Container coated with MgAl2O4 spinel coating and corundum
By coating high-content MgAl2O4 spinel and corundum on the inner wall of the container, the problem of short service life of the container during the manufacturing process of lithiated transition metal oxide powder is solved, and the production efficiency and stability of lithium-ion battery modules are achieved sex.
Patent Information
- Application Number
- CN202280085329.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-23
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-29
AI Technical Summary
The existing containers have a short service life in the manufacturing process of lithiated transition metal oxide powder, resulting in unstable production efficiency and quality of lithium-ion battery modules.
The surface of the inner wall of the container is covered with at least 80% of a specific coating. The coating consists of crystalline phases such as MgAl2O4 spinel, corundum, etc., and the coating thickness is between 50μm and 1500μm to ensure the wear resistance and oxidation resistance of the container.
It extends the service life of the container, improves the cycle number of lithiated transition metal oxide powder, and enhances the production stability and efficiency of lithium-ion battery modules.
Smart Images

Figure GDA0004949562830000111 
Figure GDA0004949562830000131
Abstract
Description
Technical Field
[0001] The invention relates to a container, the surface of the inner wall of which is at least partially, preferably more than 80%, covered by a coating, and to the use of said container for producing lithium-containing oxide powders, in particular oxides of one or several lithiated transition metals. Background Art
[0002] The demand for lithium-ion batteries is increasing. Many of them contain lithium-containing oxides, especially oxides of one or several lithiated transition metals, especially LiFePO 4 (or LPF), LiMn 2 O 4 A component, typically the cathode, made of lithium-nickel-cobalt-manganese (or LMO) or lithium-nickel-cobalt-manganese (or Li-NMC) oxide.
[0003] The cathode is generally produced by shaping a powder of the oxide of the lithiated transition metal or metals.
[0004] The conventional method for producing the powders comprises producing a mixture of oxides and / or different oxide precursors, followed by a heat treatment to enable solid phase synthesis of one or more oxides of lithiated transition metals. During the heat treatment, the mixture is placed in a container, usually referred to as a "sagger". The conditions for synthesizing the powders and the mixture, in particular the lithium-containing elements, place the container under a particular pressure.
[0005] There is a need to increase the useful life of the containers.
[0006] It is an object of the present invention to at least partially meet this need. SUMMARY OF THE INVENTION
[0008] According to the invention, this object is achieved by a container, the surface portion of the inner wall of the container, preferably more than 80%, preferably on the entire inner wall, is covered by a coating, the coating having the following crystalline phases, calculated as weight percentages based on the total weight of the crystalline phases:
[0009] -MgAl 2 O 4 Spinel: greater than 25% and up to 60%, and
[0010] - Removal of MgAl 2 O 4 Crystalline phases other than spinel and corundum: <10%, and
[0011] -Corundum: Refill to 100%.
[0012] The inventors have found that the coated container according to the invention exhibits lower degradation during its use, which allows a longer service life and in particular a greater number of cycles for the production of one or several lithiated transition metal oxide powders.
[0013] According to preferred but non-limiting embodiments of the present invention, which can be combined with each other if appropriate:
[0014] - the coating has a spinel content, measured as a percentage by weight based on the crystalline phase, of greater than 30%, preferably greater than 35% and / or less than 55%, preferably less than 50%;
[0015] - the container contains more than 90% by weight, preferably more than 95% by weight, preferably more than 99% by weight of oxides, carbides, nitrides, oxynitrides, borides and mixtures thereof;
[0016] the coating has a thickness of greater than 50 μm, preferably greater than 100 μm, preferably greater than 200 μm, preferably greater than 300 μm and less than 2000 μm, preferably less than 1500 μm, preferably less than 1000 μm, preferably less than 800 μm;
[0017] - the surface of the covered inner wall includes the bottom of the container and the part of the side in contact with the bottom;
[0018] - more than 85%, preferably more than 90%, preferably more than 95% of the surface of the inner wall is covered;
[0019] - the coating extends substantially over the entire surface of the inner wall of the container;
[0020] - the container contains more than 90% by weight, preferably more than 95% by weight, of oxides;
[0021] - The container contains Al 2 O 3 、MgO、ZrO 2 、SiO 2 , Y 2 O 3 and mixtures thereof;
[0022] - The container has more than 90%, preferably more than 95%, Al in terms of oxide weight percentage 2 O 3 +MgO+ZrO 2 +SiO 2 +Y 2 O 3 content;
