Non-conformal oxide film deposition using carbonaceous inhibitors

By using carbon-containing inhibitors and plasma technologies in the oxide film deposition cycle, the problems of non-conformal growth and pore formation of oxide films in electronic equipment manufacturing are solved, and a more uniform and efficient film filling effect is achieved.

CN119053726APending Publication Date: 2024-11-29LAM RES CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035402.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-21
Filing Date
2023-04-06
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the process of manufacturing electronic equipment, it is difficult for the prior art to effectively control the non-conformal growth of oxide films, especially in the process of gap filling on the substrate, problems of pore formation and uneven film growth are prone to occur.

Method used

By introducing carbon-containing inhibitors in the oxide film deposition cycle, the reaction of oxide film precursors and oxygen-containing gas is controlled, plasma is formed using radio frequency power sources, and carbon-containing inhibitors are introduced under specific conditions to regulate membrane growth This method is to achieve non-conformal growth and avoid pore formation.

Benefits of technology

It realizes uniform filling in the gap, avoids pore formation, improves the thickness control and uniformity of the film, and enhances the filling effect of the oxide film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053726A_ABST
    Figure CN119053726A_ABST
Patent Text Reader

Abstract

Examples are disclosed that relate to the use of carbon-containing inhibitors to non-conformally grow an oxide film on a substrate. An example includes performing a plurality of oxide film deposition cycles, at least one of the plurality of oxide film deposition cycles includes exposing the substrate to an oxide film precursor to adsorb the oxide film precursor to the substrate, exposing the substrate to an oxygen-containing gas, reacting the oxide film precursor with the oxygen-containing gas, and exposing the substrate to a carbon-containing inhibitor.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] The electronic device manufacturing process may involve many steps of material deposition, patterning, and removal to form an integrated circuit on a substrate. Various methods may be used to deposit a material film onto a substrate. As an example, atomic layer deposition (ALD) forms a film using one or more deposition cycles. In an ALD deposition cycle, an oxide film precursor gas is adsorbed onto the surface of a substrate placed in a processing chamber. Excess oxide film precursor is purged from the chamber, and the adsorbed oxide film precursor is chemically converted to a film on the substrate, for example, by oxidation to form an oxide film. A highly conformal film having a target thickness may be grown via one or more deposition cycles. Summary of the invention

[0002] This summary is provided to introduce a selection of concepts in a simplified form, which concepts are further described in the detailed description below. This summary is not intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter. Furthermore, the claimed subject matter is not limited to implementations that address any or all of the disadvantages noted in any part of this disclosure.

[0003] Examples involving the use of a carbon-containing inhibitor to non-conformally grow an oxide film in a gap are disclosed. One example provides a method of forming an oxide film on a substrate, the method comprising performing a plurality of oxide film deposition cycles, at least one of the plurality of oxide film deposition cycles comprising exposing the substrate to an oxide film precursor to adsorb the oxide film precursor to the substrate, exposing the substrate to an oxygen-containing gas, reacting the oxide film precursor with the oxygen-containing gas, and exposing the substrate to a carbon-containing inhibitor.

[0004] In some such examples, the method includes an atomic layer deposition process.

[0005] In some such examples, additionally or alternatively, a subsequent oxide film deposition cycle in the plurality of oxide film deposition cycles performed after the at least one oxide film deposition cycle omits exposing the substrate to a carbon-containing inhibitor.

[0006] In some such examples, reacting the oxide film precursor with the oxygen-containing gas additionally or alternatively includes forming a plasma including the oxygen-containing gas.

[0007] In some such examples, the method additionally or alternatively includes reacting the plasma with an oxidizable carbon-containing species from a previous oxide film deposition cycle in the plurality of oxide film deposition cycles.

[0008] In some such examples, the substrate additionally or alternatively includes alternating layers of a first material and a second material, wherein gaps are formed in the alternating layers of materials and wherein the oxide film is deposited in the gaps.

[0009] In some such examples, the gap additionally or alternatively includes an aspect ratio in a range of 40:1 to 100:1.

[0010] In some such examples, the gap additionally or alternatively includes a reentrant structure.

[0011] In some such examples, the carbon-containing inhibitor additionally or alternatively comprises one or more of an alkane, an alkene, an alkyne, a cyclic hydrocarbon, an aromatic, an alcohol, a diol, an aldehyde, an ester, an ether, a ketone, an alkyl halide, an alkylamine, or an alkyldiamine.

[0012] In some such examples, the oxide film includes a silicon oxide film.

