Fluorine-doped phosphorus-carbon composite negative electrode material and preparation method thereof

By building a polar interface on the porous carbon surface and introducing fluorine atoms to form a C-F-P structure, the problem of insufficient Coulomb efficiency and cycling performance of the negative electrode material of sodium ion battery is solved, and efficient preparation of phosphorus-carbon composite materials is achieved, which improves the energy of the battery Density and cyclic stability.

CN119050302AActive Publication Date: 2024-11-29INST OF CHEM CHINESE ACAD OF SCI

Patent Information

Application Number
CN202411147424.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing sodium ion battery anode materials have problems such as low efficiency, insufficient capacity, insufficient circulation performance and poor rate performance for the first time, especially in the capacity attenuation caused by volume expansion and sodium polyphosphide dissolution shuttle in phosphorus carbon materials.

Method used

By constructing a polar interface on the porous carbon surface, introducing fluorine atoms and forming a C-F-P structure, the continuous dense composite structure of fluoride carbon and carbon buffers the volume expansion of phosphorus, and increasing the interaction force between phosphorus and carbon substrate, it is prepared with high Coulomb efficiency and cycle stability phosphorus carbon composite material.

Benefits of technology

It significantly improves the Coulomb efficiency and reversible capacity of sodium ion batteries, enhances the cyclic stability of the material, and simplifies the preparation process, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050302A_ABST
    Figure CN119050302A_ABST
Patent Text Reader

Abstract

The invention provides a fluorine-doped phosphorus-carbon composite negative electrode material, which is composed of elemental phosphorus and a fluorine-doped porous carbon substrate, the content of carbon fluoride in the fluorine-doped porous carbon substrate from the surface layer to the interior is gradually reduced, and the X-ray photoelectron spectroscopy (XPS spectrogram) of the F element has characteristic peaks of 687.2 + / -0.1 eV and 685.5 + / -0.1 eV. The composite material is composed of elemental phosphorus and a porous carbon substrate, wherein the porous carbon is composed of carbon and carbon fluoride. Fluorine atoms are introduced into porous carbon, a carbon and carbon fluoride structure is constructed, the carbon content from the surface layer to the interior of the porous carbon material is gradually increased, and the carbon fluoride content is gradually reduced. The introduction of fluorine successfully constructs a polar interface on the surface of the material, and in the battery cycle process, the polar interface effectively improves the adsorption of the material to sodium polyphosphide and inhibits the dissolution and shuttling of the sodium polyphosphide, thereby effectively improving the cycle performance of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a phosphorus-carbon composite material and a preparation method thereof, and in particular to a fluorine-doped phosphorus-carbon composite negative electrode material and a preparation method thereof. Background Art

[0002] With the demand for large-scale energy storage, secondary batteries with high energy density and low price have developed rapidly. Sodium-ion batteries have become an inevitable choice in the context of lithium resource shortage, sharp price increase and strong demand for energy storage due to their advantages such as abundant resources, wide distribution, low cost and good safety. And with the growth of demand for high energy density, sodium-ion batteries are developing towards higher energy density. Most of the commercialized sodium-ion batteries currently use sodium vanadium phosphate / hard carbon system. Due to the low theoretical capacity of the electrode itself, the battery energy density cannot be greatly improved. Generally speaking, the energy density of sodium-ion batteries is determined by the specific capacity of the positive and negative electrode materials and other components of the battery. Among them, the specific capacity of the positive and negative electrode materials is the key to improving the energy density of sodium-ion batteries. Based on this, it is urgent to develop new high-capacity positive and negative electrode materials for sodium-ion batteries.

