improves the battery's safety and stability through synergistic effects.
Smart Images

Figure CN119050261A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a negative electrode interface coating process for solid-state batteries. Background Art
[0002] Solid-state batteries are a type of battery technology that uses solid electrolytes instead of traditional liquid electrolytes. Compared with traditional lithium-ion batteries, solid-state batteries show significant advantages in terms of safety and energy density. The energy density of solid-state batteries is several times that of traditional lithium-ion batteries, which means that more energy can be stored in the same volume. Since solid-state electrolytes are non-flammable, non-corrosive, and non-volatile, the safety performance of solid-state batteries is greatly enhanced. Solid-state batteries have a longer cycle life.
[0003] Metal lithium has the highest energy density as anode material, which can reach 2600-3500Wh / kg. However, direct use of metal lithium sheets has significant safety risks, mainly because metal lithium is prone to form lithium dendrites, which can cause short circuits and even fires. Therefore, materials with high shear modulus, such as some high-hardness solid electrolyte materials, can be selected for coating to improve the surface stability of lithium metal or lithium compound anodes, inhibit the growth of lithium dendrites, prevent lithium dendrites from penetrating, improve safety and cycle stability, and extend service life.
[0004] When selecting solid electrolyte materials, aluminum (Al) incorporation can improve the performance of solid electrolytes, such as increasing ionic conductivity and optimizing the microstructure of the material. However, at the same time, to a certain extent, it will lead to an increase in the porosity of the coating formed by the electrolyte powder and a decrease in the density, making it easier to be penetrated by lithium dendrites, resulting in a decrease in service life / cycle number. Summary of the invention
[0005] In order to solve the problems existing in the background technology, the present invention provides a negative electrode interface coating process for solid-state batteries, which can significantly improve the service life of the manufactured battery.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A negative electrode interface coating process for a solid-state battery comprises the following steps:
[0008] S1. Mix 25-28 parts of electrolyte powder, 2-3 parts of hydrophilic modified conductive powder, 8-10 parts of binder and 57-60 parts of water by weight to obtain a coating slurry;
[0009] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 5-6 mg / cm 2 ;
[0010] The electrolyte powder is Li7-3x La 3 Zr 2 Al x O 12 , where 0.3≤x≤0.5.
[0011] Furthermore, the preparation method of the electrolyte powder is as follows:
[0012] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H 2 O、Zr(NO 3 ) 4 ·5H 2 O and Al(NO 3 ) 3 , dissolved in deionized water until the solution is transparent to obtain a nitrate solution;
[0013] A2, add citric acid to the nitrate solution obtained in A1, stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry to obtain a brown xerogel;
[0014] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 700-750°C for 4.5-5.5h in an air atmosphere to obtain electrolyte powder.
[0015] Furthermore, in A1, LiNO 3 Overdose 4-6%.
[0016] Further, in A2, the amount of citric acid is LiNO 3 、La(NO 3 ) 3 6H 2 O、Zr(NO 3 ) 4 ·5H 2 O and Al(NO 3 ) 3 Twice the total amount of the substance.
[0017] Furthermore, in A2, the drying treatment is: drying in a forced air drying oven at 160° C. for 12 h.
[0018] Furthermore, the preparation method of the hydrophilic modified conductive powder is as follows:
[0019] B1. Add 1 g of conductive powder into 250 mL of deionized water and stir at a stirring rate of 200 r / min for 20 min to obtain a powder-water slurry;
[0020] B2. Add 1 g of catechol and 4 g of diethylenetriamine into 250 mL of deionized water, shake and mix to obtain a modified solution;
[0021] B3. Pour the powder-water slurry obtained in B1 into the modified solution obtained in B2, adjust the pH to 8-10, continue stirring the reaction at 200 r / min at 20°C for 4.5-5.5 hours, then wash and dry to obtain the hydrophilic modified conductive powder.
[0022] Furthermore, the conductive powder is nano carbon black.
[0023] Furthermore, in B3, Tris-HCl buffer was used to adjust the pH.
[0024] Furthermore, the binder includes polyvinyl alcohol or polyacrylamide.
