Porphyrin-based MOF modified diaphragm for lithium battery as well as preparation method and application of porphyrin-based MOF modified diaphragm

By modifying the porphyrin-based MOF coating on the separator of the lithium battery, the problem of transition metal ions and lithium ions is solved in lithium batteries by using its pore structure and active sites to adsorb and coordinate transition metal ions and lithium ions, the problems of transition metal ions deposition and lithium dendrites in lithium batteries are solved. , improves the battery's cycle life and safety performance.

CN119050602AActive Publication Date: 2024-11-29DONGFENG MOTOR GRP

Patent Information

Application Number
CN202411036338.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-29
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The current technology is difficult to effectively solve the battery capacity attenuation caused by the dissolution of transition metal ions in high-specific energy lithium batteries to the negative electrode deposition, as well as the safety problems caused by the growth of lithium dendrites in lithium metal batteries.

Method used

The separator is modified by porphyrin-based MOF, and the transition metal ions are blocked by forming a porphyrin-based MOF coating on the base film, using its ultra-high specific surface area and regular pore structure, physical adsorption and chemical coordination are used to block transition metal ions, and mutually through Li-N The effect is to homogenize the lithium ion flux and inhibit the growth of lithium dendrites.

Benefits of technology

The battery cycle life and safety performance are effectively improved, the capacity retention rate and Coulomb efficiency are significantly improved, and the battery safety is guaranteed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050602A_ABST
    Figure CN119050602A_ABST
Patent Text Reader

Abstract

The invention provides a porphyrin-based MOF modified diaphragm for a lithium battery, and a preparation method and application thereof, and belongs to the field of lithium batteries. The porphyrin-based MOF modified diaphragm comprises a base membrane and a porphyrin-based MOF coating, and the porphyrin-based MOF coating is arranged on the surface of at least one side of the base membrane. The porphyrin-based MOF coating is formed on the base membrane, and the MOF modified diaphragm anchors transition metal ions at the positive electrode end containing transition metal elements through the physical and chemical common adsorption effect, so that the situation that the transition metal ions are deposited at the negative electrode to cause attenuation of the battery capacity is avoided. And at the negative electrode end, the MOF modified diaphragm homogenizes the lithium ion flux through uniform pore channels and Li-N interaction, so that the deposition of lithium metal becomes more uniform, and the growth of lithium dendrites is inhibited. In conclusion, the porphyrin-based MOF modified diaphragm solves the battery capacity attenuation caused by the deposition of transition metal ions from dissolution to a negative electrode in a high-specific-energy battery system, and the safety problem caused by the growth of lithium dendrites in a lithium metal battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium batteries, and in particular to a porphyrin-based MOF-modified diaphragm for lithium batteries and a preparation method and application thereof. Background Art

[0002] With the explosive growth in demand for portable electronic devices and new energy vehicles, it is urgent to develop secondary lithium batteries with high energy density, high power density and long cycle life. In order to overcome mileage anxiety and meet the demand for long battery life, the batteries currently installed in high-end electric vehicles basically use high-nickel ternary materials as the positive electrode.

[0003] However, the battery capacity attenuation caused by the dissolution of transition metal ions to the negative electrode deposition in the high specific energy battery system, and the safety problems caused by the growth of lithium dendrites in lithium metal batteries, seriously affect the application of lithium batteries. In view of the above two application problems, in addition to conventional material modification and electrode interface modification, functional coating modification from the diaphragm end is a practical and effective solution. For example, a PVDF coated diaphragm is disclosed in the prior art, which has the characteristics of low internal resistance, high (thickness / porosity) uniformity, good mechanical properties, good chemical and electrochemical stability, etc. Due to the presence of nanofiber coating, the new diaphragm has better compatibility and adhesion to lithium battery electrodes than ordinary battery diaphragms, and can greatly improve the high temperature resistance and safety of the battery. However, the PVDF coated diaphragm has high crystallinity and a hydrophobic surface, which leads to obstructed lithium ion transmission and poor electrolyte retention. In particular, for nickel-containing layered material systems and lithium metal systems, it cannot specifically solve the problems of transition metal ion dissolution to negative electrode deposition and metallic lithium deposition. At the same time, the prior art discloses an alumina / boehmite coating diaphragm, and the ultrafine alumina has the characteristics of good conductivity, thermal stability and corrosion resistance, but the energy density is low and the cost is high. Boehmite has the characteristics of high safety, good cycle life and low self-discharge rate, but it has low conductivity, relatively low specific capacity and high cost. However, for nickel-containing layered material systems and lithium metal systems, the alumina / boehmite coating diaphragm cannot specifically solve the problem of transition metal ion dissolution to negative electrode deposition and metallic lithium deposition. Therefore, it is urgent to solve the battery capacity attenuation caused by the dissolution of transition metal ions to negative electrode deposition in high specific energy battery systems and the safety problems caused by the growth of lithium dendrites in lithium metal batteries from the diaphragm level. Summary of the invention