[0003] Among the negative electrode materials for sodium ion batteries currently developed, hard carbon materials are favored for their low sodium storage point, low cost and environmental protection, stable structure, good charge and discharge cycle performance, and high safety performance. They are considered to be the most likely negative electrode materials for sodium ion batteries to be commercialized on a large scale. However, hard carbon materials also have the characteristics of low first coulombic efficiency, insufficient capacity, insufficient long cycle performance, and poor rate performance. Therefore, it is urgent to develop a negative electrode material for sodium ion batteries with high capacity and high first coulombic efficiency, which can take into account both first coulombic efficiency and cycle performance while obtaining high capacity. As a type of negative electrode material for sodium ion batteries, phosphorus-carbon negative electrode materials have the advantages of abundant resources, low cost, high capacity, good air stability, excellent rate performance, moderate working potential and flame retardancy. They are also considered to be negative electrode materials that surpass hard carbon in terms of energy density. The application of phosphorus-carbon to the negative electrode of sodium ion batteries, just as silicon-carbon is applied to the negative electrode of lithium ion batteries, can effectively improve the energy density of sodium ion batteries. However, phosphorus still cannot avoid huge volume expansion during the process of sodium insertion and extraction, and due to the huge solvation energy of the electrolyte, sodium polyphosphides dissolve and shuttle during the cycle, resulting in a large attenuation of capacity. Based on this, people use various methods to improve the cyclability of phosphorus-carbon negative electrode materials. Porous carbon materials have rich pore structures, which can provide buffer space for the volume expansion of phosphorus and effectively improve the cycle stability of phosphorus-carbon negative electrode materials. Another effective way is to construct a polar interface on the surface of the phosphorus-carbon negative electrode material, improve the adsorption of sodium polyphosphides through the polar interface, effectively inhibit its dissolution and shuttle, and thus improve the material cycle performance. Therefore, the development of a phosphorus-carbon negative electrode material with both a spatial buffer structure and a polar interface is the key to solving the problem of insufficient material cycle performance. The buffer space can effectively alleviate the volume expansion of phosphorus during the charge and discharge process, and the polar interface increases the interaction between phosphorus and the carbon substrate, reducing the shedding of the material. This application is based on the above two key scientific issues. By constructing a polar interface on the porous carbon surface, introducing fluorine atoms, and then depositing phosphorus, a stable CFP structure is formed. The pores of the porous carbon can effectively buffer the volume expansion of phosphorus. The formed CFP structure can enhance the interaction between phosphorus and the carbon substrate, ultimately achieving the purpose of improving the recycling performance of the material.

[0004] CN115832264A discloses a phosphorus-carbon composite material, which is composed of carbon balls and red phosphorus filled in the carbon balls; CN117673304A discloses a phosphorus-carbon composite material, which is obtained by depositing a phosphorus source on a carbon source by vapor deposition; CN116759556A discloses a phosphorus-carbon composite material, which is obtained by pre-activating phosphorus and carbon after mixing, and then mixing and crushing the slurry with water and a dispersant and subjecting it to a series of treatments. Phosphorus-carbon composite materials are reported in many prior art, but there are few reports that take into account both the spatial buffer structure and the polar carbon interface. There are also reports of fluorine doping of carbon sources in the prior art, such as CN115036519A. F doping can modify the pore density and hydrophilicity of carbon materials of different scales to a certain extent, but there is no report on the formation of stable chemical bonds between fluorine and phosphorus. CN117832462A discloses a fluorine-doped carbon-loaded red phosphorus material, which is a carbon material obtained by carbonizing a polymer obtained from urea and p-phenylene diisocyanate, and mechanically grinding with polytetrafluoroethylene to obtain a mixture, sintering under an inert atmosphere to obtain a fluorine-doped carbon nanosheet, and then infiltrating red phosphorus into the carbon nanosheet by evaporation-condensation to obtain a fluorine-doped carbon-loaded red phosphorus material. This patent simultaneously performs fluorine doping and phosphorus-carbon composite, but lacks a clear understanding of the construction design of the spatial buffer structure and the chemical structure between carbon and fluorine, and the preparation method is complicated. Summary of the invention

[0005] In view of the above technical problems, the present invention provides a phosphorus-carbon negative electrode material with a polar interface and a preparation method thereof, in which a porous carbon substrate uses a dual-temperature zone heating furnace to pyrolyze the introduced fluorine-containing substance to produce a fluorine-active component, so that the fluorine-active component and the porous carbon undergo a thermal reaction, so that fluorinated carbon is formed in situ on the surface, and the fluorinated carbon and carbon form a continuous and dense composite structure. Subsequently, the fluorinated porous carbon is used to load phosphorus to prepare a phosphorus-carbon negative electrode material as a negative electrode material for use in sodium ion batteries, which can effectively improve the coulombic efficiency and reversible capacity of the battery, and make the battery have a more excellent cycle stability. Moreover, the phosphorus-carbon negative electrode material is simple to prepare, easy to industrialize, and has broad application prospects.