[0025] This application has the following beneficial effects:
[0026] 1. The hydrophilic modified conductive powder is introduced into the coating slurry for the negative electrode interface coating of the solid-state battery of the present invention, which can significantly improve the capacity retention rate of the battery after 50 cycles and 100 cycles; on this basis (the coating slurry contains the hydrophilic modified conductive powder), Al is introduced into the electrolyte powder, that is, the electrolyte powder is composed of Li 5.8 La 3 Zr 2 O 12 Replaced by Li 5.8 La 3 Zr 2 Al 0.4 O 12 , and can work synergistically with the hydrophilic modified conductive powder to further improve the capacity retention rate of the battery after 50 and 100 cycles.
[0027] 2. The incorporation of Al in the present invention increases the porosity of the coating formed by the electrolyte powder and reduces the density; while a dense, uniform, and permanent hydrophilic polymer is coated on the surface of the nano-carbon black to obtain a hydrophilic modified conductive powder, which can increase the hydrophilic functional groups on the surface of the nano-carbon black, so that the nano-carbon black has excellent hydrophilicity and exhibits good dispersibility and stability in an aqueous environment, thereby better filling the pores of the coating and increasing the density; the two work synergistically to achieve the effect of synergistically improving the service life of the obtained battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 , a trend chart showing the comparison of the capacity retention test data of the batteries prepared in Examples 1-6 of the present invention and Comparative Examples 1-5 after 50 and 100 cycles. DETAILED DESCRIPTION
[0029] The present application is further described in detail below in conjunction with embodiments.
[0030] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.
[0031] Example 1: (1) Preparation of electrolyte powder, the electrolyte powder is Li 5.8 La 3 Zr 2 Al 0.4 O 12 , and its preparation method is as follows:
[0032] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H 2 O、Zr(NO 3 ) 4 ·5H 2 O and Al(NO 3 ) 3 On this basis, LiNO 3 Weigh out 5% excess; dissolve all in deionized water until the solution is transparent to obtain a nitrate solution.
[0033] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry in a forced air drying oven at 160°C for 12 hours to obtain a brown xerogel.
[0034] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 720°C for 5 h in an air atmosphere to obtain electrolyte powder.
[0035] Among them, lithium nitrate LiNO 3 , purchased from Hubei Kewode Chemical Co., Ltd. Lanthanum nitrate hexahydrate La(NO 3 ) 3 6H 2 O, effective ingredient 99%, purchased from Shandong New Kinetic Energy Chemical Co., Ltd. Zirconium nitrate pentahydrate Zr(NO 3 ) 4 ·5H 2 O, purchased from Shandong Desheng New Materials Co., Ltd. Aluminum nitrate Al(NO 3 ) 3 , purchased from Langfang Pengcai Fine Chemical Co., Ltd. Anhydrous citric acid (superior grade) was purchased from Henan Mingzhixin Chemical Products Co., Ltd.
[0036] (2) Prepare hydrophilic modified conductive powder, the preparation method is as follows:
[0037] B1. Add 1 g of nano carbon black into 250 mL of deionized water and stir at a stirring rate of 200 r / min for 20 min to obtain a powder-water slurry;
[0038] B2. Add 1 g of catechol and 4 g of diethylenetriamine into 250 mL of deionized water, shake and mix to obtain a modified solution;
[0039] B3. Pour the powder slurry obtained in B1 into the modified solution obtained in B2, add Tris-HCl buffer, adjust the pH to about 9.0, continue stirring the reaction at 200 r / min at 20°C for 5 hours, then wash and dry to obtain the hydrophilic modified conductive powder.
[0040] Among them, nano carbon black (BC-80, content 99.7%) was purchased from Tianjin Baochi Chemical Technology Co., Ltd. Catechol was purchased from Jinan Huifengda Chemical Co., Ltd. Diethylenetriamine was purchased from Jiangsu Pules Biotechnology Co., Ltd. Tris-HCl buffer can be prepared according to actual needs, and the product used here was purchased from Qingdao Kester Biotechnology Co., Ltd.
[0041] (3) Anode interface coating process for solid-state batteries, comprising the following steps:
[0042] S1. Mix 26 parts of electrolyte powder, 2.5 parts of hydrophilic modified conductive powder, 9 parts of polyvinyl alcohol and 58 parts of water by weight to obtain a coating slurry.
[0043] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 5.5 mg / cm 2 .
[0044] Among them, polyvinyl alcohol (brand Japanese Kuraray), brand PVA-205, property level adhesive 1788, was purchased from Dongguan Yingxiang Plastic Raw Materials Co., Ltd.