[0004] The present application provides a porphyrin-based MOF-modified diaphragm for lithium batteries, a preparation method and an application thereof, in order to solve the battery capacity attenuation caused by the dissolution of transition metal ions to the negative electrode deposition in a high-energy-density battery system, and the safety problems caused by the growth of lithium dendrites in lithium metal batteries.

[0005] In a first aspect, the present application provides a porphyrin-based MOF-modified diaphragm for a lithium battery, wherein the porphyrin-based MOF-modified diaphragm is used for a lithium battery, wherein the positive electrode active material of the lithium battery contains a transition metal element, and the porphyrin-based MOF-modified diaphragm comprises:

[0006] basement membrane; and

[0007] A porphyrin-based MOF coating is provided on at least one side surface of the base film, and a coating slurry of the porphyrin-based MOF coating comprises a porphyrin-based MOF material, and the porphyrin-based MOF material comprises one or more of PCN222 and PCN223.

[0008] Optionally, the coating slurry further comprises: a dispersant, a binder and a solvent. The mass ratio of the porphyrin-based MOF material, the dispersant and the binder is (90-96):(0.2-3):(1-10).

[0009] Optionally, the dispersant includes: one or more of sodium carboxymethyl cellulose and polyacrylates.

[0010] Optionally, the binder includes: one or more of polyvinylidene fluoride, polyacrylic acid and sodium alginate.

[0011] Optionally, the solvent includes: one or more of water, N-methylpyrrolidone, ethanol and acetone.

[0012] Optionally, the base film includes one or more of polyolefin, polyvinylidene fluoride, polyethylene oxide, polyvinylidene fluoride and hexafluoropropylene copolymer, polyvinyl chloride, polytetrafluoroethylene, polyacrylonitrile, polymethyl methacrylate, polyimide, cellulose and polyurethane.

[0013] Optionally, the base film has a thickness of 9 μm to 11 μm, and the porphyrin-based MOF coating has a thickness of 2 μm to 3 μm.

[0014] In a second aspect, the present application provides a method for preparing a porphyrin-based MOF-modified diaphragm according to any one of the embodiments in the first aspect, the method comprising:

[0015] Obtaining porphyrin-based MOF materials;

[0016] The porphyrin-based MOF material is mixed with a dispersant, a binder and a solvent to obtain a coating slurry;

[0017] The coating slurry is coated on at least one surface of the base film to obtain a porphyrin-based MOF modified membrane.

[0018] Optionally, the coating baking temperature is 70°C to 90°C.

[0019] In a third aspect, the present application provides a lithium battery, comprising: a positive electrode, a negative electrode, an electrolyte and a diaphragm, the active material of the positive electrode comprising: one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium-rich manganese base, lithium iron manganese phosphate and lithium nickel manganese oxide, and the diaphragm is a porphyrin-based MOF modified diaphragm as described in any one of the embodiments in the first aspect.