[0023] - The container has more than 90%, preferably more than 95%, Al in terms of oxide weight percentage2 O 3 content;
[0024] - The container has more than 90%, preferably more than 95%, SiO in terms of oxide weight percentage 2 content;
[0025] - The container has more than 90%, preferably more than 95%, Al in terms of oxide weight percentage 2 O 3 +MgO content;
[0026] - The container has more than 90%, preferably more than 95%, Al in terms of oxide weight percentage 2 O 3 +Y 2 O 3 content;
[0027] - The container has more than 90%, preferably more than 95%, Al in terms of oxide weight percentage 2 O 3 +MgO+SiO 2 content;
[0028] - The container has more than 90%, preferably more than 95%, Al in terms of oxide weight percentage 2 O 3 +ZrO 2 +SiO 2 content;
[0029] - The container has more than 90%, preferably more than 95%, Al in terms of oxide weight percentage 2 O 3 +ZrO 2 content;
[0030] - The container has more than 90%, preferably more than 95%, Al in terms of oxide weight percentage 2 O 3 +SiO 2 content;
[0031] - the container contains more than 90%, preferably more than 95%, of corundum, MgAl 2 O 4 Spinel, cordierite, mullite, optionally stabilized zirconium dioxide, periclase and mixtures thereof;
[0032] - In total and by weight percentage based on the weight of the crystalline phase, the container contains more than 90%, preferably more than 95%, of corundum, or mullite, or a mixture of corundum and cordierite, or a mixture of corundum and mullite, or corundum and MgAl2 O 4 A mixture of spinel, or a mixture of corundum and cordierite and spinel, or a mixture of corundum and zirconium dioxide, or a mixture of corundum and mullite and zirconium dioxide, or a mixture of cordierite and mullite;
[0033] - the container contains more than 90% by weight, preferably more than 95% by weight, of carbides, nitrides, oxynitrides, borides and mixtures thereof;
[0034] - the container contains more than 90% by weight, preferably more than 95% by weight, of carbides, nitrides, SiAlON and mixtures thereof;
[0035] - the container contains more than 90% by weight, preferably more than 95% by weight, of silicon carbide, silicon nitride, SiAlON and mixtures thereof;
[0036] - the container contains more than 90% by weight, preferably more than 95% by weight, of a mixture of silicon carbide and silicon nitride;
[0037] - the container has a perimeter selected from a polygonal, circular or elliptical shape;
[0038] - the container comprises a bottom and at least one side, preferably having an average thickness of less than 20 mm and greater than 2 mm;
[0039] - The container has a volume greater than 0.1 litre and less than 25 litres.
[0040] The invention also relates to the use of a coated container according to the invention for producing lithium-containing oxide powders, in particular oxides of one or several lithiated transition metals.
[0041] definition
[0042] - "Ceramic" is understood to mean a product which is neither metallic nor organic. In the context of the present invention, carbon is considered to be a ceramic product.
[0043] - "Coating" is understood to mean a layer of material having properties different from those of the container surface.
[0044] A "precursor" of a crystalline oxide is understood to mean one or more materials which, after a heat treatment at a temperature above 1100° C., preferably in air, give rise to said crystalline oxide. For example, a corundum precursor may be a transition alumina or boehmite or aluminum hydroxide.
[0045] - For the sake of clarity, the chemical formulas of simple oxides are used to indicate the content of these oxides in the composition. For example, "MgO" or "Al 2 O 3” refers to the content of these simple oxides in the composition under consideration, while "magnesium oxide" and "aluminum oxide" are used to represent MgO and Al 2 O 3 for the effective presence of the phases of these constituent oxides.
[0046] - "Corundum" is generally understood to refer to aluminum oxide in a rhombohedral crystal form.
[0047] - "Sialon", or SiAlON, is a nitrogen oxide compound of at least the elements Si, Al, and N, in particular a compound conforming to one of the following formulas:
[0048] - Si x Al y O u N v , where:
[0049] - x is greater than or equal to 0, greater than 0.05, greater than 0.1, or greater than 0.2, and less than or equal to 1, less than or equal to 0.8, or less than or equal to 0.4,
[0050] - y is greater than or equal to 0, or greater than 0.1, greater than 0.3, or greater than 0.5, and less than or equal to 1,
[0051] - u is greater than 0, greater than 0.1, or greater than 0.2, and less than or equal to 1 or less than or equal to 0.7,
[0052] - v is greater than 0, greater than 0.1, greater than 0.2, or greater than 0.5, or greater than 0.7, and less than or equal to 1,
[0053] - x + y > 0,
[0054] x, y, u, and v are stoichiometric indices and are normalized with respect to the highest index such that the highest index is equal to 1;
[0055] - Me x Si 12-(m+n) Al (m+n) O n N 16-n , where 0 ≤ x ≤ 2, Me is a cation selected from lanthanide elements, Fe, Y, Ca, Li cations, and mixtures thereof, 0 ≤ m ≤ 12, 0 ≤ n ≤ 12, and 0 < n + m ≤ 12, and is commonly referred to as "α'-SiAlON" or "SiAlON-α'".