[0045] According to the battery assembly process, the negative electrode, solid electrolyte and positive electrode are assembled into a battery. Among them, the negative electrode is the negative electrode for solid-state battery prepared by the above method. Preparation of solid electrolyte: weigh 0.6g of basic electrolyte powder (Li 5.8 La 3 Zr 2 O 12) was ground in an agate mortar for 10 minutes to obtain a powder with uniform particles, and then the powder was loaded into a mold with a diameter of 13 mm and pressed into a blank using a tablet press. The blank disc obtained was pressed into a compact blank at 250 MPa, and then placed in an alumina crucible covered with a layer of mother powder of the same composition. The compact blank was covered with another layer of mother powder to form a lithium-rich sintering atmosphere, and sintered at 1050 ° C for 10 hours. After sintering, the mother powder was scraped off and the surface was polished with 1000# sandpaper until it was smooth. Aluminum foil was used as the positive electrode substrate.
[0046] Example 2: The difference between this example and example 1 is that the electrolyte powder is Li 6.1 La 3 Zr 2 Al 0.3 O 12 .
[0047] Specifically, (1) preparing electrolyte powder, the electrolyte powder is Li 6.1 La 3 Zr 2 Al 0.3 O 12 , and its preparation method is as follows:
[0048] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H 2 O、Zr(NO 3 ) 4 ·5H 2 O and Al(NO 3 ) 3 On this basis, LiNO 3 Weigh out 4% excess; dissolve all in deionized water until the solution is transparent to obtain a nitrate solution.
[0049] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry in a forced air drying oven at 160°C for 12 hours to obtain a brown xerogel.
[0050] A3. Using a tubular furnace, the dry gel obtained in A2 was calcined at 700° C. for 4.5 h in an air atmosphere to obtain electrolyte powder.
[0051] (2) Prepare hydrophilic modified conductive powder, the preparation method is as follows:
[0052] B1. Add 1 g of nano carbon black into 250 mL of deionized water and stir at a stirring rate of 200 r / min for 20 min to obtain a powder-water slurry;
[0053] B2. Add 1 g of catechol and 4 g of diethylenetriamine into 250 mL of deionized water, shake and mix to obtain a modified solution;
[0054] B3. Pour the powder slurry obtained in B1 into the modified solution obtained in B2, add Tris-HCl buffer, adjust the pH to about 9.0, continue stirring the reaction at 200 r / min at 20°C for 5 hours, then wash and dry to obtain the hydrophilic modified conductive powder.
[0055] (3) Anode interface coating process for solid-state batteries, comprising the following steps:
[0056] S1. Mix 26 parts of electrolyte powder, 2.5 parts of hydrophilic modified conductive powder, 9 parts of polyvinyl alcohol and 58 parts of water by weight to obtain a coating slurry.
[0057] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 5.5 mg / cm 2 .
[0058] Example 3: The difference between this example and example 1 is that the electrolyte powder is Li 5.5 La 3 Zr 2 Al 0.5 O 12 .
[0059] Specifically, (1) preparing electrolyte powder, the electrolyte powder is Li 5.5 La 3 Zr 2 Al 0.5 O 12 , and its preparation method is as follows:
[0060] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H 2 O、Zr(NO 3 ) 4 ·5H 2 O and Al(NO 3 ) 3 On this basis, LiNO 3 Weigh out an excess of 6%; dissolve all of it in deionized water until the solution is transparent to obtain a nitrate solution.
[0061] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry in a forced air drying oven at 160°C for 12 hours to obtain a brown xerogel.
[0062] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 750°C for 5.5 h in an air atmosphere to obtain electrolyte powder.
[0063] (2) Prepare hydrophilic modified conductive powder, the preparation method is as follows:
[0064] B1. Add 1 g of nano carbon black into 250 mL of deionized water and stir at a stirring rate of 200 r / min for 20 min to obtain a powder-water slurry;
[0065] B2. Add 1 g of catechol and 4 g of diethylenetriamine into 250 mL of deionized water, shake and mix to obtain a modified solution;
[0066] B3. Pour the powder slurry obtained in B1 into the modified solution obtained in B2, add Tris-HCl buffer, adjust the pH to about 9.0, continue stirring the reaction at 200 r / min at 20°C for 5 hours, then wash and dry to obtain the hydrophilic modified conductive powder.
[0067] (3) Anode interface coating process for solid-state batteries, comprising the following steps:
[0068] S1. Mix 26 parts of electrolyte powder, 2.5 parts of hydrophilic modified conductive powder, 9 parts of polyvinyl alcohol and 58 parts of water by weight to obtain a coating slurry.