[0020] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0021] The present application provides a porphyrin-based MOF modified diaphragm for lithium batteries, the porphyrin-based MOF modified diaphragm is used for lithium batteries, the positive electrode active material of the lithium battery contains transition metal elements, the porphyrin-based MOF modified diaphragm includes a base film and a porphyrin-based MOF coating, the porphyrin-based MOF coating is coated on at least one side of the base film, the coating slurry of the porphyrin-based MOF coating includes a porphyrin-based MOF material, and the porphyrin-based MOF material includes: one or more of PCN222 and PCN223. By forming a porphyrin-based MOF coating on the base film, the porphyrin-based MOF has an ultra-high specific surface area and a regular pore structure, and at the same time, there are abundant and uniform nitrogen-containing active sites inside its pores. On the one hand, at the positive end, it can use the capillary action of the pores to physically adsorb transition metal ions dissolved from the metal oxide positive electrode, and the active nitrogen nodes in its pores can coordinate with the transition metal ions, anchoring the transition metal ions through physical and chemical adsorption, and blocking them at the positive end through the modified diaphragm to prevent them from depositing at the negative electrode and causing battery capacity decay. On the other hand, at the negative end, especially the lithium metal negative end, the MOF-modified diaphragm can homogenize the lithium ion flux through its uniform pores and Li-N interactions, making the deposition of lithium metal more uniform, inhibiting the growth of lithium dendrites, and effectively ensuring battery safety. This solves the battery capacity decay caused by the dissolution of transition metal ions to the negative electrode deposition in high-energy-density battery systems, as well as the safety issues caused by the growth of lithium dendrites in lithium metal batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0023] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0024] Figure 1A schematic flow chart of a method for preparing a porphyrin-based MOF-modified diaphragm for a lithium battery provided in an embodiment of the present application. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0026] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0027] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0028] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0029] The creative concept of this application is:

[0030] In order to overcome mileage anxiety and meet the needs of high endurance, the batteries currently installed in high-end electric vehicles basically use high-nickel ternary materials as the positive electrode. With the increase of nickel content, the energy density of lithium batteries has been greatly improved, but the thermal stability of the battery has been significantly reduced and the cycle performance has deteriorated. Moreover, with the increase of nickel content (especially high nickel ternary with nickel content>60%), the sintering temperature is lower, resulting in a decrease in the volatilization of lithium salts, an increase in the content of lithium salts remaining on the surface of the material, and the formation of lithium oxide (Li2O), which is easy to adsorb CO2 and H2O in the air, forming Li2CO3 and LiOH on the surface of the material. Li2CO3 will cause the battery to decompose and produce gas when stored at high temperature, full charge and high potential. LiOH will react with the electrolyte lithium salt to generate HF, which will etch the positive electrode material, causing the transition metal to dissolve and pass through the diaphragm to deposit on the negative electrode. This is one of the main reasons for the battery capacity decay. At the same time, the metal foreign matter produced by the deposition may also pierce the diaphragm and threaten the battery safety.

[0031] At the same time, in the industrial pre-research projects, in order to further improve the energy density of the battery, lithium metal batteries using metallic lithium as the negative electrode have attracted much attention. They have ultra-high theoretical specific capacity (3860mAh / g), extremely low standard redox potential (-3.04V) and extremely small density, and have excellent performance in solid-state batteries and new battery systems such as lithium-sulfur batteries / lithium-air batteries. However, the development of lithium metal batteries also faces many challenges, the most critical of which is that the uneven lithium flux and electrode exchange current density will lead to the growth of lithium dendrites, and the continuous growth of lithium dendrites will pierce the diaphragm, leading to safety problems.

[0032] For the above two application scenarios, in addition to conventional material modification and electrode interface modification, functional coating modification from the diaphragm end is a practical and effective solution.

[0033] Therefore, in view of the battery capacity attenuation caused by the dissolution of transition metal ions to the negative electrode deposition in the high specific energy battery system, and the safety problems caused by the growth of lithium dendrites in lithium metal batteries, the present application provides a porphyrin-based metal organic framework compound (MOF) modified diaphragm, the porphyrin-based MOF has an ultra-high specific surface area and a regular pore structure, and at the same time, there are rich and uniform nitrogen-containing active sites inside its pores. On the one hand, at the positive end, it can use the capillary action of the pores to physically adsorb the transition metal ions dissolved from the positive electrode of the metal oxide, and the active nitrogen nodes in its pores can coordinate with the transition metal ions, anchor the transition metal ions through physical and chemical joint adsorption, and block them at the positive end by modifying the diaphragm to avoid the attenuation of the battery capacity caused by its deposition at the negative electrode. On the other hand, at the negative end, especially the lithium metal negative end, the MOF modified diaphragm can homogenize the lithium ion flux through its uniform pores and Li-N interactions, so that the deposition of lithium metal becomes more uniform, inhibiting the growth of lithium dendrites, and effectively ensuring battery safety.

[0034] The present application provides a porphyrin-based MOF-modified diaphragm for a lithium battery, wherein the porphyrin-based MOF-modified diaphragm is used for a lithium battery, wherein the positive electrode active material of the lithium battery contains a transition metal element, and the porphyrin-based MOF-modified diaphragm comprises: a base membrane; and a porphyrin-based MOF coating, wherein the porphyrin-based MOF coating is disposed on at least one side surface of the base membrane, and the coating slurry of the porphyrin-based MOF coating comprises a porphyrin-based MOF material, and the porphyrin-based MOF material comprises: one or more of PCN222 and PCN223.