[0013] Another example provides a processing tool. The processing tool includes a processing chamber, an RF power source, one or more gas inlets into the processing chamber, and flow control hardware configured to control the flow of gas through the one or more gas inlets. The processing tool further includes a controller operably coupled to the flow control hardware and the RF power source. The controller is configured to fill a gap in a substrate located in the processing chamber. The controller is configured to operate the flow control hardware to introduce an oxide film precursor into the processing chamber. The controller is further configured to operate the flow control hardware to introduce an oxygen-containing gas into the processing chamber. The controller is further configured to operate the RF power source to form a plasma containing the oxygen-containing gas. The controller is further configured to operate the flow control hardware to introduce a carbon-containing inhibitor into the processing chamber after operating the RF power source to extinguish the plasma.

[0014] In some such examples, the controller is further configured to operate the flow control hardware to purge the processing chamber after the controller operates the RF power source to extinguish the plasma.

[0015] In some such examples, the processing tool additionally or alternatively includes a source of a carbon-containing inhibitor.

[0016] In some such examples, the carbon-containing inhibitor source additionally or alternatively comprises one or more of an alkane, an alkene, an alkyne, a cyclic hydrocarbon, an aromatic, an alcohol, a diol, an aldehyde, an ester, an ether, a ketone, an alkyl halide, an alkylamine, or an alkyldiamine.

[0017] In some such examples, the controller is additionally or alternatively configured to operate flow control hardware with the RF power source to perform a plurality of oxide film deposition cycles, at least some of the oxide film deposition cycles omitting operating the flow control hardware to introduce the carbon-containing inhibitor.

[0018] In some such examples, the controller is additionally or alternatively configured to control the processing tool to fill a recessed gap in the substrate.

[0019] In some such examples, the processing tool additionally or alternatively includes a substrate heater operably coupled to the controller, and wherein the controller is configured to control heating of the substrate heater to a temperature within a range of 25°C to 75°C.

[0020] Another example provides a computer readable storage device, the computer readable storage device containing instructions executable by a computing device, the computing device containing a processor to control a substrate processing tool to fill a gap in a substrate. The instructions are executable to operate flow control hardware of the substrate processing tool to introduce an oxide film precursor into a processing chamber, thereby exposing the gap to the oxide film precursor. The instructions are further executable to operate the flow control hardware to introduce an oxygen-containing gas into the processing chamber. The instructions are further executable to operate a radio frequency power source to form a plasma containing an oxygen-containing gas. The instructions are further executable to operate the flow control hardware to introduce a carbon-containing inhibitor into the processing chamber after extinguishing the plasma, thereby exposing the gap to the carbon-containing inhibitor.

[0021] In some such examples, instructions executable to operate flow control hardware to introduce a carbon-containing inhibitor into a processing chamber are executable to control the introduction of one or more of an alkane, an alkene, an alkyne, a cyclic hydrocarbon, an aromatic, an alcohol, a diol, an aldehyde, an ester, an ether, a ketone, an alkyl halide, an alkylamine, or an alkyldiamine into the processing chamber.

[0022] In some such examples, the instructions may additionally or alternatively be executable to perform an oxide film deposition cycle that omits introducing a carbon-containing inhibitor into the processing chamber.

[0023] Examples involving the use of a carbon-containing inhibitor to grow an oxide film non-conformally are also disclosed. One example provides a method for forming an oxide film. The method includes performing at least one oxide film deposition cycle. The oxide film deposition cycle in the at least one oxide film deposition cycle includes exposing a substrate placed in a processing chamber to an oxide film precursor, introducing an oxygen-containing gas into the processing chamber, reacting the oxide film precursor with the oxygen-containing gas, and exposing the substrate to a carbon-containing inhibitor.

[0024] In some such examples, the method includes an atomic layer deposition process.

[0025] In some such examples, the method additionally or alternatively includes purging residual oxide film precursor from the processing chamber prior to reacting the oxide film precursor with the oxygen-containing gas.

[0026] In some such examples, reacting the oxide film precursor with the oxygen-containing gas additionally or alternatively includes forming a plasma including the oxygen-containing gas.

[0027] In some such examples, the method additionally or alternatively includes purging the processing chamber after quenching the plasma and before introducing the carbon-containing suppressant.

[0028] In some such examples, the carbon-containing inhibitor comprises an alkane.

[0029] In some such examples, the alkane includes one or more of methane, ethane, propane, butane, pentane, or hexane.

[0030] In some such examples, the carbon-containing inhibitor additionally or alternatively comprises one or more of an olefin, an alkyne, a cyclic hydrocarbon, an aromatic, an alcohol, a diol, an aldehyde, an ester, an ether, a ketone, an alkyl halide, an alkylamine, or an alkyl diamine.

[0031] In some such examples, the method additionally or alternatively includes performing a plurality of oxide film deposition cycles, wherein a subsequent oxide film deposition cycle of the plurality of oxide film deposition cycles omits introducing a carbon-containing inhibitor into the process chamber.