[0056] - Unless otherwise mentioned, all oxide contents are in weight percentages of the oxide. The weight content of the oxide of a metallic element refers to the total content of the element expressed in the form of the most stable oxide according to the usual practice in the industry.
[0057] The sum of the oxide contents does not imply the presence of all these oxides.
[0058] - “Comprising” or “including” should be interpreted without limitation as meaning that elements other than those stated may be present. DETAILED DESCRIPTION OF THE INVENTION
[0060] container
[0061] The container is preferably ceramic.
[0062] Preferably, the container comprises more than 90 wt. %, preferably more than 95 wt. %, preferably more than 99 wt. %, preferably more than 99.5 wt. % of oxides, carbides, nitrides, oxynitrides, borides and mixtures thereof.
[0063] The container preferably comprises more than 90% by weight, preferably more than 95% by weight, preferably more than 99% by weight, preferably more than 99.5% by weight of:
[0064] - oxide, or
[0065] - carbides, nitrides, oxynitrides, borides and mixtures thereof, preferably carbides, nitrides, oxynitrides and mixtures thereof, preferably carbides, nitrides, SiAlON and mixtures thereof, preferably carbides, nitrides and mixtures thereof, preferably silicon carbide, silicon nitride and mixtures thereof.
[0066] In a first embodiment, the container comprises more than 90 wt. %, preferably more than 95 wt. %, preferably more than 99 wt. %, preferably more than 99.5 wt. % oxides.
[0067] Preferably, the oxide is selected from or comprises Al 2 O 3 、MgO、ZrO 2 、SiO 2 , Y 2 O 3 and mixtures thereof.
[0068] The container preferably has more than 90 wt. %, preferably more than 95 wt. %, preferably more than 98 wt. % Al, based on oxide weight percentage. 2 O 3 +MgO+ZrO 2 +SiO 2 +Y 2 O 3 content.
[0069] The container preferably has more than 90 wt. %, preferably more than 95 wt. %, preferably more than 98 wt. % Al, based on oxide weight percentage. 2 O3 +MgO+ZrO 2 +SiO 2 content.
[0070] More preferably, the container has greater than 90 wt. %, preferably greater than 95 wt. %, preferably greater than 98 wt. % Al, calculated as oxide weight percentage. 2 O 3 +MgO+SiO 2 content.
[0071] In one embodiment of the first embodiment, the container has greater than 90 wt%, preferably greater than 95 wt%, preferably greater than 98 wt%, preferably greater than 99 wt% Al, calculated as oxide weight percentage. 2 O 3 content.
[0072] In one embodiment of the first embodiment, the container has greater than 90 wt. %, preferably greater than 95 wt. %, preferably greater than 98 wt. %, preferably greater than 99 wt. % SiO2 by weight percentage. 2 content.
[0073] In one embodiment of the first embodiment, the container has greater than 90 wt%, preferably greater than 95 wt%, preferably greater than 98 wt%, preferably greater than 99 wt% Al, calculated as oxide weight percentage. 2 O 3 +MgO content.
[0074] In one embodiment of the first embodiment, the container has greater than 90 wt%, preferably greater than 95 wt%, preferably greater than 98 wt%, preferably greater than 99 wt% Al, calculated as oxide weight percentage. 2 O 3 +Y 2 O 3 content.
[0075] In one embodiment of the first embodiment, the container has greater than 90 wt%, preferably greater than 95 wt%, preferably greater than 98 wt%, preferably greater than 99 wt% Al, calculated as oxide weight percentage. 2 O 3 +MgO+SiO 2 content.
[0076] In one embodiment of the first embodiment, the container has greater than 90 wt%, preferably greater than 95 wt%, preferably greater than 98 wt%, preferably greater than 99 wt% Al, calculated as oxide weight percentage. 2 O 3+ZrO 2 +SiO 2 content.
[0077] In one embodiment of the first embodiment, the container has greater than 90 wt%, preferably greater than 95 wt%, preferably greater than 98 wt%, preferably greater than 99 wt% Al, calculated as oxide weight percentage. 2 O 3 +ZrO 2 content.