[0035] Through extensive research, this application selects a specific type of porphyrin-based MOF material (PCN222 and PCN223) to modify the diaphragm. The porphyrin-based MOF has an ultra-high specific surface area and a regular pore structure. At the same time, there are rich and uniform nitrogen-containing active sites inside its pores, which can not only adsorb and anchor transition metal ions dissolved from the positive electrode, but also use its uniform pores and Li-N interactions to homogenize the lithium ion flux, inhibit the growth of lithium dendrites, and effectively improve the safety performance and cycle life of the battery.

[0036] In some embodiments, the coating slurry further comprises: a dispersant, a binder and a solvent. The mass ratio of the porphyrin-based MOF material, the dispersant and the binder is (90-96): (0.2-3): (1-10).

[0037] In the above embodiment, the mass ratio of the porphyrin-based MOF material, the dispersant and the binder is controlled to be porphyrin-based MOF material: dispersant: binder = (90-96): (0.2-3): (1-10) with positive effects: by adding the dispersant, the affinity between the particle surface of the porphyrin-based MOF material and the medium can be improved, so that the porphyrin-based MOF material particles can be easily infiltrated and maintained in a uniformly dispersed state in the coating slurry, thereby preventing the agglomeration of the porphyrin-based MOF material particles; and the binder makes the porphyrin-based MOF material particles closely adhere to the base film. The present application reasonably designs the composition of the coating slurry to ensure that the porphyrin-based MOF material can be smoothly coated on the surface of the base film to form a coating. Exemplarily, the mass ratio of the porphyrin-based MOF material, the dispersant and the binder can be 90:0.2:9.8, 90:1:9, 90:2:8, 90:3:7, 95:0.2:4.8, 95:1:4, 95:2:3, 95:3:2, 96:0.2:3.8, 96:1:3, 96:2:2, 96:3:1, etc.

[0038] In some embodiments, the dispersant includes: one or more of sodium carboxymethyl cellulose and polyacrylates.

[0039] In some embodiments, the binder includes: one or more of polyvinylidene fluoride, polyacrylic acid and sodium alginate.

[0040] In some embodiments, the solvent includes: one or more of water, N-methylpyrrolidone, ethanol and acetone.

[0041] In some embodiments, the base film includes one or more of polyolefin, polyvinylidene fluoride, polyethylene oxide, polyvinylidene fluoride and hexafluoropropylene copolymer, polyvinyl chloride, polytetrafluoroethylene, polyacrylonitrile, polymethyl methacrylate, polyimide, cellulose and polyurethane.

[0042] In some embodiments, the base film has a thickness of 9 μm to 11 μm, and the porphyrin-based MOF coating has a thickness of 2 μm to 3 μm.

[0043] Figure 1 A schematic flow chart of a method for preparing a porphyrin-based MOF-modified diaphragm for a lithium battery provided in an embodiment of the present application.

[0044] See also Figure 1 The present application provides a method for preparing a porphyrin-based MOF-modified diaphragm according to any one of the above embodiments, the method comprising:

[0045] S1, obtaining a porphyrin-based MOF material;

[0046] In some embodiments, the obtaining of the porphyrin-based MOF material comprises:

[0047] S101. Weigh a certain amount of methyl p-formylbenzoate into a three-necked flask, and add an appropriate amount of propionic acid to dissolve it completely. Set up a reflux condenser, heat to 120°C in a dark environment under the protection of an argon atmosphere, and then slowly add an appropriate amount of pyrrole to the flask in a dark environment. After reacting at 120°C for a short time, heat to 140°C and react for 12 hours. After the reaction is complete, filter, wash repeatedly with deionized water and ethanol, and dry to obtain the ligand precursor tetrakis(4-carboxymethylesterphenyl)porphyrin;

[0048] S102. Weigh a certain amount of tetrakis(4-carboxymethyl ester phenyl)porphyrin into a round-bottom flask, add appropriate amounts of methanol and tetrahydrofuran to dissolve it completely. Weigh appropriate amounts of potassium hydroxide and deionized water to prepare alkali solution and add it to the above solution, slowly heat to 85°C, and condense and reflux for 12 hours. After the reaction is completed, add deionized water to dissolve it after rotary evaporation, acidify it with acetic acid to a system pH ≥ 5, filter the resulting suspension, wash it with deionized water, and dry it to obtain the ligand tetrakis(4-carboxyphenyl)porphyrin;