[0032] Another example provides a processing tool, the processing tool comprising a processing chamber, a substrate support positioned in the processing chamber, a radio frequency power source, one or more gas inlets leading to the processing chamber, and flow control hardware configured to control the flow of gas through the one or more gas inlets. The processing tool further comprises a controller operably coupled to the flow control hardware and the radio frequency power source. The controller is configured to operate the flow control hardware to introduce an oxide film precursor into the processing chamber. The controller is further configured to operate the flow control hardware to introduce an oxygen-containing gas into the processing chamber. The controller is further configured to operate the radio frequency power source to form a plasma containing the oxygen-containing gas. The controller is further configured to operate the flow control hardware to introduce a carbon-containing inhibitor into the processing chamber after operating the radio frequency power source to extinguish the plasma.

[0033] In some such examples, the controller is further configured to operate the flow control hardware to purge the processing chamber after the controller operates the RF power source to extinguish the plasma.

[0034] In some such examples, the processing tool additionally or alternatively includes a source of a carbon-containing inhibitor.

[0035] In some such examples, the carbonaceous inhibitor source additionally or alternatively comprises one or more of methane, ethane, propane, butane, pentane, or hexane.

[0036] In some such examples, the carbon-containing inhibitor source additionally or alternatively comprises one or more of an olefin, an alkyne, a cyclic hydrocarbon, an aromatic, an alcohol, a diol, an aldehyde, an ester, an ether, a ketone, an alkyl halide, an alkylamine, or an alkyl diamine.

[0037] In some such examples, the controller is additionally or alternatively configured to operate the flow control hardware and the RF power source to perform a plurality of oxide film deposition cycles, at least some of the oxide film deposition cycles omitting introduction of the carbon-containing inhibitor.

[0038] In some such examples, the processing tool additionally or alternatively includes a substrate heater operably coupled to the controller, and the controller is configured to control heating of the substrate heater to a temperature within a range of 25°C to 75°C.

[0039] Another example provides a computer readable storage device containing instructions executable by a computing device including a processor. The instructions are executable to control a processing tool to operate flow control hardware of a substrate processing tool to introduce an oxide film precursor into a processing chamber. The instructions are further executable to operate the flow control hardware to introduce an oxygen-containing gas into the processing chamber. The instructions are further executable to operate a radio frequency power source to form a plasma containing an oxygen-containing gas. The instructions are further executable to operate the flow control hardware to introduce a carbon-containing inhibitor into the processing chamber after operating the radio frequency power source to extinguish the plasma.

[0040] In some such examples, instructions executable to operate flow control hardware to introduce a carbon-containing inhibitor into a processing chamber are executable to control the introduction of one or more of an alkane, an alkene, an alkyne, a cyclic hydrocarbon, an aromatic, an alcohol, a diol, an aldehyde, an ester, an ether, a ketone, an alkyl halide, an alkylamine, or an alkyldiamine into the processing chamber.

[0041] In some such examples, the instructions may additionally or alternatively be executable to perform an oxide film deposition cycle that omits introducing a carbon-containing inhibitor into the processing chamber.

[0042] In some such examples, the instructions may additionally or alternatively be executable to control the flow control hardware to purge the processing chamber after operating the RF power source to extinguish the plasma. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 A block diagram of an exemplary processing tool is shown.

[0044] Figure 2 A flow chart depicting an exemplary method for performing a deposition process is shown.

[0045] Figure 3 A flow chart depicting an exemplary method for performing a deposition process cycle that omits the introduction of a carbon-containing inhibitor is shown.

[0046] Figure 4 A flow chart depicting an exemplary method for performing a deposition process cycle including the introduction of a carbon-containing inhibitor is shown.

[0047] Figures 5A to 5B An exemplary substrate structure including a gap is schematically shown.

[0048] Figures 6A to 6B An exemplary gap fill process using exposures of different carbon-containing inhibitors is schematically shown.

[0049] Figure 7 An exemplary gap fill process for filling a high aspect ratio gap is schematically shown.

[0050] Figure 8 A flow chart depicting an exemplary method for filling a gap in a substrate is shown.

[0051] Fig. 9 An example of non-conformal growth of an oxide film as a function of varying times of exposure to a carbon-containing inhibitor during a deposition cycle is schematically shown.

[0052] Fig.10 An example of non-conformal growth of an oxide film as a function of varying proportions of carbon deposition cycles to carbon-free deposition cycles is schematically shown.

[0053] Figures 11A to 11B The fabrication of an exemplary spacer on a substrate is schematically shown.

[0054] Fig.12 A flow chart depicting an exemplary method for performing non-conformal oxide film deposition using a carbon-containing inhibitor is shown.