[0078] In one embodiment of the first embodiment, the container has greater than 90 wt%, preferably greater than 95 wt%, preferably greater than 98 wt%, preferably greater than 99 wt% Al, calculated as oxide weight percentage. 2 O 3 +SiO 2 content.
[0079] Preferably, the container comprises, in total, more than 90%, preferably more than 95%, of corundum, MgAl 2 O 4 Spinel, cordierite, mullite, optionally stabilized zirconium dioxide, periclase and mixtures thereof. More preferably, the container comprises a total of greater than 90%, preferably greater than 95%, preferably greater than 99%, preferably greater than 99.5% of corundum, MgAl 2 O 4 Spinel, cordierite, mullite, optionally stabilized zirconium dioxide and mixtures thereof.
[0080] Preferably, the container comprises more than 90%, preferably more than 95%, of corundum, or mullite, or a mixture of corundum and cordierite, or a mixture of corundum and mullite, or a mixture of corundum and MgAl 2 O 4 A mixture of spinel, or a mixture of corundum and cordierite and spinel, or a mixture of corundum and zirconium dioxide, or a mixture of corundum and mullite and zirconium dioxide, or a mixture of cordierite and mullite.
[0081] In a second embodiment, the container comprises greater than 90%, preferably greater than 95%, preferably greater than 99%, preferably greater than 99.5% of carbides, nitrides, oxynitrides, borides and mixtures thereof, preferably carbides, nitrides, oxynitrides and mixtures thereof, preferably carbides, nitrides, SiAlON and mixtures thereof.
[0082] The container preferably contains more than 90 wt. %, preferably more than 95 wt. %, preferably more than 98 wt. %, preferably more than 99 wt. % of silicon carbide, silicon nitride, SiAlON and mixtures thereof.
[0083] In one embodiment of said second embodiment, the container comprises greater than 90% silicon carbide and the supplement comprises silicon metal.
[0084] More preferably, the container comprises more than 90 wt. %, preferably more than 95 wt. %, preferably more than 98 wt. %, preferably more than 99 wt. % of silicon carbide, silicon nitride and mixtures thereof.
[0085] In one embodiment of said second embodiment, the container comprises greater than 90 wt. %, preferably greater than 95 wt. %, preferably greater than 98 wt. %, preferably greater than 99 wt. % silicon carbide.
[0086] In one embodiment of the second embodiment, the container contains more than 90% by weight, preferably more than 95% by weight, preferably more than 98% by weight, preferably more than 99% by weight of a mixture of silicon carbide and silicon nitride, preferably the weight ratio of the amount of silicon carbide to the amount of silicon nitride is greater than 1, preferably greater than 2 and less than 10, preferably less than 8, preferably less than 6.
[0087] Preferably, the container comprises, as a percentage by weight based on the weight of the crystalline phase, a total of more than 90%, preferably more than 95% of:
[0088] -Corundum, MgAl 2 O 4 Spinel, cordierite, mullite, optionally stabilized zirconium dioxide, periclase and mixtures thereof, preferably corundum, MgAl 2 O 4 spinel, cordierite, mullite, optionally stabilized zirconium dioxide and mixtures thereof, preferably corundum, spinel, cordierite and mixtures thereof, or
[0089] -Silicon carbide, silicon nitride and mixtures thereof.
[0090] The container may have any shape.
[0091] The perimeter of the container according to the invention may be chosen from polygonal, in particular rectangular and square, circular or oval.
[0092] Preferably, the container according to the present invention comprises a bottom and at least one side, the bottom and at least one side preferably having an average thickness of less than 20 mm, more preferably less than 15 mm, or even less than 10 mm and / or preferably greater than 2 mm, preferably greater than 4 mm, more preferably greater than 5 mm.
[0093] In one embodiment, the thickness of the bottom of the container is greater than the thickness of its sides, preferably 10% greater, preferably 20% greater, preferably 30% greater.
[0094] In one embodiment, the bottom and sides of the container have a difference in thickness of less than 10%, preferably less than 5%.Preferably, in such embodiments, the thickness of the bottom of the container is substantially the same as the thickness of the sides thereof.
[0095] In one embodiment, the thickness of the wall is not constant. Preferably, the thickness of the side is greater on the side of the container bottom. Preferably, the thickness of the part of the side in contact with the container bottom is 10% greater than the thickness of the part of the side opposite to the container bottom.
