Composite sodium-ion battery positive electrode material with radial heterojunction and preparation method of composite sodium-ion battery positive electrode material
By constructing Ni0.3Mn0.7(OH)2 on the surface of Ni0.5Mn0.5(OH)2 precursor, a composite positive electrode material with radial heterojunction was synthesized, and the air stability and circulation of the positive electrode material of sodium ion battery were solved. Stability issues have achieved low cost and good electrical performance of sodium ion battery cathode material, suitable for commercial production.
Patent Information
- Application Number
- CN202411472835.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-10-22
AI Technical Summary
The air stability and circulation stability of the existing sodium ion battery cathode materials affect the performance of sodium ion batteries. The lithium resources of lithium ion batteries are limited, resulting in increased costs, limiting their application in the field of large-scale power storage. .
Ni0.3Mn0.7(OH)2 of different thicknesses are constructed using the surface of Ni0.5Mn0.5(OH)2 to synthesize a composite positive electrode material with radial heterojunction to form a core-shell structure to improve the air stability of the material and cycle stability to improve sodium ion transport kinetics.
It improves the air stability and circulation stability of sodium ion batteries, reduces material costs, achieves good electrical performance, and is suitable for commercial production.
Smart Images

Figure CN119050335A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a composite sodium ion battery positive electrode material with a radial heterojunction and a preparation method thereof. Background Art
[0002] As society continues to progress and new energy vehicles become more widespread and increasingly developed, the demand for lithium resources is rapidly increasing. However, limited and unevenly distributed lithium reserves have led to rising costs, restricting their application in large-scale power storage. In contrast, sodium-ion batteries (Na-ion batteries) share similar charge and discharge mechanisms with Li-ion batteries, and Na resources are abundant and widely distributed. Therefore, the development of Na-ion battery technology holds positive prospects for large-scale energy storage systems.
[0003] As a highly-regarded energy storage technology, the design and improvement of the positive electrode materials of sodium-ion batteries are crucial to improving battery performance. The key lies in improving the interfacial charge transfer, cycle structural stability, air stability and high-voltage stability of the materials. Summary of the Invention
[0004] The purpose of the present invention is to provide a composite sodium ion battery positive electrode material with radial heterojunction and a preparation method thereof, which can reduce the material cost while adopting the method of using Ni 0.5 Mn 0.5 Ni with different thicknesses is constructed on the surface of (OH)2 precursor 0.3 Mn 0.7 (OH)2 method is used to synthesize a composite positive electrode material with radially heterogeneous component distribution, thereby improving the air stability and cycle stability of the material and improving the sodium ion transmission kinetics. The present invention has low cost, is simple and reasonable, has good electrical properties, and is suitable for commercial production.
[0005] To achieve the above objectives, the present invention provides a composite sodium ion battery positive electrode material with a radial heterojunction. The positive electrode material is prepared by sintering a precursor and a sodium source. The prepared positive electrode material has a core-shell structure with a radial heterojunction. The core of the positive electrode material is an O3-type nickel-manganese-based layered oxide, and there is a coating material on the surface of the core, which is a P2-type nickel-manganese-based layered oxide.
[0006] Preferably, the coating material has a thickness of 0-1 μm.
[0007] Preferably, the particle size of the precursor material is 3.6-4.2 μm, and the precursor is a core-shell structure, the core chemical formula of which is Ni 0.5 Mn 0.5 (OH)2, Ni is deposited on the surface of the core 0.3 Mn 0.7 (OH)2,Ni 0.3 Mn 0.7The size of (OH)2 is x μm, where 0≤x≤1.