[0055] Fig.13 An exemplary computing device is shown schematically. DETAILED DESCRIPTION

[0056] The term "alcohol" refers to a hydrocarbon containing the general formula R-OH, where R is an aromatic or aliphatic group. Alcohols may have more than one OH group (polyols), such as diols having two OH functional groups. Exemplary alcohols include methanol, ethanol and propanol.

[0057] The term "aldehyde" refers to a hydrocarbon containing a terminal carbonyl group. Aldehydes have the general formula R-CHO, where R is an aromatic or aliphatic group. Exemplary aldehydes include formaldehyde and acetaldehyde.

[0058] The term "aliphatic" refers to organic compounds that lack aromatic groups.

[0059] The term "alkane" refers to an alkane containing the general formula C n H 2n+2 and substituted linear alkanes. Exemplary alkanes include methane, ethane, propane, and butane. Exemplary alkanes that may be suitable for use as carbon-containing inhibitors may include the general formula C wherein n is equal to 1 to 10. n H 2n+2 .

[0060] The term "olefin" refers to a hydrocarbon containing at least one carbon-carbon double bond. n H 2n Exemplary olefins include ethylene, propylene, and butene. Olefins may have more than one carbon-carbon double bond, such as dienes, allenes, and cumulenes. Exemplary olefins that may be suitable for use as carbon-containing inhibitors may include the general formula C wherein n is equal to 2 to 10. n H 2n .

[0061] The term "alkylamine" refers to a hydrocarbon containing nitrogen with 1 to 3 alkyl substituents and 0 to 2 H substituents. Alkylamines include primary amines, secondary amines, tertiary amines, and cyclic amines. Examples of alkylamines include methylamine, dimethylamine, trimethylamine, and piperidine.

[0062] The term "alkyl halide" refers to a hydrocarbon containing a halogen. Examples of alkyl halides include ethyl fluoride (fluoroethane), isopropyl bromide (2-bromopropane), and tert-butyl chloride (2-chloro-2-methylpropane). Alkyl halides may have two or more halogen groups, such as 1,2-dichlorobutane.

[0063] The term "alkyne" refers to a hydrocarbon containing at least one carbon-carbon triple bond. Alkynes containing one carbon-carbon triple bond have C n H 2n-2 The alkyne may have more than one carbon-carbon triple bond, such as a diyne having two carbon-carbon triple bonds. Exemplary alkynes that may be suitable for use as carbon-containing inhibitors may include the general formula C wherein n is equal to 2 to 10 n H 2n-2 .

[0064] The term "aromatic" refers to a planar cyclic compound containing a pi bond in resonance. The term "aromatic" includes homocyclic compounds in which all atoms in the ring structure are carbon, and also includes heterocyclic compounds in which one or more atoms in the ring structure are elements other than carbon (e.g., nitrogen).

[0065] The term "aspect ratio" refers to the ratio between the depth of a feature, such as a substrate gap, and the average width of the feature.

[0066] The term "atomic layer deposition (ALD)" refers to a process in which a film is formed on a substrate in one or more separate layers by sequentially conformally adsorbing precursors to the substrate and reacting the adsorbed precursors to form the film layers. Examples of ALD processes include plasma enhanced ALD (PEALD) and thermal ALD (TALD). PEALD and TALD utilize plasma of a reactive gas and heat, respectively, to promote the chemical conversion of a precursor adsorbed to a substrate into a film on the substrate. The terms "growth" and "deposition", and variations thereof, may also be used to refer to film formation.

[0067] The term "carbon-containing inhibitor" refers to a carbon-containing compound that can be introduced into a processing chamber in a vapor phase, non-conformally deposited on a substrate surface, and oxidized by an oxygen-containing gas to form a gas-phase product. The carbon-containing inhibitor can inhibit the growth of the oxide film by consuming oxygen, thereby leaving less oxygen to react with the oxide film precursor. Exemplary carbon-containing inhibitors can include various alkanes, alkenes, alkynes, cyclic hydrocarbons, aromatics, alcohols, aldehydes, esters, ethers, ketones, aldehydes, alkyl halides, alkylamines, and alkyl diamines.

[0068] The term "cyclic hydrocarbon" refers to a saturated or unsaturated hydrocarbon molecule containing a closed ring structure. Exemplary cyclic hydrocarbons include cyclopropane and cyclobutene.

[0069] The term "ether" refers to a hydrocarbon comprising the general formula RO-R', wherein R and R' are independently aryl or aliphatic. Exemplary ethers include diethyl ether, methyl phenyl ether, and cyclic ethers such as furan.

[0070] The term "ester" refers to a hydrocarbon comprising the general formula RC(O)OR', wherein R and R' are independently aryl or aliphatic and wherein R may alternatively comprise H (eg, formate). Exemplary esters include ethyl formate, methyl acetate, and ethyl acetate.