[0096] In one embodiment, the container according to the present invention has a length (i.e. the maximum length) of less than 500 mm, preferably less than 400 mm, and / or preferably greater than 100 mm, preferably greater than 200 mm, and a width (i.e. the smallest dimension measured perpendicular to the length) of less than 500 mm, preferably less than 400 mm, and / or preferably greater than 100 mm, preferably greater than 200 mm.
[0097] In one embodiment, the angle between the bottom of the container and the at least one side is equal to 90°. In one embodiment, the angle is greater than 90° and less than 100°.
[0098] In one embodiment, the container has a diameter of less than 500 mm, preferably less than 400 mm and / or preferably greater than 100 mm, preferably greater than 200 mm.
[0099] Preferably, the container has a volume greater than 0.1 liter, preferably greater than 1 liter, preferably greater than 2 liters, preferably greater than 3 liters and / or preferably less than 25 liters, preferably less than 20 liters, preferably less than 15 liters.
[0100] In one embodiment, the CMC bottom and sides of the container according to the present invention form an integral assembly. In other words, the bottom and the sides are the same part, and the connection between the bottom and the sides comprises a radius preferably greater than 5 mm, preferably greater than 10 mm, preferably greater than 20 mm.
[0101] In one embodiment, the container is an assembly of different parts, such as plates, and the connections between the various parts can be achieved in particular by means of mortise and tenon assemblies, and / or bracket-type assemblies, and / or embedded assemblies (in particular using notches or grooves), and / or ceramic pins, and / or ceramic screws, and / or ceramic rivets, and / or ceramic cotter pins.
[0102] coating
[0103] The coating has the following crystalline phases, measured by weight percentage based on the crystalline phase:
[0104] -MgAl 2 O 4 Spinel: greater than 25% and up to 60%, and
[0105] - Removal of MgAl 2 O 4 Crystalline phases other than spinel and corundum: <10%,
[0106] -Corundum: Refill to 100%.
[0107] The crystalline phases present in a coating can usually be identified by X-ray diffraction on the coating.
[0108] The acquisition of the diffraction patterns was carried out with an instrument of the D8 Endeavour type from Bruker over an angular range 2θ of 5° to 80°, with a step size of 0.01° and a counting time of 0.34 seconds per step. The front optical assembly had a main slit of 0.3° and a Soller slit of 2.5°. The sample was rotated on its axis at a speed equal to 5 rpm using an automatic cutter. The rear optical assembly had a Soller slit of 2.5°, a 0.0125 mm nickel foil and a 1D detector with an opening equal to 4°.
[0109] The diffraction patterns were then qualitatively analyzed using EVA software and the ICDD2016 database.
[0110] Once the phases present were identified, the diffraction patterns were quantitatively analyzed using HighScore Plus software with Rietveld refinement according to the following strategy:
[0111] - Perform a refinement of the background signal using the "Process", "Determine background" function and select the following options: "Bending factor" equal to 1, "Granularity" equal to 40;
[0112] - By convention, ICDD files are selected for current phases that are identified and quantifiable, and therefore considered during refinement;
[0113] - Automatic refinement was then performed by selecting the previously determined background signal ("Use available background") and by selecting the "Automatic, option Phase fitting - default Rietveld" mode;
[0114] - A manual refinement of the "B Global" parameters was then performed for all selected phases simultaneously.
[0115] The inventors have demonstrated that, when producing oxide powders comprising lithium, in particular oxides of one or more lithiated transition metals, such a coating can increase the service life of the container.
[0116] The inventors have also demonstrated that MgAl with more than 60% 2 O 4 The spinel-containing coatings exhibit cracking and / or flaking of the container surface when the temperature is raised to the operating temperature, which does not allow such coatings of the container to have an improved service life.
[0117] Contains less than 10% MgAl 2 O 4 Coated containers with a spinel-containing coating do not have an improved service life.
[0118] The coating preferably has more than 30%, preferably more than 35% and preferably less than 55%, preferably less than 50% MgAl, as a percentage by weight based on the crystalline phase. 2 O 4 Spinel content.
[0119] Preferably, the coating has less than 8%, preferably less than 5%, excluding MgAl, as a percentage by weight based on the crystalline phase. 2 O 4 Preferably, the coating has a crystalline phase content other than spinel and corundum. 2 O 4 The content of crystalline phases other than spinel and corundum is essentially zero.
[0120] Preferably, the coating has an amount of amorphous phase of less than 10%, preferably less than 5%, preferably substantially zero.