[0008] The present invention provides a method for preparing a composite sodium ion battery positive electrode material with a radial heterojunction, comprising the following steps: Step 1: dissolving nickel salt and manganese salt in deionized water in proportion to obtain mixed solution No. 1 and mixed solution No. 2, respectively; adding a precipitant to the deionized water to dissolve the precipitant solution; and diluting the complexing agent to a certain concentration to obtain a complexing agent solution; Step 2: simultaneously introducing the No. 1 mixed solution, the precipitant solution, and the complexing agent solution into a reactor protected by protective gas, maintaining the pH and temperature in the reactor, and removing the material when the reaction is carried out until the particle size of the material reaches the required level. Then, the salt solution in the reactor is switched from the No. 1 mixed solution to the No. 2 mixed solution, and the above operation is repeated; Step 3: Wash and dry the extracted material to obtain Ni 0.5 Mn 0.5 (OH)2 and Ni of different sizes 0.3 Mn 0.7 (OH)2-coated precursor particles; Step 4: uniformly mixing the sodium source and the precursor particles in a certain molar ratio to obtain a mixed material; Step 5: Sinter the mixture in air atmosphere, then transfer it to atmosphere furnace for further sintering, and finally synthesize a series of positive electrode materials Na x Ni y Mn z O2 samples.
[0009] Preferably, in step 1, the nickel salt is one or more of nickel sulfate, nickel nitrate and nickel chloride, the manganese salt is one or more of manganese sulfate, manganese nitrate and manganese chloride, the precipitant is one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate and potassium bicarbonate, and the complexing agent is one or more of ammonia water and oxalic acid.
[0010] Preferably, the OH in the precipitant solution - / CO3 2- / HCO 3- The concentration is 3-7 mol / L, and the concentration of the complexing agent solution is 1.5-2 mol / L.
[0011] Preferably, the ratio of Ni to Mn in the No. 1 mixed solution is 1:1, the ratio of Ni to Mn in the No. 2 mixed solution is 3:7, and the concentrations of the No. 1 mixed solution and the No. 2 mixed solution are both 3-10 mol / L.
[0012] Preferably, the reactor has a capacity of 50 L, the protective gas is nitrogen or argon, the pH in the reactor is 11.0-11.6, and the ammonia concentration is maintained at 6-9 g / L.
[0013] Preferably, the sodium source in step 4 is one or more of Na2CO3, NaOH and NaNO3, and the sodium source and the precursor particles are uniformly mixed in a molar ratio of Na:M=0.9:1.
[0014] Preferably, the mixed material in step 5 is first sintered at 500° C. in an air atmosphere for 6 h, and then transferred to an atmosphere furnace with an oxygen atmosphere and sintered at 900° C. for 24 h.
[0015] Therefore, the present invention adopts the composite sodium ion battery positive electrode material with radial heterojunction and the preparation method, which has the following beneficial effects: (1) Sodium-ion batteries and lithium-ion batteries have similar charging and discharging mechanisms, but sodium resources are more abundant and widely distributed than lithium resources, and the cost is lower. Sodium-ion batteries are also safer, with relatively high internal resistance and less instantaneous heat generation in short-circuit conditions, making them safer and more resistant to cold and heat.
[0016] (2) The present invention is achieved by 0.5 Mn 0.5 (OH)2 surface construction of Ni with different thicknesses 0.3 Mn 0.7 (OH)2, and then synthesize a composite positive electrode material with radially heterogeneous component distribution, which solves the problems of poor air stability of O3-type nickel-manganese-based layered oxides, improves the air stability and cycle stability of the material, and improves the sodium ion transfer kinetics.
[0017] (3) The positive electrode material prepared by the present invention has good cycle performance and rate performance.
[0018] (4) The preparation method of the positive electrode material proposed in the present invention is simple to operate, low in cost, and has commercial application value.