[0071] The term "gap" refers to a recessed feature in the surface of a substrate.

[0072] The term "gap fill" refers to the process of filling a gap on a substrate with a material.

[0073] The term "intermediate structure" refers to structure formed by earlier processing steps and modified in later processing steps.

[0074] The term "ketone" refers to a hydrocarbon containing a non-terminal carbonyl group. Ketones have the general formula RC(O)-R', wherein R and R' are independently aromatic or aliphatic. Exemplary ketones include acetone and methyl ethyl ketone.

[0075] The term "mandrel" refers to an intermediate structure that defines the position of the spacer during the patterning process, and the mandrel is removed from the substrate to produce the spacer. The mandrel may comprise any suitable material, such as polysilicon, amorphous silicon, silicon oxide, silicon nitride, or amorphous carbon.

[0076] The term "oxide film" refers to a film deposited on the surface of a substrate and contains oxygen and oxidizing substances. Examples of oxide films include doped or undoped silicon oxide films (e.g., silicon dioxide (SiO2), silicon oxynitride (SiO x N y , 0≤x≤2, 0≤y≤1.33), silicon oxycarbide (SiC x O 2-y , 0≤x≤1, y=2x)) and metal oxides (e.g., hafnium oxide (HfO x ), titanium oxide (TiO x ), tungsten oxide (WO x ), tin oxide (SnO x ) and molybdenum oxide (MoO x )) membrane.

[0077] The term "oxide film deposition cycle" refers to a sequence of processes used to form an oxide film layer. As described below, certain oxide film deposition cycles may include deposition of a carbon-containing inhibitor, and / or may include oxidation of a carbon-containing inhibitor deposited in a previous cycle, to cause non-conformal growth.

[0078] The term "oxygen-containing gas" refers to a gaseous substance containing oxygen that can react with an oxide film precursor to form an oxide film. Examples of the oxygen-containing gas include molecular oxygen (O2), water vapor (H2O), and ozone (O3).

[0079] The term "oxide film precursor" refers to any material that can be introduced into a process chamber to form an oxide film on a substrate placed in the process chamber. Examples of oxide film precursors include silicon-containing precursors that can be used to form silicon-containing films such as silicon dioxide films, silicon oxynitride films, and silicon oxycarbide films. Other examples of oxide film precursors include metal-containing precursors that are used to form metal oxide films. Examples of such metal-containing precursors include hafnium-containing precursors, titanium-containing precursors, tungsten-containing precursors, tin-containing precursors, and molybdenum-containing precursors, which can be used to form hafnium oxide (HfO x ) film, titanium oxide (TiO x ) film, tungsten oxide (WO x ) film, tin oxide (SnO x ) film and molybdenum oxide (MoO x )membrane.

[0080] The term "silicon-containing precursor" refers to any material that can be introduced into a processing chamber in the vapor phase to form a silicon-containing oxide film on a substrate. An exemplary oxide film precursor for forming a silicon-containing film using PEALD may include a material having the following general structure: Wherein R1, R2 and R3 may be the same or different substituents and may include silane, siloxy, amine, halide, hydrogen, or an organic group, such as an alkylamine, alkoxy, alkyl, alkenyl, alkynyl and aromatic group.

[0081] Exemplary silicon-containing precursors include polysilane (H3Si-(SiH2) n -SiH3), where n≥1, such as silane, disilane, trisilane, tetrasilane and trisilylamine.

[0082] In some examples, the silicon-containing precursor is an alkoxysilane. Useful alkoxysilanes include the following: x -Si-(OR) y , wherein x=1 to 3, x+y=4, and each R is a substituted or unsubstituted alkyl, alkenyl, alkynyl or aromatic group; and H x (RO) y ,-Si-Si-(OR) y H x , is a substituted or unsubstituted alkyl, alkenyl, alkynyl or aromatic group.

[0083] Examples of silicon-containing precursors include tetraethylorthosilicate (TEOS), tetramethoxysilane (TMOS), monosilane, trimethylsilane (3MS), disilane, butasilane, pentasilane, octasilane, heptsilane, hexasilane, cyclotetrasilane, cycloheptasilane, cyclohexasilane, cyclooctylsilane, cyclopentasilane, 1,4-dioxane-2,3,5,6-tetrasilcyclohexane, diethoxymethylsilane (DEMS), diethoxysilane (DES), dimethoxymethylsilane, dimethoxysilane (DMOS), methyldiethoxysilane (MDES), methyldimethoxysilane (MDMS), tert-butoxydisilane, triethoxysilane (TES), and trimethoxysilane (TMS or TriMOS).