[0121] Preferably, the coating has the following chemical composition in terms of oxide weight percentage:
[0122] MgO: >2.8%, preferably >4%, preferably >5.5%, preferably >7%, preferably >8.5% and preferably <16.9%, preferably <15.5%, preferably <14%, and / or
[0123] -Al 2 O 3 :>73.1%, preferably>75%, preferably>78%, preferably>80%, preferably>83% and preferably<97%, preferably<95%, preferably<92%, preferably<90%, and / or
[0124] - Removal of MgO and Al 2 O 3 Oxides other than: <10%, preferably <8%, preferably <6%, preferably <5%, preferably <3%, preferably <1%, preferably <0.5%.
[0125] The coating consists of more than 90 wt. %, preferably more than 95 wt. %, preferably more than 98 wt. %, preferably more than 99 wt. %, preferably more than 99.5 wt. % oxides. Preferably, the coating consists essentially of oxides.
[0126] The thickness of the coating is preferably greater than 50 μm, preferably greater than 100 μm, preferably greater than 200 μm, preferably greater than 300 μm, or even greater than 400 μm, or even greater than 500 μm, or even greater than 600 μm and / or preferably less than 2000 μm, preferably less than 1500 μm, preferably less than 1000 μm, preferably less than 800 μm.
[0127] Preferably, the covered inner wall surface includes the bottom of the container and the part of the side in contact with the bottom. In other words, the coating extends over the lower part of the side of the container, the container being considered to be in its operating position, the part being the part in contact with the powder during use of the container.
[0128] Preferably, more than 85%, preferably more than 90%, preferably more than 95%, preferably more than 96%, preferably more than 98%, preferably more than 99% of the inner wall surface of the container is covered by the coating. Preferably, the coating extends substantially over the entire surface of the inner wall of the container.
[0129] Preferably, at least a portion of the surface of the outer wall of the bottom of the container, preferably the entire surface, is covered with the coating.
[0130] In one embodiment, more than 90%, preferably more than 95%, preferably more than 99% of the total surface area of the wall of the container is covered with the coating.
[0131] The coating can be applied to at least a portion of the surface of the inner wall of the container according to any technique known to those skilled in the art, in particular by application with a brush, by spraying (in particular wet spraying), by vacuum impregnation, by dipping. Preferably, the coating is applied by wet spraying comprising one or more MgAl 2 O 4 The suspension is applied by mixing the corundum powder with one or more corundum or corundum precursor powders. Preferably, the suspension does not contain corundum precursor powders.
[0132] Preferably, the coating has been subjected to a heat treatment before its use, the maximum temperature reached during said heat treatment being preferably greater than 1100°C, preferably greater than 1200°C and preferably less than 1500°C, preferably less than 1400°C.
[0133] The holding time at the maximum temperature is preferably greater than 0.5 hours and less than 5 hours, preferably less than 2 hours. Example
[0134] To illustrate the invention, the following non-limiting examples are given.
[0135] Manufacturing scheme of the embodiment
[0136] To produce the examples, N-Durance plates sold by Saint-Gobain Performance Ceramics and Refractories were machined on 6 faces with dimensions of 50×50×10 mm. 3 of tiles.
[0137] The large surface of each tile is subsequently coated by wet spraying of the suspension.
[0138] The suspensions used to obtain the various coatings were prepared as follows.
[0139] A mixture M of aluminum oxide powder and aluminum hydroxide powder is obtained with a mass purity greater than 99%. The mixture M has a median particle size D equal to 7 μm. 50 and D equal to 51 μm 90 .
[0140] The mixture was then produced according to Table 1 below (in weight percent).
[0141] [Table 1]
[0142]
[0143] Subsequently, 0.3% of sodium silicate and 0.5% of a stabilizing solution were added to each mixture to prevent any segregation in the coating when it was applied to the tile, and alumina beads were added, the percentages of sodium silicate to the stabilizing suspension being weight percentages based on the total weight of the mixture M and the spinel powder.
[0144] The solution was placed in a jar and spun on a rotating jar for 10 minutes to mix the ingredients.
[0145] Subsequently, 40% of water and 2.5% of a binder dispersion were added to the tank, in particular in order to achieve adequate wear resistance for the coating, the percentages being by weight based on the total weight of the mixture M and the spinel powder.
[0146] The jar was closed and then rotated using a rotating jar for 8 hours to obtain a homogeneous suspension.
[0147] The beads are subsequently separated from the suspension by sieving.
[0148] The suspension is then placed in a compressed air gun and sprayed onto the large surface of the tile in order to obtain, after a consolidation step by sintering, a coating of substantially uniform thickness equal to 300 μm.
[0149] The coated tiles were then dried in an oven at 70°C for 12 hours.