[0019] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is an SEM image of a precursor prepared in Example 2 of a composite sodium ion battery positive electrode material with radial heterojunction and a preparation method thereof of the present invention; Figure 2 This is an SEM image of the positive electrode material prepared in Example 2 of the composite sodium ion battery positive electrode material with radial heterojunction and preparation method of the present invention; Figure 3This is a partial enlarged SEM image of a precursor prepared in Example 2 of the composite sodium ion battery positive electrode material with radial heterojunction and preparation method of the present invention; Figure 4 This is a partial enlarged SEM image of the positive electrode material prepared in Example 2 of the composite sodium ion battery positive electrode material with radial heterojunction and preparation method of the present invention; Figure 5 This is the XRD pattern of the positive electrode material prepared in Example 2 of the composite sodium ion battery positive electrode material with radial heterojunction and preparation method of the present invention; Figure 6 This is a comparison chart of the cycle performance of Example 2 and Comparative Example 1 of the composite sodium ion battery positive electrode material with radial heterojunction and preparation method of the present invention at 2.0-4.0V. DETAILED DESCRIPTION
[0021] The technical solution of the present invention is further described below with reference to the accompanying drawings and embodiments.
[0022] Unless otherwise defined, technical or scientific terms used in the present invention shall have the same meaning as commonly understood by one of ordinary skill in the art to which the present invention belongs.
[0023] Example The present invention provides a composite sodium-ion battery positive electrode material with a radial heterojunction. The positive electrode material is prepared by sintering a precursor and a sodium source. The prepared positive electrode material has a core-shell structure with a radial heterojunction. The core of the positive electrode material is an O3-type nickel-manganese-based layered oxide. There is a coating material on the surface of the core. The coating material is a P2-type nickel-manganese-based layered oxide. The thickness of the coating material is 0-1 μm.
[0024] The particle size of the precursor material is 3.6-4.2 μm, and the precursor is a core-shell structure, the core chemical formula of which is Ni 0.5 Mn 0.5 (OH)2, Ni is deposited on the surface of the core 0.3 Mn 0.7 (OH)2,Ni 0.3 Mn 0.7 The size of (OH)2 is x μm, where 0≤x≤1.
[0025] The present invention also provides a method for preparing a composite sodium ion battery positive electrode material having a radial heterojunction, comprising the following steps: Step 1: Dissolve nickel and manganese salts in deionized water in the appropriate proportions to form mixed solutions No. 1 and No. 2, respectively. Add a precipitant to the deionized water to form a precipitant solution, and dilute the complexing agent to a desired concentration to form a complexing agent solution. Nickel salts (such as nickel sulfate and nickel chloride) increase the nickel content in the positive electrode material, thereby improving the battery's energy density. This increased nickel content allows the battery to store more energy and extend its battery life. The addition of manganese salts (such as manganese sulfate and manganese nitrate) improves the structural stability and safety of the positive electrode material. Manganese helps form a stable lattice structure, resisting structural changes during charge and discharge cycles, thereby extending battery life.
[0026] Mixed solution #1 has a 1:1 ratio of Ni to Mn, with each solution having a concentration of 2M. Mixed solution #2 has a 3:7 ratio of Ni to Mn, with each solution having a concentration of 2M. The resulting concentrations of both mixed solutions #1 and #2 are 3-10moL / L. By adjusting the ratio of nickel to manganese, the battery's charge and discharge efficiency, cycle stability, and rate performance can be optimized to meet the needs of different applications.
[0027] The nickel salt is one or more of nickel sulfate, nickel nitrate, and nickel chloride; the nickel sulfate is nickel sulfate hexahydrate; the manganese salt is one or more of manganese sulfate, manganese nitrate, and manganese chloride; and the manganese sulfate is manganese sulfate monohydrate. The precipitant is one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, and potassium bicarbonate; and the complexing agent is one or more of ammonia water and oxalic acid.
[0028] OH in the precipitant solution - / CO3 2- / HCO 3- The concentration is 3-7 mol / L, and the concentration of the complexing agent solution is 1.5-2 mol / L. The complexing agent can form a stable complex with the metal ions and can also increase the solubility of the metal salt. The precipitant can promote the pre-reaction of the metal ions in the solution to form a water-insoluble precipitate.
[0029] Step 2: Introduce the No. 1 mixed solution, the precipitant solution, and the complexing agent solution into the reactor protected by protective gas at the same time, maintain the pH and temperature in the reactor, and remove the material when the reaction proceeds until the material particle size reaches the requirement. Then switch the salt solution in the reactor from the No. 1 mixed solution to the No. 2 mixed solution, and repeat the above operation.