[0049] S103, weigh a certain amount of zirconium salt and tetrakis (4-carboxyphenyl) porphyrin in a glass bottle, add DMF to dissolve it completely, then add an appropriate amount of pH adjuster, and react at 120°C for 12 hours. After the reaction is complete and cooled to room temperature, centrifuge to pour out the supernatant and add an appropriate amount of DMF to fully disperse it. Repeat the exchange several times and then dry and grind to obtain porphyrin-based MOF.

[0050] In some embodiments, the zirconium salt includes: hydrated zirconium oxychloride.

[0051] In some embodiments, the pH adjuster determines the type of porphyrin-based MOF; wherein, when the pH adjuster is p-tert-butylbenzoic acid, the porphyrin-based MOF material is PCN222; when the pH adjuster is p-chlorobenzoic acid, the porphyrin-based MOF material is PCN223.

[0052] S2, mixing the porphyrin-based MOF material with a dispersant, a binder and a solvent to obtain a coating slurry;

[0053] S3, coating the coating slurry on at least one side of the surface of the base film to obtain a porphyrin-based MOF modified membrane.

[0054] In some embodiments, the coating baking temperature is 70°C to 90°C.

[0055] In the above embodiment, the coating baking temperature is controlled to efficiently remove the solvent in the coating slurry and prevent the coating from cracking. Exemplarily, the coating baking temperature can be 70°C, 75°C, 80°C, 85°C, 90°C, etc.

[0056] The product prepared by the preparation method of the porphyrin-based MOF modified membrane is the above-mentioned porphyrin-based MOF modified membrane. The chemical composition and microstructure of the porphyrin-based MOF modified membrane prepared by the preparation method of the porphyrin-based MOF modified membrane can refer to the above-mentioned embodiment. Since the preparation method of the porphyrin-based MOF modified membrane adopts part or all of the technical solutions of the porphyrin-based MOF modified membrane embodiment, it at least has all the beneficial effects brought by the technical solutions of the porphyrin-based MOF modified membrane embodiment, which will not be repeated here one by one.

[0057] Based on a general inventive concept, the present application provides a lithium battery, which includes: a positive electrode, a negative electrode, an electrolyte and a separator, the active material of the positive electrode includes: one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium-rich manganese base, lithium iron manganese phosphate and lithium nickel manganese oxide, and the separator is a porphyrin-based MOF modified separator described in any one of the above embodiments.

[0058] In some embodiments, the negative electrode includes one or more of a graphite negative electrode, a silicon-carbon negative electrode, and a lithium metal negative electrode; and the electrolyte consists of a lithium salt and a carbonate solvent.

[0059] The lithium battery provided in the present application is charged and discharged at a current density of 1C, and the capacity retention rate after 50 cycles is ≥99%.

[0060] The lithium battery provided in this application is 1mA / cm 2 The charge and discharge test was carried out under the current density, and the coulomb efficiency in the first week was ≥99.8%, and the average coulomb efficiency after 200 weeks was ≥99.6%.

[0061] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0062] Example 1

[0063] This embodiment provides a method for preparing a porphyrin-based MOF modified diaphragm, and the specific steps are as follows:

[0064] S11, obtaining PCN222 powder;

[0065] S21, weighing raw materials according to the mass ratio of PCN222, CMC and PAA of 95:1:4, mixing CMC and deionized water to obtain a dispersion, adding the dispersion to the PCN222 powder material, and then adding PAA and stirring for 30 minutes to obtain a coating slurry;

[0066] S31: Use a micro-concave coater to coat the coating slurry on both sides of the PE base film, the base film thickness is 9 μm, and the coating thickness is 2 μm, to obtain a porphyrin-based MOF modified diaphragm.

[0067] Example 2

[0068] This embodiment provides a method for preparing a porphyrin-based MOF modified diaphragm, and the specific steps are as follows:

[0069] S11, obtaining PCN223 powder;

[0070] S21, weighing raw materials according to the mass ratio of PCN223, CMC and PAA of 95:1:4, mixing CMC and deionized water to obtain a dispersion, adding the dispersion to the PCN223 powder material, and then adding PAA and stirring for 30 minutes to obtain a coating slurry;

[0071] S31: Use a micro-concave coater to coat the coating slurry on both sides of the PE base film, the base film thickness is 9 μm, and the coating thickness is 2 μm, to obtain a porphyrin-based MOF modified diaphragm.