[0150] Finally, the coated tiles were subjected to the following consolidation heat treatment in an electric furnace in air:
[0151] - at a rate of 300°C / h to 1450°C,
[0152] - 1450℃ for 1 hour,
[0153] - Decrease to 500°C at a rate equal to 300°C / h and then free decrease.
[0154] The coated tiles thus obtained were subsequently subjected to a degradation resistance test as described below:
[0155] The degradation resistance of lithium nickel manganese cobalt (Li-NMC) oxide powder was evaluated on the above-described coated tiles according to Examples 1 to 4, the surface of the tile in contact with the powder being the surface having the aforementioned coating.
[0156] The powder of lithium nickel manganese cobalt oxide used was produced in the following manner:
[0157] By adding NaOH and NH under stirring at a temperature equal to 50 °C 4 OH, an aqueous solution of nickel nitrate, cobalt nitrate and manganese nitrate in a stoichiometric ratio of 0.8:0.1:0.1 was coprecipitated to obtain Ni 0.8 Co 0.1 Mn 0.1 (OH) 2 powder.
[0158] After drying the precipitate, the mixture was heated to 1.03% LiOH. 2 O versus Ni 0.8 Co 0.1 Mn 0.1 (OH) 2 The molar ratio of LiOH.H 2 O added to Ni 0.8 Co 0.1 Mn 0.1 (OH) 2 The mixture was then mixed vigorously.
[0159] The mixture was then heat treated at 480°C for 4 hours.
[0160] The powder obtained after the heat treatment was pulverized in an agate mortar. The powder obtained from the pulverization was the powder used in the degradation resistance test.
[0161] For each example, 4.5 grams of the powder was placed on the center portion of the tile being tested, taking care not to cover the peripheral surface of the tile with powder.
[0162] The tiles are then placed in an electric tube furnace, the tube of which is made of alumina, to undergo the following heat treatment cycle:
[0163] - Raise the temperature to 800°C at a rate of 200°C / h,
[0164] -Keep at 800℃ for 10 hours,
[0165] - Decrease to 500°C at a rate equal to 200°C / h and then decrease freely to room temperature.
[0166] During the entire heat treatment process, oxygen was circulated in the tube at a flow rate of 20 L / min.
[0167] The tile was then removed from the furnace. The powder present on the top of the tile was removed and 4.5 grams of new powder were placed again on the central part of the tile under test, taking care not to cover the peripheral surface of the tile with powder. The tile was then placed in an electric tube furnace, the tube being made of alumina, to undergo a second heat treatment cycle identical to the first heat treatment cycle.
[0168] The tile was then removed from the furnace. The powder present on top of the tile was removed. The same protocol as previously described was repeated three more times so that each tile was subjected to a total of five heat treatment cycles in the presence of the above powder.
[0169] The tiles are then removed from the furnace and each tile is cut to obtain a cross section of the center region of the tile. The cross section is coated with resin and mirror polished.
[0170] Each polished sample was then observed using a scanning electron microscope, using a magnification of ×200 to ×500.
[0171] Table 2 below summarizes the results obtained.
[0172] [Table 2]
[0173]
[0174] Comparison of Examples 1 and 2 to 4 shows that the coatings of Examples 2 to 4 still exist after the degradation resistance test, unlike the coating of Example 1 which almost completely disappears.
[0175] However, a comparison of Examples 2 to 4 shows that the coating of Example 2, with a spinel amount equal to 15%, comprises a plurality of cracks present on the outer surface of the coating and reaching the interface between the coating and the surface of the tile.
[0176] After the degradation resistance test, the coating of Example 3 with a spinel amount equal to 30% had some cracks present on the outer surface of the coating and not extending to the interface between the coating and the tile surface.
[0177] The coating of Example 4, with a spinel amount equal to 45%, has the best resistance; no cracks were observed after the degradation resistance test.
[0178] These results show the effectiveness of the container according to the invention.
[0179] Of course, the invention is not limited to the embodiments described, which are provided as illustrative and non-limiting examples.
[0180] In particular, the product according to the invention is not limited to a specific shape or size.
Claims
1. A container for producing a lithium-containing oxide powder, the surface of the inner wall of which is at least partially, preferably more than 80%, covered by a coating having the following crystalline phases, as percentages and based on the total weight of the crystalline phases: -MgAl2O4 spinel: greater than 25% and up to 60%, and - Crystalline phases other than MgAl2O4 spinel and corundum: <10%, -Corundum: Refill to 100%.