[0030] Step 3: Wash and dry the extracted material to obtain precursor particles of different sizes. The precursor particles are Ni 0.5 Mn 0.5 (OH)2 and Ni of different sizes 0.3 Mn 0.7(OH)2-coated particles. During the reaction of mixed solution No. 1, the material was removed when the particle size reached 3.6 μm; during the reaction of mixed solution No. 2, the material was removed when the particle size reached 3.8, 4.0, and 4.2 μm, respectively.
[0031] Step 4: Evenly mix the sodium source and the precursor particles in a certain molar ratio to obtain a mixed material; the sodium source is one or more of Na2CO3, NaOH and NaNO3, and the sodium source and the precursor particles are evenly mixed in a molar ratio of Na:M=0.9:1.
[0032] Step 5: Sinter the mixture in air atmosphere, then transfer it to atmosphere furnace for further sintering, and finally synthesize a series of positive electrode materials Na x Ni y Mn z O2 samples, in which the mixed materials were first sintered at 500°C in an air atmosphere for 6 h, and then transferred to an atmosphere furnace with an oxygen atmosphere and sintered at 900°C for 24 h. The finally synthesized positive electrode materials were recorded as NM, NM+0.2μm, NM+0.4μm and NM+0.6μm, respectively.
[0033] Example 1 This embodiment prepares a composite sodium ion battery positive electrode material with a radial heterojunction, comprising the following steps: (1) Nickel sulfate hexahydrate and manganese sulfate monohydrate were dissolved in deionized water in the required ratio to obtain two mixed solutions. The Ni:Mn ratio in mixed solution No. 1 was 1:1, and the Ni:Mn ratio in mixed solution No. 2 was 3:7, and the concentration of both solutions was 2M.
[0034] (2) First, the mixed solution No. 1, 4M NaOH solution, and 2M NH3·H2O solution were simultaneously introduced into the reactor with nitrogen as the protective gas, and the pH in the reactor was maintained at 11.2 and the ammonia concentration was maintained at 7.5 g / L. When the particle size of the material in the reactor reached 3.6 μm, 200 g of the material was taken out.
[0035] Then, the mixed solution No. 1 was switched to the mixed solution No. 2, the pH in the reactor was maintained at 11.2, and the ammonia concentration was maintained at 7.5 g / L. When the particle size of the material in the reactor reached 3.8 μm, 200 g of material was taken out each time; after washing and drying, the precursor particles were screened out, wherein the core of the precursor particles was Ni 0.5 Mn 0.5 (OH)2, Ni with a size of 0.2 μm is deposited on the surface of the core 0.3 Mn 0.7 (OH)2.
[0036] (3) Na2CO3 and precursor particles were mixed uniformly at a molar ratio of 0.9:1 (Na:M) to obtain a mixture. The mixture was first sintered at 500°C for 6 h in an air atmosphere, then transferred to an oxygen atmosphere furnace and sintered at 900°C for 24 h. The cathode material sample was obtained and marked as NM+0.2 μm.
[0037] (4) Measure the first-cycle discharge specific capacity and capacity retention rate after 300 cycles of the composite sodium-ion battery positive electrode material with radial heterojunction.
[0038] Example 2 This embodiment prepares a composite sodium ion battery positive electrode material with a radial heterojunction, comprising the following steps: (1) Nickel sulfate hexahydrate and manganese sulfate monohydrate were dissolved in deionized water in the required ratio to obtain two mixed solutions. The Ni:Mn ratio in mixed solution No. 1 was 1:1, and the Ni:Mn ratio in mixed solution No. 2 was 3:7, and the concentration of both solutions was 2M.
[0039] (2) First, the mixed solution No. 1, 4M NaOH solution, and 2M NH3·H2O solution were simultaneously introduced into the reactor with nitrogen as the protective gas, and the pH in the reactor was maintained at 11.2 and the ammonia concentration was maintained at 7.5 g / L. When the particle size of the material in the reactor reached 3.6 μm, 200 g of the material was taken out.