[0084] In some examples, the silicon-containing precursor may be a siloxane. Exemplary siloxanes include octamethylcyclotetrasiloxane (OMCTS), octamethoxydodecylsiloxane (OMODDS), tetramethylcyclotetrasiloxane (TMCTS), triethoxysiloxane (TRIES), and tetraoxymethylcyclotetrasiloxane (TOMCTS).

[0085] As mentioned above, in some examples, the silicon-containing precursor may be an aminosilane, such as bisdiethylaminosilane, diisopropylaminosilane, bis(tert-butylamino)silane (BTBAS), di-sec-butylaminosilane, or tris(dimethylamino)silane (3DMAS). The aminosilane precursor may have the general formula: x -Si-(NR) y , wherein x=1 to 3, x+y=4, and each R is a substituted or unsubstituted alkyl, alkenyl, alkynyl or aromatic group or a hydride group.

[0086] In some examples, a halogen-containing silane may be used such that the silane includes at least one hydrogen atom. Such a silane may have a chemical formula of SiX a H y , wherein X is a halogen and y ≥ 1. In some examples, dichlorosilane (H2SiCl2) can be used.

[0087] An exemplary precursor for providing nitrogen for the formation of silicon oxynitride films is N2O.

[0088] For forming hafnium oxide film (HfO x ) include hafnium tetrachloride (HfCl4), tetrakis(diethylamino)hafnium (Hf(N(C2H5)2)4), and tetrakis(tert-butyloxide)hafnium (Hf(OC(CH3)3)4).

[0089] For forming titanium oxide film (TiO x Examples of titanium-containing precursors of ) include titanium tetrachloride (TCl4) and titanium isopropoxide (Ti(OCH(CH3)2)4).

[0090] For forming tungsten oxide film (WO x Examples of tungsten-containing precursors include tungsten hexafluoride (WF6), tungsten hexachloride (WCl6), and tungsten hexacarbonyl (W(CO)6).

[0091] For forming tin oxide film (SnO x ) include tin tetrachloride (SnCl4), tetramethyltin ((CH3)4Sn), tetraethyltin ((C2H5)4Sn), dimethyltin dichloride ((CH3)2SnCl2), dibutyl(dimethoxy)stannane (Bu2Sn(OMe)2), tetrakis(dimethylamino)tin(IV) (Sn(NMe2)4), dimethylaminodimethyltin (Me2Sn(NMe2)2), and dimethylaminotrimethyltin (Me3Sn(NMe2)).

[0092] For forming molybdenum oxide film (MoO x) include molybdenum pentachloride (MoCl5), molybdenum dioxide dichloride (MoO2Cl2), molybdenum tetrachloride (MoOCl4) and molybdenum hexacarbonyl (Mo(CO)6).

[0093] The term "processing chamber" refers to a housing in which a chemical and / or physical process is performed on a substrate. The pressure, temperature, and atmosphere composition within the processing chamber may be controllable to perform the chemical and / or physical process.

[0094] The term "processing tool" refers to a structure that includes a processing chamber and other hardware configured to enable processing to be performed in the processing chamber.

[0095] The term "sweep" and variations thereof refer to a process in which unwanted material is removed from a process chamber.

[0096] The term "sticking coefficient" refers to the ratio of the amount of gas-phase species impinging on the substrate surface compared to the amount of gas-phase species adsorbed to the substrate surface.

[0097] The term "substrate" refers to anything on which a film can be deposited. A substrate can refer to a single piece of material or a structure comprising two or more materials, such as a multilayer stack.

[0098] The term "substrate support" refers to any structure used to support a substrate in a processing chamber. Examples include chucks, pedestals, and showerhead pedestals for backside deposition processing.

[0099] The term “3D NAND” is an abbreviation for three-dimensional NOT AND, and refers to a memory architecture based on NOT AND logic gates.

[0100] The term "3D DRAM" is an abbreviation for Three-Dimensional Dynamic Random Access Memory.

[0101] As mentioned above, atomic layer deposition (ALD) involves performing one or more deposition cycles to grow a thin film, such as an oxide film, on a substrate surface. ALD is often used in the manufacture of devices on semiconductor substrates. In contrast, chemical vapor deposition (CVD) processes, which are also commonly used in the manufacture of devices, form films in a continuous growth process rather than in a layer-by-layer growth process.

[0102] Plasma enhanced ALD (PEALD) utilizes plasma to promote the deposition of films. For example, PEALD can be used to grow oxide films. During the PEALD oxide film cycle, an oxide film precursor gas is introduced into the processing chamber and adsorbed onto the substrate. Next, the processing chamber is purged to remove excess oxide film precursor. Then, an oxygen-containing reactant gas is introduced into the processing chamber. The reactant gas may include an oxygen-containing gas (e.g., oxygen, ozone, or steam). A plasma is then formed in the processing chamber, for example, by applying radio frequency power to an electrode. The plasma forms reactive oxygen species that react with the oxide film precursor to form a layer of oxide film. Examples of oxide films that can be formed by PEALD include silicon oxynitride (SiO x N y ), silicon dioxide (SiO2), silicon oxycarbide SiC x O 2-y 、HfO x ), titanium oxide (TiO x ), tungsten oxide (WO x ), tin oxide (SnO x ) and molybdenum oxide (MoO x In some examples, the growth rate of the oxide film can be on the order of 0.10 nm to 0.16 nm per cycle. Thus, the PEALD process can involve tens to hundreds of deposition cycles depending on the desired film thickness.