[0069] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 5.5 mg / cm 2 .
[0070] Example 4: The difference between this example and Example 1 is that 25 parts of electrolyte powder, 2 parts of hydrophilic modified conductive powder, 8 parts of polyvinyl alcohol and 57 parts of water are mixed to obtain a coating slurry.
[0071] Specifically, (1) preparing electrolyte powder, the electrolyte powder is Li 5.8 La 3 Zr 2 Al 0.4 O 12 , and its preparation method is as follows:
[0072] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H2 O、Zr(NO 3 ) 4 ·5H 2 O and Al(NO 3 ) 3 On this basis, LiNO 3 Weigh out 5% excess; dissolve all in deionized water until the solution is transparent to obtain a nitrate solution.
[0073] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry in a forced air drying oven at 160°C for 12 hours to obtain a brown xerogel.
[0074] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 720°C for 5 h in an air atmosphere to obtain electrolyte powder.
[0075] (2) Prepare hydrophilic modified conductive powder, the preparation method is as follows:
[0076] B1. Add 1 g of nano carbon black into 250 mL of deionized water and stir at a stirring rate of 200 r / min for 20 min to obtain a powder-water slurry;
[0077] B2. Add 1 g of catechol and 4 g of diethylenetriamine into 250 mL of deionized water, shake and mix to obtain a modified solution;
[0078] B3. Pour the powder slurry obtained in B1 into the modified solution obtained in B2, add Tris-HCl buffer, adjust the pH to about 9.0, continue stirring the reaction at 200 r / min at 20°C for 5 hours, then wash and dry to obtain the hydrophilic modified conductive powder.
[0079] (3) Anode interface coating process for solid-state batteries, comprising the following steps:
[0080] S1. Mix 25 parts of electrolyte powder, 2 parts of hydrophilic modified conductive powder, 8 parts of polyvinyl alcohol and 57 parts of water by weight to obtain a coating slurry.
[0081] S2. Roll the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery with a surface loading of 5 mg / cm 2 .
[0082] Example 5: The difference between this example and Example 1 is that 28 parts of electrolyte powder, 3 parts of hydrophilic modified conductive powder, 10 parts of polyvinyl alcohol and 60 parts of water are mixed to obtain a coating slurry.
[0083] Specifically, (1) preparing electrolyte powder, the electrolyte powder is Li5.8 La 3 Zr 2 Al 0.4 O 12 , and its preparation method is as follows:
[0084] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H 2 O、Zr(NO 3 ) 4 ·5H 2 O and Al(NO 3 ) 3 On this basis, LiNO 3 Weigh out 5% excess; dissolve all in deionized water until the solution is transparent to obtain a nitrate solution.
[0085] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry in a forced air drying oven at 160°C for 12 hours to obtain a brown xerogel.
[0086] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 720°C for 5 h in an air atmosphere to obtain electrolyte powder.
[0087] (2) Prepare hydrophilic modified conductive powder, the preparation method is as follows:
[0088] B1. Add 1 g of nano carbon black into 250 mL of deionized water and stir at a stirring rate of 200 r / min for 20 min to obtain a powder-water slurry;
[0089] B2. Add 1 g of catechol and 4 g of diethylenetriamine into 250 mL of deionized water, shake and mix to obtain a modified solution;
[0090] B3. Pour the powder slurry obtained in B1 into the modified solution obtained in B2, add Tris-HCl buffer, adjust the pH to about 9.0, continue stirring the reaction at 200 r / min at 20°C for 5 hours, then wash and dry to obtain the hydrophilic modified conductive powder.
[0091] (3) Anode interface coating process for solid-state batteries, comprising the following steps:
[0092] S1. Mix 28 parts of electrolyte powder, 3 parts of hydrophilic modified conductive powder, 10 parts of polyvinyl alcohol and 60 parts of water by weight to obtain a coating slurry.
[0093] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 6 mg / cm 2 .
[0094] Example 6: The difference between this example and Example 1 is that 27 parts of electrolyte powder, 2.5 parts of hydrophilic modified conductive powder, 9 parts of polyvinyl alcohol and 59 parts of water are mixed to obtain a coating slurry.