[0040] Then, the No. 1 mixed solution was switched to the No. 2 mixed solution, the pH in the reactor was maintained at 11.2, and the ammonia concentration was maintained at 7.5 g / L. When the particle size of the material in the reactor reached 4.0 μm, 200 g of material was taken out each time; after washing and drying, the precursor particles were screened out, wherein the core of the precursor particles was Ni 0.5 Mn 0.5 (OH)2, Ni with a size of 0.4 μm is deposited on the surface of the core 0.3 Mn 0.7 (OH)2.
[0041] (3) Na2CO3 and precursor particles were mixed evenly in a molar ratio of 0.9:1 (Na:M) to obtain a mixture. The mixture was first sintered at 500°C for 6 h in an air atmosphere, and then transferred to an atmosphere furnace with an oxygen atmosphere and sintered at 900°C for 24 h to obtain the positive electrode material sample, which was marked as NM+0.4 μm.
[0042] (4) Measure the first-cycle discharge specific capacity and cycle retention rate after 300 cycles of the composite sodium-ion battery positive electrode material with radial heterojunction.
[0043] Figure 1 is the SEM image of the prepared precursor. Figure 3 This is a partially enlarged SEM image of the prepared precursor. It can be seen from the image that the precursor particles were successfully prepared, and the prepared precursor has good particle morphology and distribution. Figure 2 The SEM image of the prepared cathode material is shown in Figure 2. Figure 4 This is a partial enlarged SEM image of the prepared cathode material. Figure 5 is the XRD pattern of the prepared positive electrode material. Figure 2 、 Figure 4 and Figure 5 It can be seen that the positive electrode material was successfully prepared, and the prepared precursor particles and the positive electrode material both have a two-phase structure.
[0044] Example 3 This embodiment prepares a composite sodium ion battery positive electrode material with a radial heterojunction, comprising the following steps: (1) Nickel sulfate hexahydrate and manganese sulfate monohydrate were dissolved in deionized water in the required ratio to obtain two mixed solutions. The Ni:Mn ratio in mixed solution No. 1 was 1:1, and the Ni:Mn ratio in mixed solution No. 2 was 3:7, and the concentration of both solutions was 2M.
[0045] (2) First, the mixed solution No. 1, 4M NaOH solution, and 2M NH3·H2O solution were simultaneously introduced into the reactor with nitrogen as the protective gas, and the pH in the reactor was maintained at 11.2 and the ammonia concentration was maintained at 7.5 g / L. When the particle size of the material in the reactor reached 3.6 μm, 200 g of the material was taken out.
[0046] Then, the mixed solution No. 1 was switched to the mixed solution No. 2, and the pH in the reactor was maintained at 11.2, and the ammonia concentration was maintained at 7.5 g / L. When the particle size of the material in the reactor reached 4.2 μm, 200 g of material was taken out each time; after washing and drying, the precursor particles were screened out, wherein the core of the precursor particles was Ni 0.5 Mn 0.5 (OH)2, Ni with a size of 0.6 μm is deposited on the surface of the core 0.3 Mn 0.7 (OH)2.
[0047] (3) Na2CO3 and precursor particles were mixed uniformly at a molar ratio of 0.9:1 (Na:M) to obtain a mixture. The mixture was first sintered at 500°C for 6 h in an air atmosphere, then transferred to an oxygen atmosphere furnace and sintered at 900°C for 24 h. The cathode material sample was obtained and marked as NM+0.6 μm.
[0048] (4) Measure the first-cycle discharge specific capacity and capacity retention rate after 300 cycles of the composite sodium-ion battery positive electrode material with radial heterojunction.
[0049] Comparative Example 1 The preparation of sodium ion battery positive electrode materials includes the following steps: (1) Nickel sulfate hexahydrate and manganese sulfate monohydrate were dissolved in deionized water in the required ratio to obtain two mixed solutions. The Ni:Mn ratio in mixed solution No. 1 was 1:1, and the Ni:Mn ratio in mixed solution No. 2 was 3:7, and the concentration of both solutions was 2M.