[0103] PEALD can be used to conformally grow oxide films. However, as described in more detail below, conformal growth may not be desired in certain applications. Accordingly, examples are disclosed regarding the use of carbon-containing inhibitors in deposition processes to provide controlled non-conformal growth of oxide films. Although PEALD processes are described in the context, the disclosed examples may also be used in other ALD processes (e.g., TALD). In addition, carbon-containing inhibitors as disclosed herein may also be used in suitable CVD processes to selectively inhibit CVD film growth.

[0104] In a PEALD process, one or more deposition cycles may be performed to form an oxide film on a substrate. In each deposition cycle, an oxide film precursor gas is introduced into a processing chamber to be conformally adsorbed to the substrate surface. The processing chamber is purged, and an oxygen-containing gas is introduced into the processing chamber. An RF power source is used to form an RF plasma containing the oxygen-containing gas. Reactive oxygen-containing species formed in the plasma may react with the adsorbed oxide film precursor to form an oxide film.

[0105] A TALD process may similarly include one or more deposition cycles. In TALD, a chemical reaction is effected by a relatively high temperature of a substrate heater within a process chamber. In each deposition cycle, an oxide film precursor is conformally adsorbed to the substrate surface. The process chamber is purged, and an oxygen-containing gas is introduced into the process chamber. The oxygen-containing gas reacts with the oxide film precursor due to the elevated temperature of the substrate. In contrast, thermal CVD may be used to form a film via a continuous growth process. In such a process, rather than pulsing gases into the process chamber, gases may be continuously introduced and reacted to form an oxide film on the substrate surface.

[0106] An example of a process in which non-conformal ALD film deposition may be desired is an oxide gap filling process. In such a process, an oxide material is used to fill a gap on a substrate. In ALD oxide gap filling, an oxide film precursor gas diffuses into the gap and adsorbs onto a surface within the gap. The adsorbed gas is reacted with an oxygen-containing gas to form a film on a surface within the gap. The process may be repeated to gradually fill the gap. However, some gaps may have concave features that block features of direct line of sight from a position below the concave feature in a direction orthogonal to the substrate surface plane to the gap surface. Conformal film growth in a gap with a concave feature may cause the gap to close at the concave feature before a deeper region of the gap is filled. This may leave unfilled pores in the gap and may affect the performance of the gap. In addition, gaps with a high aspect ratio, such as channel holes formed in a 3D NAND memory manufacturing process, may also experience a faster ALD film growth rate near the opening of the gap rather than deeper within the gap, and thus may also appear when a position within the gap closer to the gap opening is closed before a position farther away from the gap opening is completely filled.

[0107] Thus, as described in more detail below, during the oxide gap fill process, in at least some deposition cycles, a carbon-containing inhibitor is introduced into the processing chamber. The carbon-containing inhibitor may be introduced together with the oxide film precursor or may be introduced separately. The carbon-containing inhibitor is non-conformally adsorbed on the surface of the substrate so that a larger amount of the carbon-containing inhibitor is deposited in the gap at a position closer to the opening of the gap than at a position farther away from the gap opening. Without wishing to be bound by theory, the use of the carbon-containing inhibitor in the oxide film deposition cycle may preferentially inhibit the growth of the oxide film by reacting with the oxygen-containing gas used in the oxide deposition process to form a gas phase product. When the oxygen-containing gas is at least partially consumed by the carbon-containing inhibitor, less oxygen-containing gas is available to react with the adsorbed oxide film precursor. Thus, the oxide film growth may be inhibited to different degrees at different locations on the surface based on the amount of the carbon-containing inhibitor adsorbed to different locations. In some examples, the non-conformal adsorption of the carbon-containing inhibitor may depend on the processing conditions, such as pressure, partial pressure of the carbon-containing inhibitor, partial pressure of other gases, and / or plasma conditions. For example, the use of capacitively coupled plasma or inductively coupled plasma can result in directionality of ion bombardment on the substrate surface. Thus, such conditions can be controlled to assist in achieving non-conformal adsorption. In various examples, the carbon-containing inhibitor can be chemisorbed and / or physically adsorbed to the substrate surface. In addition, the carbon-containing inhibitor on the substrate surface can be converted to other substances, such as elemental carbon, by the processing environment.