[0095] Specifically, (1) preparing electrolyte powder, the electrolyte powder is Li 5.8 La 3 Zr 2 Al 0.4 O 12 , and its preparation method is as follows:
[0096] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H 2 O、Zr(NO 3 ) 4 ·5H 2 O and Al(NO 3 ) 3 On this basis, LiNO 3 Weigh out 5% excess; dissolve all in deionized water until the solution is transparent to obtain a nitrate solution.
[0097] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry in a forced air drying oven at 160°C for 12 hours to obtain a brown xerogel.
[0098] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 720°C for 5 h in an air atmosphere to obtain electrolyte powder.
[0099] (2) Prepare hydrophilic modified conductive powder, the preparation method is as follows:
[0100] B1. Add 1 g of nano carbon black into 250 mL of deionized water and stir at a stirring rate of 200 r / min for 20 min to obtain a powder-water slurry;
[0101] B2. Add 1 g of catechol and 4 g of diethylenetriamine into 250 mL of deionized water, shake and mix to obtain a modified solution;
[0102] B3. Pour the powder slurry obtained in B1 into the modified solution obtained in B2, add Tris-HCl buffer, adjust the pH to about 9.0, continue stirring the reaction at 200 r / min at 20°C for 5 hours, then wash and dry to obtain the hydrophilic modified conductive powder.
[0103] (3) Anode interface coating process for solid-state batteries, comprising the following steps:
[0104] S1. Mix 27 parts of electrolyte powder, 2.5 parts of hydrophilic modified conductive powder, 9 parts of polyvinyl alcohol and 59 parts of water by weight to obtain a coating slurry.
[0105] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 6 mg / cm 2 .
[0106] Comparative Example 1: The difference between this comparative example and Example 1 is that: there is no Al in the electrolyte powder; and there is no hydrophilic modified conductive powder in the coating slurry.
[0107] Specifically, electrolyte powder is prepared, and the electrolyte powder is Li 5.8 La 3 Zr 2 O 12 , and its preparation method is as follows:
[0108] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H 2 O and Zr(NO 3 ) 4 ·5H 2 O, on this basis, LiNO 3 Weigh out 5% excess; dissolve all in deionized water until the solution is transparent to obtain a nitrate solution.
[0109] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and dry in a forced air drying oven at 160°C for 12 hours to obtain a xerogel.
[0110] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 720°C for 5 h in an air atmosphere to obtain electrolyte powder.
[0111] The negative electrode interface coating process for solid-state batteries includes the following steps:
[0112] S1. Mix 26 parts of electrolyte powder, 9 parts of polyvinyl alcohol and 58 parts of water by weight to obtain a coating slurry.
[0113] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 5.5 mg / cm 2 .
[0114] Comparative Example 2: The difference between this comparative example and Example 1 is that: there is no Al in the electrolyte powder; and the hydrophilic modified conductive powder is replaced by graphite.
[0115] Specifically, electrolyte powder is prepared, and the electrolyte powder is Li 5.8 La 3 Zr 2 O 12 , and its preparation method is as follows:
[0116] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H 2 O and Zr(NO 3 ) 4 ·5H 2 O, on this basis, LiNO 3 Weigh out 5% excess; dissolve all in deionized water until the solution is transparent to obtain a nitrate solution.
[0117] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry in a forced air drying oven at 160°C for 12 hours to obtain a brown xerogel.
[0118] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 720°C for 5 h in an air atmosphere to obtain electrolyte powder.
[0119] The negative electrode interface coating process for solid-state batteries includes the following steps:
[0120] S1. Mix 26 parts of electrolyte powder, 2.5 parts of graphite, 9 parts of polyvinyl alcohol and 58 parts of water by weight to obtain a coating slurry.
[0121] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 5.5 mg / cm 2 .
[0122] Comparative Example 3: The difference between this comparative example and Example 1 is that: there is no Al in the electrolyte powder; and the hydrophilic modified conductive powder is replaced by nano carbon black.
[0123] Specifically, the electrolyte powder is prepared, and the electrolyte powder is Li 5.8La 3 Zr 2 O 12 , and its preparation method is as follows:
[0124] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H 2 O and Zr(NO 3 ) 4 ·5H 2 O, on this basis, LiNO 3 Weigh out 5% excess; dissolve all in deionized water until the solution is transparent to obtain a nitrate solution.
[0125] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry in a forced air drying oven at 160°C for 12 hours to obtain a brown xerogel.
[0126] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 720°C for 5 h in an air atmosphere to obtain electrolyte powder.