[0006] In order to achieve the above-mentioned purpose of the invention, the present invention provides a fluorine-doped phosphorus-carbon composite negative electrode material, which is composed of elemental phosphorus and a fluorine-doped porous carbon substrate. The fluorinated carbon content gradually decreases from the surface layer to the interior of the fluorine-doped porous carbon substrate, and the X-ray photoelectron energy spectrum (XPS spectrum) of the F element has characteristic peaks of 687.2±0.1eV and 685.5±0.1eV.

[0007] The total mass of the phosphorus-carbon composite material is 100%, wherein the mass percentage of carbon is 20-40%, the mass percentage of phosphorus is 40-60%, and the mass percentage of fluorine is 2-7%.

[0008] The phosphorus-carbon composite material can be in the form of powder, block, fiber, etc., and the median particle size of the powder is 1-10 μm.

[0009] Furthermore, the porous carbon material is selected from at least one of spherical activated carbon, activated carbon fiber, mesoporous carbon, carbon nanotubes, carbon molecular sieves, carbon aerogels, carbon nanocages, porous carbon microspheres, columnar activated carbon, granular activated carbon, powdered activated carbon, expanded graphite, porous graphite, MOFs material, and biomass carbon.

[0010] Furthermore, the specific surface area of ​​the porous carbon material is 800-1500m 2 / g, the pores include micropores, mesopores and macropores; the pore size distribution of micropores is >0 to 2nm, the pore size distribution of mesopores is >2 to 50nm, and the pore size of macropores is >50nm.

[0011] Furthermore, the elemental phosphorus is selected from red phosphorus, white phosphorus, purple phosphorus and black scale. The elemental phosphorus is uniformly confined in the pores of the porous carbon to form a uniformly distributed composite structure.

[0012] The present invention also provides a method for preparing the above fluorine-doped phosphorus-carbon composite negative electrode material, comprising the following steps:

[0013] (1) placing the porous carbon downstream of a double-temperature zone heating furnace (lower air outlet of the double-temperature zone tubular furnace), placing a fluorine source upstream (upper air inlet of the double-temperature zone tubular furnace), heating the upstream to 700-1000° C. under an inert atmosphere, keeping the temperature for 1-5 h, heating the downstream to 400-600° C., keeping the temperature for 1-5 h, and cooling to room temperature to obtain the fluorine-doped porous carbon material;

[0014] (2) Add fluorine-doped porous carbon material and phosphorus element into a closed reactor, heat to 420-600°C under vacuum conditions, keep warm for 5-30 hours, and then cool naturally for condensation deposition. After the temperature cools to room temperature, heat it again to 280-400°C, keep warm for 10-40 hours, and cool naturally to obtain a fluorine-doped phosphorus-carbon composite material.

[0015] Furthermore, in step (1) and step (2), the heating rate is independently 1-20°C / min, preferably 5-10°C / min; in step (2), the vacuum is evacuated to a vacuum degree of 0.01-10Pa.

[0016] Furthermore, in step (1), the mass ratio of the porous carbon to the fluorine source is 1:5-10; and in step (S2), the mass ratio of the fluorine-doped porous carbon material to the phosphorus element is 1:2-4.