[0072] Example 3

[0073] This embodiment provides a method for preparing a lithium battery, and the specific steps are as follows:

[0074] The coated diaphragm obtained in Example 1 was used as the diaphragm, commercial NCM811 was used as the positive electrode, commercial graphite was used as the negative electrode, and a mature commercial electrolyte was selected to assemble a small soft-pack battery in an environmentally controlled soft-pack line.

[0075] Example 4

[0076] This embodiment provides a method for preparing a lithium battery, and the specific steps are as follows:

[0077] The coated diaphragm obtained in Example 2 was used as the diaphragm, commercial NCM811 was used as the positive electrode, commercial graphite was used as the negative electrode, and a mature commercial electrolyte was selected to assemble a small soft-pack battery in an environmentally controlled soft-pack line.

[0078] Example 5

[0079] This embodiment provides a method for preparing a lithium battery, and the specific steps are as follows:

[0080] The coated membrane obtained in Example 1 was used as a membrane, a mature electrolyte was selected, and a Li||Li symmetric battery (CR2032 button cell) was assembled in a glove box filled with argon.

[0081] Example 6

[0082] This embodiment provides a method for preparing a lithium battery, and the specific steps are as follows:

[0083] The coated membrane obtained in Example 2 was used as a membrane, a mature electrolyte was selected, and a Li||Li symmetric battery (CR2032 button cell) was assembled in a glove box filled with argon.

[0084] Comparative Example 1

[0085] This comparative example provides a commercial PVDF separator.

[0086] Comparative Example 2

[0087] This comparative example provides a method for preparing a lithium battery, and the specific steps are as follows:

[0088] Select the commercial separator in Comparative Example 1, use commercial NCM811 as the positive electrode, commercial graphite as the negative electrode, select a mature commercial electrolyte, and assemble a small soft-pack battery in an environmentally controlled soft-pack line.

[0089] Comparative Example 3

[0090] This comparative example provides a method for preparing a lithium battery, and the specific steps are as follows:

[0091] The commercial separator in Comparative Example 1 was selected, and a mature electrolyte was selected to assemble a Li||Li symmetric battery (CR2032 button cell) in an argon-filled glove box.

[0092] Performance test results of the embodiments and comparative examples:

[0093] The diaphragms prepared in Examples 1 and 2 and the commercial diaphragm provided in Comparative Example 1 were placed in a NiCl2 aqueous solution for adsorption test, and the color change of the solution was observed. The results are shown in Table 1.

[0094] Table 1 Adsorption test results of diaphragm in NiCl2 aqueous solution

[0095] Group <![CDATA[Color change of NiCl2 aqueous solution]]> Example 1 From green to colorless Example 2 From green to colorless Comparative Example 1 No change

[0096] The batteries prepared in Examples 3 and 4 were subjected to charge and discharge tests at a current density of 1 C, and the capacity retention rate after 50 cycles was recorded and compared with the battery of Comparative Example 2. The results are shown in Table 2.

[0097] Table 2 Charge and discharge test results of lithium batteries prepared in Examples 3, 4 and Comparative Example 2

[0098] Group Capacity retention after 50 cycles Example 3 99.5% Example 4 99.1% Comparative Example 2 97.9%

[0099] As can be seen from Table 2, the battery assembled using porphyrin-based MOF-modified composite diaphragms has significantly improved cycle stability compared to ordinary commercial diaphragms.

[0100] The batteries prepared in Examples 5, 6 and Comparative Example 3 were subjected to charge and discharge tests at a current density of 1 mA / cm 2 The number of cycles is 200, and all the metal lithium in the negative electrode is removed at the 201st cycle, and the average coulombic efficiency is calculated from this. The results are shown in Table 2.

[0101] Table 3 Charge and discharge test results of lithium batteries prepared in Examples 5, 6 and Comparative Example 3

[0102]

[0103]

[0104] As can be seen from Table 3, the average coulombic efficiency of the battery assembled using the porphyrin-based MOF modified composite diaphragm is significantly improved compared with the ordinary commercial diaphragm, indicating that it inhibits the growth of lithium dendrites and reduces the formation of dead lithium.