[0127] The negative electrode interface coating process for solid-state batteries includes the following steps:
[0128] S1. Mix 26 parts of electrolyte powder, 2.5 parts of nano carbon black, 9 parts of polyvinyl alcohol and 58 parts of water by weight to obtain a coating slurry.
[0129] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 5.5 mg / cm 2 .
[0130] Comparative Example 4: The difference between this comparative example and Example 1 is that there is no Al in the electrolyte powder.
[0131] Specifically, (1) preparing electrolyte powder, the electrolyte powder is Li 5.8 La 3 Zr 2 O 12 , and its preparation method is as follows:
[0132] A1. Weigh LiNO according to the stoichiometric ratio 3 、La(NO 3 ) 3 6H 2 O and Zr(NO 3 ) 4 ·5H 2 O, on this basis, LiNO3 Weigh out 5% excess; dissolve all in deionized water until the solution is transparent to obtain a nitrate solution.
[0133] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry in a forced air drying oven at 160°C for 12 hours to obtain a brown xerogel.
[0134] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 720°C for 5 h in an air atmosphere to obtain electrolyte powder.
[0135] (2) Prepare hydrophilic modified conductive powder, the preparation method is as follows:
[0136] B1. Add 1 g of nano carbon black into 250 mL of deionized water and stir at a stirring rate of 200 r / min for 20 min to obtain a powder-water slurry;
[0137] B2. Add 1 g of catechol and 4 g of diethylenetriamine into 250 mL of deionized water, shake and mix to obtain a modified solution;
[0138] B3. Pour the powder slurry obtained in B1 into the modified solution obtained in B2, add Tris-HCl buffer, adjust the pH to about 9.0, continue stirring the reaction at 200 r / min at 20°C for 5 hours, then wash and dry to obtain the hydrophilic modified conductive powder.
[0139] (3) Anode interface coating process for solid-state batteries, comprising the following steps:
[0140] S1. Mix 26 parts of electrolyte powder, 2.5 parts of hydrophilic modified conductive powder, 9 parts of polyvinyl alcohol and 58 parts of water by weight to obtain a coating slurry.
[0141] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 5.5 mg / cm 2 .
[0142] Comparative Example 5: The difference between this comparative example and Example 1 is that there is no hydrophilic modified conductive powder in the coating slurry.
[0143] Specifically, an electrolyte powder is prepared, wherein the electrolyte powder is Li 5.8 La 3 Zr 2 Al 0.4 O 12 , and its preparation method is as follows:
[0144] A1. Weigh LiNO according to the stoichiometric ratio 3、La(NO 3 ) 3 6H 2 O、Zr(NO 3 ) 4 ·5H 2 O and Al(NO 3 ) 3 On this basis, LiNO 3 Weigh out 5% excess; dissolve all in deionized water until the solution is transparent to obtain a nitrate solution.
[0145] A2. Add citric acid to the nitrate solution obtained in A1, the amount of citric acid used being twice the total amount of all nitrate substances; stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry in a forced air drying oven at 160°C for 12 hours to obtain a brown xerogel.
[0146] A3. Use a tubular furnace to calcine the dry gel obtained in A2 at 720°C for 5 h in an air atmosphere to obtain electrolyte powder.
[0147] The negative electrode interface coating process for solid-state batteries includes the following steps:
[0148] S1. Mix 26 parts of electrolyte powder, 9 parts of polyvinyl alcohol and 58 parts of water by weight to obtain a coating slurry.
[0149] S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 5.5 mg / cm 2 .
[0150] Test example: Test object: Batteries prepared in Examples 1-6 and Comparative Examples 1-5.
[0151] Test content: Under the conditions of 60℃ and 0.2C, the capacity retention rate of each test object was tested for 50 and 100 cycles.
[0152] Test results: See Table 1.
[0153] Table 1. Test data of the experimental example
[0154]
[0155] Result analysis: Analyze examples 1-6 and combine the data in Table 1 and Figure 1 It can be seen that the capacity retention rate of the battery produced by the present invention is as high as over 94.8% after 50 cycles, and the capacity retention rate after 100 cycles is as high as over 91.9%.