[0017] Further, the fluorine source is selected from at least one of fluorine-containing polymers and fluorine-containing small molecules; the fluorine-containing polymer is selected from at least one of fluorine-containing polyimide, perfluoropolyether (PFPE), polyvinylidene fluoride (PVDF), vinylidene fluoride fluororubber (AFLAS), polytrifluorochloroethylene, fluorinated ethylene propylene copolymer, tetrafluoroethylene and hexafluoropropylene copolymer, polyhexafluoroisobutylene, polyhexafluoropropylene, polytetrafluoroethylene, perfluoroalkoxyethylene polymer, poly(2,2,3,3,3-pentafluoropropyl acrylate), poly(1,1,1,3,3,3-hexafluoroisopropyl acrylate), poly(2,2,3,3,4,4,4-heptafluorobutyl methacrylate), poly(2,2,3,3,4,4,4-heptafluorobutyl methacrylate); the fluorine-containing small molecule is selected from at least one of ammonium fluoride, calcium fluoride, and lanthanum fluoride.

[0018] Preferably, the fluorine source is a compound of a fluorine-containing polymer and a fluorine-containing small molecule in a mass ratio of 1-3:1. The inventor unexpectedly found that the use of a fluorine source compounded with a polymer and a small molecule for fluorine doping can effectively increase the amount of fluorine incorporated. At low temperatures, the fluorine-containing polymer preferentially decomposes to form fluorides or fluorine gas, which fluorinates the carbon material; when the temperature rises, the fluorine-containing small molecule begins to decompose to form fluorides or fluorine gas, which then fluorinates the carbon material. Gradient fluorination is beneficial to the fluorine incorporation of the carbon material from the surface to the inside, effectively increasing the amount of fluorine incorporated, and reducing the decreasing trend of the fluorine content from the surface to the inside of the material, thereby achieving uniform fluorine incorporation.

[0019] The present invention also provides the use of the aforementioned phosphorus-carbon composite material or the phosphorus-carbon composite material prepared by the aforementioned preparation method as a negative electrode material in a sodium ion battery. The prepared sodium battery has high first coulombic efficiency, high reversible capacity and excellent cycle stability.

[0020] Compared with the prior art, the phosphorus-carbon composite material for sodium ion batteries and the preparation method thereof provided by the present invention have the advantages that: the phosphorus-carbon composite material for sodium ion batteries prepared by the present invention has a structure composed of elemental phosphorus and a porous carbon substrate, and the porous carbon is composed of carbon and carbon fluoride. By introducing fluorine atoms into the porous carbon, the introduction of fluorine successfully constructs a polar interface (CF) on the surface of the material; through the gradient fluorination strategy, that is, the mixed use of fluorine-containing polymers and fluorine-containing small molecules, the amount of fluorine incorporation is effectively increased, and the decreasing trend of fluorine content from the surface to the inside of the material is reduced, thereby achieving uniform fluorine incorporation. Finally, through the deposition of phosphorus, a stable structure of CFP is formed, and the pores of the porous carbon can effectively buffer the volume expansion of phosphorus. The formed CFP structure can increase the interaction between phosphorus and the carbon substrate, effectively improve the material's adsorption of sodium polyphosphides, and inhibit the dissolution and shuttle of sodium polyphosphides during the cycle, thereby improving the material's cycle performance. The present invention also preferably adopts a dual-temperature zone heating furnace, places a fluorine-containing polymer upstream of the heating furnace, and places a porous carbon material downstream, which can produce a fluorine-containing active ingredient and porous carbon to react under safer and more peaceful conditions to form a continuous composite structure of fluorinated carbon and carbon. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the X-ray diffraction spectrum (XRD) of the phosphorus-carbon composite material prepared in Example 1.

[0022] Figure 2 This is the photoelectron spectrum (XPS) of the F element of the phosphorus-carbon composite material prepared in Example 1.

[0023] Figure 3 This is a scanning electron microscope photograph (SEM) of the phosphorus-carbon composite material prepared in Example 1.

[0024] Figure 4 This is a transmission electron microscope (TEM) photograph of the phosphorus-carbon composite material prepared in Example 1.

[0025] Figure 5 This is the element distribution map (Mapping) of the phosphorus-carbon composite material prepared in Example 1.

[0026] Figure 6 The charge and discharge curves of the phosphorus-carbon composite material prepared in Example 1 when used as the negative electrode of a sodium ion battery.