[0050] (2) First, the No. 1 mixed solution, 4M NaOH solution, and 2M NH3·H2O solution were simultaneously introduced into a reactor with nitrogen as the protective gas, and the pH in the reactor was maintained at 11.2, and the ammonia concentration was maintained at 7.5g / L. When the particle size of the material in the reactor reached 3.6μm, 200g of the material was taken out; then the No. 1 mixed solution was switched to the No. 2 mixed solution, and the pH in the reactor was maintained at 11.2, and the ammonia concentration was maintained at 7.5g / L; after washing and drying, the positive electrode material Ni was screened out. 0.5 Mn 0.5 (OH)2, marked as NM.
[0051] (3) Measure the first-cycle discharge specific capacity and capacity retention rate after 300 cycles of the composite sodium-ion battery positive electrode material with radial heterojunction.
[0052] The composite sodium ion battery positive electrode materials with radial heterojunction obtained in Examples 1-3 and the NM material obtained in Comparative Example 1 were used as positive electrodes and lithium metal sheets as negative electrodes, and button batteries were assembled for charge and discharge comparison tests. The test results are shown in the following table: Table 1 Discharge capacity test data of battery positive electrode materials ; It can be concluded from Table 1 that the composite sodium ion battery positive electrode material with radial heterojunction obtained in Examples 1-3 is used as the positive electrode, and the metal lithium sheet is used as the negative electrode to assemble a button battery for charge and discharge comparison test. At a rate of 1C, the first-cycle discharge capacity can reach up to 119.61 mAh / g, and the capacity retention rate after 300 cycles can reach up to 64.61. Although the first-cycle discharge capacity of the NM material obtained in Comparative Example 1 as the positive electrode reaches 134.82 mAh / g, the capacity retention rate after 300 cycles is only 11.69%.
[0053] It can be seen from this that the cycle stability of the battery made of the composite sodium-ion battery positive electrode material with radial heterojunction is much higher than that of the battery made of ordinary sodium-ion battery positive electrode material. Overall, the battery made of the composite sodium-ion battery positive electrode material with radial heterojunction is better than the battery made of ordinary sodium-ion battery positive electrode material, and the optimal thickness of the coating material of the composite sodium-ion battery positive electrode material with radial heterojunction is 0.4μm.
[0054] Figure 6 This is a comparison chart of the cycle performance of Example 2 and Comparative Example 1 at 2.0-4.0V. As can be seen from the figure, Example 2 performs well under long cycle conditions and can maintain a higher specific energy.
[0055] Therefore, the present invention adopts the composite sodium ion battery positive electrode material with radial heterojunction and the preparation method, while reducing the material cost, using Ni 0.5 Mn 0.5 Ni with different thicknesses is constructed on the surface of (OH)2 precursor 0.3 Mn 0.7 (OH)2 method is used to synthesize a composite positive electrode material with radially heterogeneous component distribution, thereby improving the air stability and cycle stability of the material and improving the sodium ion transmission kinetics. The present invention has low cost, is simple and reasonable, has good electrical properties, and is suitable for commercial production.
[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solutions of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A composite sodium ion battery positive electrode material with radial heterojunction, characterized in that: The positive electrode material is prepared by sintering a precursor and a sodium source. The prepared positive electrode material is a core-shell structure with a radial heterojunction. The inner core of the positive electrode material is an O3-type nickel-manganese-based layered oxide. There is a coating material on the surface of the inner core, and the coating material is a P2-type nickel-manganese-based layered oxide.
2. The composite sodium ion battery positive electrode material with radial heterojunction according to claim 1, characterized in that: The coating material has a thickness of 0-1 μm.
3. The composite sodium ion battery positive electrode material with radial heterojunction according to claim 1, characterized in that: The particle size of the precursor material is 3.6-4.2 μm, and the precursor is a core-shell structure, and the core chemical formula is Ni 0.5 Mn 0.5 (OH)2, Ni is deposited on the surface of the core 0.3 Mn 0.7 (OH)2,Ni 0.3 Mn 0.7 The size of (OH)2 is x μm, where 0≤x≤1.