[0156] Analyze Comparative Examples 1-4 and combine the data in Table 1 and Figure 1 It can be seen that the electrolyte powder does not contain Al (the electrolyte powder is Li5.8 La 3 Zr 2 O 12 ), adding graphite to the coating slurry slightly improved the capacity retention rate of the battery after 50 and 100 cycles. Adding nano carbon black to the coating slurry significantly improved the capacity retention rate of the battery after 50 and 100 cycles; using the nano carbon black as the hydrophilic modified conductive powder of the present invention, the capacity retention rate of the battery after 50 and 100 cycles was further improved.
[0157] Analyze Comparative Example 1 and Comparative Example 5 and combine the data in Table 1 and Figure 1 It can be seen that when there is no hydrophilic modified conductive powder in the coating slurry, Al is introduced into the electrolyte powder, that is, the electrolyte powder is composed of Li 5.8 La 3 Zr 2 O 12 Replaced by Li 5.8 La 3 Zr 2 Al 0.4 O 12 The capacity retention rate of the battery after 50 and 100 cycles was reduced.
[0158] Analyze Example 1, Comparative Example 1, Comparative Example 4 and Comparative Example 5 and combine the data in Table 1 and Figure 1 It can be seen that the introduction of hydrophilic modified conductive powder into the coating slurry significantly improves the capacity retention rate of the battery after 50 and 100 cycles. On this basis (the coating slurry contains hydrophilic modified conductive powder), Al is introduced into the electrolyte powder, that is, the electrolyte powder is composed of Li 5.8 La 3 Zr 2 O 12 Replaced by Li 5.8 La 3 Zr 2 Al 0.4 O 12 The two work synergistically to further improve the capacity retention rate of the battery after 50 and 100 cycles.
[0159] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0160] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A negative electrode interface coating process for solid-state batteries, characterized in that: The steps include: S1. Mix 25-28 parts of electrolyte powder, 2-3 parts of hydrophilic modified conductive powder, 8-10 parts of binder and 57-60 parts of water by weight to obtain a coating slurry; S2, roll-coat the coating slurry obtained in S1 onto the metal lithium sheet and dry it to obtain the negative electrode for solid-state battery, with a surface loading of 5-6 mg / cm 2 ; The electrolyte powder is Li 7-3x La3Zr2Al x O 12 , where 0.3≤x≤0.
5.
2. The negative electrode interface coating process for solid-state batteries according to claim 1, characterized in that: The preparation method of the electrolyte powder is as follows: A1. Weigh LiNO3, La(NO3)3·6H2O, Zr(NO3)4·5H2O and Al(NO3)3 according to the stoichiometric ratio and dissolve them in deionized water to obtain a nitrate solution; A2, add citric acid to the nitrate solution obtained in A1, stir in a 60°C water bath until it becomes a transparent sol, age at room temperature for 20 hours, and then dry to obtain a xerogel; A3. Calcine the dry gel obtained in A2 at 700-750°C for 4.5-5.5h to obtain electrolyte powder.
3. The negative electrode interface coating process for solid-state batteries according to claim 2, characterized in that: In A1, LiNO3 is in excess of 4-6%.
4. The negative electrode interface coating process for solid-state batteries according to claim 2, characterized in that: In A2, the amount of citric acid used is twice the total amount of LiNO3, La(NO3)3·6H2O, Zr(NO3)4·5H2O and Al(NO3)3.
5. The negative electrode interface coating process for solid-state batteries according to claim 2, characterized in that: In A2, the drying treatment is: drying in a forced air drying oven at 160°C for 12 hours.
6. The negative electrode interface coating process for solid-state batteries according to claim 1, characterized in that: The preparation method of the hydrophilic modified conductive powder is as follows: B1. Add 1 g of conductive powder into 250 mL of deionized water and stir at a stirring rate of 200 r / min for 20 min to obtain a powder-water slurry; B2. Add 1 g of catechol and 4 g of diethylenetriamine into 250 mL of deionized water, shake and mix to obtain a modified solution; B3. Pour the powder-water slurry obtained in B1 into the modified solution obtained in B2, adjust the pH to 8-10, continue stirring the reaction at 200 r / min at 20°C for 4.5-5.5 hours, then wash and dry to obtain the hydrophilic modified conductive powder.
7. The negative electrode interface coating process for solid-state batteries according to claim 6, characterized in that: The conductive powder is nano carbon black.
8. The negative electrode interface coating process for solid-state batteries according to claim 6, characterized in that: In B3, the pH was adjusted using Tris-HCl buffer. The negative electrode interface coating process for solid-state batteries according to claim 1 is characterized in that: The binder includes polyvinyl alcohol or polyacrylamide.