[0027] Figure 7 The graph shows the cycle performance of the phosphorus-carbon composite material prepared in Example 1 when used as the negative electrode of a sodium ion battery. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific examples, but the present invention is not limited to the following examples.

[0029] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0030] The median particle size of porous carbon is 8 μm, and the specific surface area is 1800 ± 100 m 2 / g, the pores include micropores, mesopores and macropores.

[0031] Example 1

[0032] (1) Powdered porous carbon particles with a median particle size of 8 μm were placed downstream of a dual-temperature zone heating furnace, and polyvinylidene fluoride was placed upstream, wherein the mass ratio of the powdered porous carbon particles to the polyvinylidene fluoride was 1:10. Under an inert atmosphere, the upstream was heated at 10 °C min -1 The heating rate is 10℃min. -1 The process is heated to 500° C. at a heating rate of , kept warm for 3 hours, and cooled to room temperature to obtain the porous carbon material composited with carbon and carbon fluoride.

[0033] (2) The fluorine-doped porous carbon material and red phosphorus were stirred and mixed at a mass ratio of 1:2.5 for 30 minutes to obtain a uniformly mixed raw material, and the raw material was placed in a closed reactor with a vacuum degree of 1 Pa and heated to 450°C at a heating rate of 5°C / min and kept warm for 20 hours. The temperature was naturally cooled for condensation deposition. After the temperature was cooled to room temperature, the temperature was heated again at a heating rate of 2°C / min to 300°C, kept warm for 30 hours, and naturally cooled to obtain a fluorine-doped phosphorus-carbon composite material. TEM-EDS energy spectrum test showed that the mass percentage of fluorine was 3.25%. The results are listed in Table 1.

[0034] Table 1 Element content test

[0035] element Line Type k-factor Absorption modifier wt% C K-line system 2.781 1.00 35.73 O K-line system 2.028 1.00 2.28 F K-line system 1.728 1.00 3.25 P K-line system 1.056 1.00 58.74 Total 100.00

[0036] Figure 1 This is the XRD diffraction spectrum of the phosphorus-carbon composite material obtained in Example 1. It can be seen that there is an obvious diffraction peak of phosphorus, and there are no other miscellaneous peaks.

[0037] Figure 2 This is an XPS graph of the porous carbon material composited with carbon and carbon fluoride obtained in Example 1. It can be seen from the figure that the porous carbon material contains the chemical structure of CF and FP.

[0038] Figure 3 This is a SEM picture of the phosphorus-carbon composite material obtained in Example 1. It can be seen from the picture that the composite material is block-shaped, has a dense surface and uniform particle size, and the particle size ranges from 1 to 10 μm.

[0039] Figure 4This is a TEM image of the phosphorus-carbon composite material obtained in Example 1. It can be seen from the image that the phosphorus in the composite material is evenly distributed, and the composite structure of carbon and carbon fluoride is continuous and dense.

[0040] Figure 5 This is a mapping diagram of the phosphorus-carbon composite material obtained in Example 1. It can be seen from the figure that carbon, fluorine and phosphorus are evenly distributed in the composite material.

[0041] The electrochemical analysis test of the phosphorus-carbon composite material obtained by the invention is as follows Figure 6 and Figure 7 The charge and discharge range is 0.005-2.0V, and the compaction density is 1.5g cm -3 , at a current density of 160 mA g -1 The charge and discharge under (0.1C) condition proves that the composite material obtained by the present invention has excellent cycle performance.

[0042] Example 2

[0043] The other conditions are the same as those in Example 1, except that:

[0044] In step (1), the upstream is heated to 1000°C and the downstream is heated to 400°C.

[0045] Example 3

[0046] The other conditions are the same as those in Example 1, except that in step (1), the mass ratio of the powdered porous carbon particles to the fluorine source is 1:5, and in step (2), the mass ratio of the fluorine-doped porous carbon material to the red phosphorus is 1:2.

[0047] Example 4

[0048] Other conditions are the same as those in Example 1, except that in step (2), the mass ratio of the fluorine-doped porous carbon material to the red phosphorus is 1:4.