[0105] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0106] In the embodiment of the present invention, a porphyrin-based metal organic framework compound (MOF) modified diaphragm is provided. At the positive terminal, it can anchor transition metal ions through physical and chemical adsorption, and block them at the positive terminal through the modified diaphragm to prevent them from being deposited at the negative electrode and causing the battery capacity to decay. At the lithium metal negative terminal, it can homogenize the lithium ion flux through its uniform pores and Li-N interaction, making the deposition of lithium metal more uniform, inhibiting the growth of lithium dendrites, and effectively ensuring battery safety.

[0107] In the embodiment of the present invention, the safety performance and cycle life of the battery are effectively improved by using a porphyrin-based MOF to modify the separator. The provided lithium battery is charged and discharged at a current density of 1C, and the capacity retention rate after 50 cycles is ≥ 99%. At 1 mA / cm 2 The charge and discharge test was carried out under the current density, and the coulomb efficiency in the first week was ≥99.8%, and the average coulomb efficiency after 200 weeks was ≥99.6%.

[0108] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A porphyrin-based MOF modified diaphragm for lithium batteries, characterized in that: The porphyrin-based MOF modified diaphragm is used for a lithium battery, wherein the positive electrode active material of the lithium battery contains a transition metal element, and the porphyrin-based MOF modified diaphragm comprises: basement membrane; and A porphyrin-based MOF coating is provided on at least one side surface of the base film, and a coating slurry of the porphyrin-based MOF coating comprises a porphyrin-based MOF material, and the porphyrin-based MOF material comprises one or more of PCN222 and PCN223.

2. The porphyrin-based MOF modified membrane according to claim 1, characterized in that: The coating slurry further includes: a dispersant, a binder and a solvent. The mass ratio of the porphyrin-based MOF material, the dispersant and the binder is (90-96): (0.2-3): (1-10).

3. The porphyrin-based MOF modified membrane according to claim 2, characterized in that: The dispersant includes: one or more of sodium carboxymethyl cellulose and polyacrylates.

4. The porphyrin-based MOF modified membrane according to claim 2, characterized in that: The binder includes: one or more of polyvinylidene fluoride, polyacrylic acid and sodium alginate.

5. The porphyrin-based MOF modified membrane according to claim 2, characterized in that: The solvent includes: one or more of water, N-methylpyrrolidone, ethanol and acetone.

6. The porphyrin-based MOF modified membrane according to claim 2, characterized in that: The base film comprises: one or more of polyolefin, polyvinylidene fluoride, polyethylene oxide, polyvinylidene fluoride and hexafluoropropylene copolymer, polyvinyl chloride, polytetrafluoroethylene, polyacrylonitrile, polymethyl methacrylate, polyimide, cellulose and polyurethane.

7. The porphyrin-based MOF modified membrane according to claim 2, characterized in that: The thickness of the base film is 9 μm to 11 μm, and the thickness of the porphyrin-based MOF coating is 2 μm to 3 μm.

8. A method for preparing a porphyrin-based MOF modified membrane according to any one of claims 1 to 7, characterized in that: The method comprises: Obtaining porphyrin-based MOF materials; The porphyrin-based MOF material is mixed with a dispersant, a binder and a solvent to obtain a coating slurry; The coating slurry is coated on at least one surface of the base film to obtain a porphyrin-based MOF modified membrane.

9. The method according to claim 8, characterized in that The baking temperature of the coating is 70°C to 90°C.

10. A lithium battery, characterized in that: The lithium battery comprises: a positive electrode, a negative electrode, an electrolyte and a separator, the active material of the positive electrode comprises: one or more of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium-rich manganese base, lithium manganese iron phosphate and lithium nickel manganese oxide, and the separator is a porphyrin-based MOF modified separator as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Functional diaphragm coating material for lithium-sulfur battery and preparation method of functional diaphragm coating material

    CN110890504A

  • Metal organic framework composite material for battery diaphragm as well as preparation method and application of metal organic framework composite material

    CN115458744A

  • Composite diaphragm, preparation method thereof, electrochemical device and electric device

    CN116805752A

  • Modified metal organic framework modified battery diaphragm and preparation method thereof

    CN118249035A

  • Electrode separators

    US20230178848A1

Cited By

  • Diaphragm and preparation method thereof, battery, energy storage device and electric equipment

    CN121035527A