2. Container according to the preceding claim: - wherein the coating has a spinel content, measured as a percentage by weight based on the crystalline phase, of greater than 30% and / or less than 55%, and / or - contains more than 90% by weight of oxides, carbides, nitrides, oxynitrides, borides and mixtures thereof, and / or - wherein the thickness of the coating is greater than 50 μm and less than 2000 μm, and / or - wherein the surface of the inner wall covered by the coating includes the bottom of the container and the portion of the side in contact with the bottom, and / or - More than 85% of the surface of its inner wall is covered by the coating.
3. The container according to claim 1 or 2: - wherein the coating has a spinel content greater than 35% and / or less than 50%, measured as a percentage by weight based on the crystalline phase, and / or - contains more than 95% by weight of oxides, carbides, nitrides, oxynitrides, borides and mixtures thereof, and / or - wherein the thickness of the coating is greater than 100 μm and less than 1500 μm, and / or - More than 90% of the surface of its inner wall is covered by the coating.
4. The container according to any one of claims 1 to 3: - contains more than 99% by weight of oxides, carbides, nitrides, oxynitrides, borides and mixtures thereof, and / or - wherein the thickness of the coating is greater than 200 μm and less than 1000 μm, and / or - More than 95% of the surface of its inner wall is covered by the coating.
5. Container according to any one of the preceding claims: - wherein the thickness of the coating is greater than 300 μm and less than 800 μm, and / or - Its coating extends substantially over the entire surface of the inner wall of said container.
6. The container according to claim 1, comprising more than 90% by weight, preferably more than 95% by weight, of oxides.
7. A container according to the preceding claim, comprising Al2O3, MgO, ZrO2, SiO2, Y2O3 and mixtures thereof.
8. Container according to one of the preceding claims, having an Al2O3+MgO+ZrO2+SiO2+Y2O3 content, expressed as percentage by weight of oxides, of greater than 90%, preferably greater than 95%.
9. The container according to claim 1, comprising: - an Al2O3 content greater than 90%, preferably greater than 95%, calculated as a percentage by weight of oxides, or - a SiO2 content greater than 90%, preferably greater than 95%, calculated as a percentage by weight of oxides, or - an Al2O3+MgO content greater than 90%, preferably greater than 95%, calculated as a percentage by weight of oxides, or - an Al2O3+Y2O3 content greater than 90%, preferably greater than 95%, calculated as a percentage by weight of oxides, or - an Al2O3+MgO+SiO2 content greater than 90%, preferably greater than 95%, calculated as a percentage by weight of oxides, or - an Al2O3+ZrO2+SiO2 content greater than 90%, preferably greater than 95%, calculated as percentage by weight of oxides, or - an Al2O3+ZrO2 content greater than 90%, preferably greater than 95%, calculated as a percentage by weight of oxides, or - an Al2O3+SiO2 content greater than 90%, preferably greater than 95%, calculated as percentage by weight of oxides.
10. The container according to claim 1, comprising, in total and as percentages by weight based on the weight of the crystalline phases, more than 90%, preferably more than 95%, of corundum, MgAl2O4 spinel, cordierite, mullite, optionally stabilized zirconium dioxide, periclase and mixtures thereof.
11. The container according to the preceding claim, comprising, in total and as a percentage based on the total weight of the crystalline phases, more than 90%, preferably more than 95%, of corundum, or mullite, or a mixture of corundum and cordierite, or a mixture of corundum and mullite, or a mixture of corundum and MgAl2O4 spinel, or a mixture of corundum and cordierite and spinel, or a mixture of corundum and zirconium dioxide, or a mixture of corundum and mullite and zirconium dioxide, or a mixture of cordierite and mullite.
12. The container according to claim 1, comprising more than 90% by weight, preferably more than 95% by weight, of carbides, nitrides, oxynitrides, borides and mixtures thereof.
13. Container according to the preceding claim, comprising a total of more than 90% by weight, preferably more than 95% by weight, of carbides, nitrides, SiAlON and mixtures thereof.
14. Container according to the preceding claim, comprising a total of more than 90% by weight, preferably more than 95% by weight, of silicon carbide, silicon nitride, SiAlON and mixtures thereof.
15. Container according to the preceding claim, comprising more than 90% by weight, preferably more than 95% by weight, of a mixture of silicon carbide and silicon nitride.
16. Container according to any one of the preceding claims: - having a perimeter selected from polygonal, circular or elliptical, and / or - including a bottom and at least one side, preferably having an average thickness of less than 20 mm and greater than 2 mm, and / or - has a volume greater than 0.1 litre and less than 25 litres.
17. Container according to any of the preceding claims, for use in the production of powders of one or more lithiated transition metal oxides.