[0049] Example 5

[0050] The other conditions are the same as those in Example 1, except that polyhexafluoropropylene is used instead of polyvinylidene fluoride in step (1).

[0051] Example 6

[0052] The other conditions are the same as those in Example 1, except that in step (1), a mixture of polyvinylidene fluoride and polyhexafluoropropylene in a mass ratio of 1:1 is used instead of polyvinylidene fluoride.

[0053] Example 7

[0054] The other conditions are the same as those in Example 1, except that in step (1), a mixture of polyvinylidene fluoride and calcium fluoride in a mass ratio of 1:1 is used instead of polyvinylidene fluoride.

[0055] Example 8

[0056] The other conditions are the same as those in Example 1, except that in step (1), a mixture of polyvinylidene fluoride and ammonium fluoride in a mass ratio of 3:1 is used instead of polyvinylidene fluoride.

[0057] Example 9

[0058] The other conditions are the same as those in Example 1, except that calcium fluoride is used instead of polyvinylidene fluoride in step (1).

[0059] Comparative Example 1

[0060] The phosphorus-carbon composite material of the present invention is prepared in the same manner as in Example 1, except that the fluorination treatment in step (1) is omitted and the porous carbon is directly subjected to the phosphorus-carbonization in step (2).

[0061] Comparative Example 2

[0062] The other conditions are the same as those in Example 1, except that the powdered porous carbon and carbon fluoride in step (1) are mixed and ball-milled to obtain a porous carbon material composite of carbon and carbon fluoride, and the F content in the final product is close.

[0063] Application Examples

[0064] The electrochemical properties of the phosphorus-carbon composite materials prepared in the following examples and comparative examples were tested according to the following method: the prepared phosphorus-carbon composite material, carbon black and carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) composite binder were mixed in a mass ratio of 8:1:1 to form a slurry (wherein the mass ratio of CMC to SBR was 2:3), the slurry was evenly coated on a copper foil current collector, and vacuum dried for 12 hours to prepare a working electrode; a sodium sheet was used as a counter electrode, a glass fiber membrane was used as a diaphragm, and 1 mol L -1 NaPF6 (the solvent is a mixture of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1) was used as the electrolyte, and 5% by volume of VC (ethylene carbonate) and 5% by volume of FEC (fluoroethylene carbonate) were added to the electrolyte. The cells were assembled into button cells in an inert gas glove box with an argon atmosphere.

[0065] The battery assembled above was subjected to charge and discharge test on a LAND charge and discharge tester. The results are listed in Table 2.

[0066] Table 2 Electrochemical performance test results of phosphorus-carbon composite materials

[0067]

Claims

1. A fluorine-doped phosphorus-carbon composite negative electrode material, characterized in that: It is composed of elemental phosphorus and fluorine-doped porous carbon substrate. The fluorinated carbon content of the fluorine-doped porous carbon substrate gradually decreases from the surface layer to the inside. The X-ray photoelectron energy spectrum (XPS spectrum) of the F element has characteristic peaks of 687.2±0.1eV and 685.5±0.1eV.

2. The fluorine-doped phosphorus-carbon composite negative electrode material according to claim 1, characterized in that: The total mass of the phosphorus-carbon composite material is 100%, wherein the mass percentage of carbon is 20-40%, the mass percentage of phosphorus is 40-60%, and the mass percentage of fluorine is 2-7%.

3. The fluorine-doped phosphorus-carbon composite negative electrode material according to claim 1, characterized in that: The phosphorus-carbon composite material is in the form of powder, block or fiber; the median particle size of the powder is 1-10 μm.

4. The fluorine-doped phosphorus-carbon composite negative electrode material according to claim 1, characterized in that: The porous carbon material is selected from at least one of spherical activated carbon, activated carbon fiber, mesoporous carbon, carbon nanotubes, carbon molecular sieves, carbon aerogels, carbon nanocages, porous carbon microspheres, columnar activated carbon, granular activated carbon, powdered activated carbon, expanded graphite, porous graphite, MOFs material, and biomass carbon; Furthermore, the specific surface area of ​​the porous carbon material is 800-1500m 2 / g, the pores include micropores, mesopores and macropores; the pore size distribution of micropores is >0 to 2nm, the pore size distribution of mesopores is >2 to 50nm, and the pore size of macropores is >50nm.