4. A method for preparing a composite sodium ion battery positive electrode material with a radial heterojunction according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1, dissolving nickel salt and manganese salt in deionized water according to a proportion to obtain a mixed solution No. 1 and a mixed solution No. 2 respectively, adding a precipitant into deionized water to dissolve to prepare a precipitant solution, and diluting a complexing agent to a certain concentration to prepare a complexing agent solution; Step 2: simultaneously introduce the No. 1 mixed solution, the precipitant solution and the complexing agent solution into a reactor protected by protective gas, maintain the pH and temperature in the reactor, take out the material when the reaction is carried out until the particle size of the material reaches the requirement, then switch the salt solution in the reactor from the No. 1 mixed solution to the No. 2 mixed solution, and repeat the above operation; Step 3: Wash and dry the taken-out material to obtain Ni 0.5 Mn 0.5 (OH)2 and different sizes of Ni 0.3 Mn 0.7 (OH)2-coated precursor particles; Step 4: uniformly mix the sodium source and the precursor particles according to a certain molar ratio to obtain a mixed material; Step 5: Sinter the mixture in air atmosphere, then transfer it to an atmosphere furnace for further sintering, and finally synthesize a series of positive electrode materials Na x Ni y Mn z O2 samples.
5. The method for preparing a composite sodium ion battery positive electrode material with radial heterojunction according to claim 4, characterized in that: In the step 1, the nickel salt is one or more of nickel sulfate, nickel nitrate and nickel chloride, the manganese salt is one or more of manganese sulfate, manganese nitrate and manganese chloride, the precipitant is one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate and potassium bicarbonate, and the complexing agent is one or more of ammonia water and oxalic acid.
6. The method for preparing a composite sodium ion battery positive electrode material with radial heterojunction according to claim 4, characterized in that: The precipitant solution contains OH - / CO3 2- / HCO 3- The concentration is 3-7 mol / L, and the concentration of the complexing agent solution is 1.5-2 mol / L.
7. The method for preparing a composite sodium ion battery positive electrode material with radial heterojunction according to claim 4, characterized in that: The ratio of Ni to Mn in the No. 1 mixed solution is 1:1, the ratio of Ni to Mn in the No. 2 mixed solution is 3:7, and the concentrations of the No. 1 mixed solution and the No. 2 mixed solution are both 3-10 moL / L.
8. The method for preparing a composite sodium ion battery positive electrode material with radial heterojunction according to claim 4, characterized in that: The reactor has a capacity of 50 L, the protective gas is nitrogen or argon, the pH in the reactor is 11.0-11.6, and the ammonia concentration is maintained at 6-9 g / L.
9. The method for preparing a composite sodium ion battery positive electrode material with radial heterojunction according to claim 4, characterized in that: The sodium source in step 4 is one or more of Na2CO3, NaOH or NaNO3, and the sodium source and the precursor particles are evenly mixed in a molar ratio of Na:M=0.9:
1.
10. The method for preparing a composite sodium ion battery positive electrode material with radial heterojunction according to claim 4, characterized in that: In the step 5, the mixed material is first sintered at 500° C. in an air atmosphere for 6 hours, and then transferred to an atmosphere furnace in an oxygen atmosphere and sintered at 900° C. for 24 hours.
Citation Information
Patent Citations
Positive electrode material precursor, positive electrode material, preparation method of positive electrode material and sodium ion battery
CN114920306A
Sodium-ion battery positive electrode material, precursor and preparation method
CN115057482A
Preparation method of precursor, precursor and positive electrode material
CN115745026A
Core-shell structure sodium ion battery positive electrode material and preparation method and application thereof
CN117976884A
Layered oxide positive electrode material and preparation method therefor, and sodium-ion battery
WO2024031913A1
Cited By
Core-shell structure sodium ion battery positive electrode material and in-situ coating preparation method thereof
CN121366885A