5. The fluorine-doped phosphorus-carbon composite negative electrode material according to claim 1, characterized in that: The elemental phosphorus is selected from red phosphorus, white phosphorus, purple phosphorus and black phosphorus.

6. The method for preparing the fluorine-doped phosphorus-carbon composite negative electrode material according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) placing the porous carbon downstream of a double-temperature zone heating furnace (lower air outlet of the double-temperature zone tubular furnace), placing a fluorine source upstream (upper air inlet of the double-temperature zone tubular furnace), heating the upstream to 700-1000° C. under an inert atmosphere, keeping the temperature for 1-5 h, heating the downstream to 400-600° C., keeping the temperature for 1-5 h, and cooling to room temperature to obtain the fluorine-doped porous carbon material; (2) Add fluorine-doped porous carbon material and phosphorus element into a closed reactor, heat to 420-600°C under vacuum conditions, keep warm for 5-30 hours, and then cool naturally for condensation deposition. After the temperature cools to room temperature, heat it again to 280-400°C, keep warm for 10-40 hours, and cool naturally to obtain a fluorine-doped phosphorus-carbon composite material.

7. The preparation method according to claim 6, characterized in that: In step (1) and step (2), the heating rate is independently 1-20°C / min, preferably 5-10°C / min; in step (2), the vacuum is evacuated to a vacuum degree of 0.01-10Pa; the mass ratio of porous carbon to fluorine source is 1:5-10; in step (S2), the mass ratio of fluorine-doped porous carbon material to phosphorus element is 1:2-4.

8. The preparation method according to claim 6, characterized in that: The fluorine source is selected from at least one of fluorine-containing polymers and fluorine-containing small molecules; the fluorine-containing polymer is selected from at least one of fluorine-containing polyimide, perfluoropolyether (PFPE), polyvinylidene fluoride (PVDF), vinylidene fluoride fluororubber (AFLAS), polytrifluorochloroethylene, fluorinated ethylene propylene copolymer, tetrafluoroethylene and hexafluoropropylene copolymer, polyhexafluoroisobutylene, polyhexafluoropropylene, polytetrafluoroethylene, perfluoroalkoxyethylene polymer, poly(2,2,3,3,3-pentafluoropropyl acrylate), poly(1,1,1,3,3,3-hexafluoroisopropyl acrylate), poly(2,2,3,3,4,4,4-heptafluorobutyl methacrylate), and poly(2,2,3,3,4,4,4-heptafluorobutyl methacrylate); the fluorine-containing small molecule is selected from at least one of ammonium fluoride, calcium fluoride, and lanthanum fluoride.

9. The preparation method according to claim 8, characterized in that: The fluorine source is a compound of a fluorine-containing polymer and a fluorine-containing small molecule in a mass ratio of 1-3:

1.

10. Use of the phosphorus-carbon composite material according to any one of claims 1 to 5 or the phosphorus-carbon composite material prepared by the preparation method according to any one of claims 6 to 9 as a negative electrode material in preparing a negative electrode for a sodium ion battery.

Citation Information

Patent Citations

  • Doped porous carbon negative electrode material, preparation method thereof and alkali metal ion battery

    CN110600713A

  • Silicon-based composite material as well as preparation method and application thereof

    CN113451561A

  • Preparation method and material of fluorine-doped carbon-loaded red phosphorus negative electrode material, sodium battery and preparation method of sodium battery

    CN117832462A

  • Phosphorus-carbon cathode material based on red phosphorus and preparation method thereof

    US20240258523A1

Cited By

  • Phosphorus-based negative electrode material with solid electrolyte interface and preparation method and application thereof

    CN119725434A

  • Phosphorus-based negative electrode material with solid electrolyte interface and preparation method and application thereof

    CN119725434B