[0108] In the case where a larger amount of carbon-containing inhibitor is adsorbed to the inner surface of the gap closer to the gap opening than to the surface deeper within the gap, film growth on the surface closer to the gap opening can be more strongly inhibited by the carbon-containing inhibitor than on the surface deeper within the gap. This can allow the oxide to fill the lower portion of the gap without pinching off at a location closer to the gap opening, thereby avoiding the formation of voids. An exemplary gap filling process is disclosed in more detail below.

[0109] In addition to gap filling applications, oxide films can also be used in patterning applications to form spacers. An exemplary process is self-aligned double patterning (SADP). In such a process, a mandrel is formed on the surface of a substrate, for example, by photolithographic patterning of a carbon film (e.g., spin-on carbon). Next, an oxide film is grown over the mandrel. A "core pull" is then performed via dry etching to remove the layer of oxide on the top surface of the mandrel, followed by ashing to remove the mandrel. In this step, the oxide on the substrate surface between the mandrels is also removed by dry etching. Portions of the oxide film on the sidewalls of the mandrel remain. Once the mandrels are removed, these portions form spacers. However, the top surface of the spacer may become tapered during dry etching and may affect transfer etching performance. Thus, a carbon-containing inhibitor may be used to grow a non-conformal film as disclosed herein. Such a film will be thinner on the top of the mandrel and between the mandrels than on the sides of the mandrel. This may allow a shorter dry etching process to be used. A shorter dry etch process may help prevent or mitigate spacer tapering by reducing sputtering effects at the top corners of the spacers.

[0110] Figure 1 A schematic diagram of an exemplary processing tool 100 for performing atomic layer deposition using a carbon-containing inhibitor is shown. The processing tool 100 is configured as a PEALD tool. However, as mentioned above, the use of carbon-containing inhibitors as disclosed herein may also be used to vary the conformality of films deposited in other types of tools. Examples may include TALD and / or other ALD tools. Examples may also include various CVD tools.

[0111] The processing tool 100 includes a processing chamber 102 and a substrate support 104 within the processing chamber. The substrate support 104 is configured to support a substrate 106 placed within the processing chamber 102. The substrate support 104 may include a pedestal, a chuck, or any other suitable structure. The processing chamber 102 may further include a substrate heater 108. In other examples, the heater may be omitted or may be located elsewhere within the processing chamber 102.

[0112] The processing tool 100 further includes a showerhead 110, a gas inlet 112, and flow control hardware 114. In other examples, the processing tool may include a nozzle or other device for introducing gas into the processing chamber 102 in addition to or in addition to the showerhead. The flow control hardware 114 is connected to an oxide film precursor gas source 116, an oxygen-containing gas source 118, a carbon-containing inhibitor source 120, and a sweep gas source 122. The oxide film precursor gas source 116 may include any suitable oxide film precursor that forms an oxide film when reacted with the oxygen-containing gas. Exemplary silicon-containing oxide films include silicon dioxide, silicon oxynitride, and silicon oxycarbide. Exemplary metal oxide films include hafnium oxide, titanium oxide, tungsten oxide, tin oxide, and molybdenum oxide. Exemplary oxide film precursors for silicon-containing oxide films may include polysilanes, aminosilanes, halogenated silanes, and organosilanes. HfCl4, Hf(N(C2H5)2)4, Hf(OC(CH3)3)4, TCl4, Ti(OCH(CH3)2)4, WF6, WCl6, W(CO)6, SnCl4, (CH3)4S n, (C2H5)4Sn, (CH3)2SnCl2, Bu2Sn(OMe)2, Sn(NMe2)4, Me2Sn(NMe2)2, Me3Sn(NMe2), MoCl5, MoO2Cl 2、 MoOCl4, and Mo(CO)6. The oxygen-containing gas source 118 may include, for example, O2, O3, water vapor, nitrogen oxides (eg, N2O), H2O2, or a mixture of two or more thereof.

[0113] The carbon-containing inhibitor source 120 comprises any suitable carbon-containing inhibitor that can be oxidized by an oxygen-containing gas to form a gas-phase product and non-conformally adsorbed to the substrate surface. Exemplary carbon-containing inhibitors suitable for non-conformal film deposition can include various alkanes, alkenes, alkynes, cyclic hydrocarbons, aromatics, alcohols, aldehydes, esters, ethers, ketones, aldehydes, alkyl halides, alkylamines, and alkyl diamines. Exemplary carbon-containing inhibitors are described in more detail below.

[0114] The purge gas source 122 may include any suitable inert gas, such as argon or nitrogen. In some examples, one or more additional purge gas sources may be included, each providing a different purge gas.

[0115] The flow control hardware 114 may be controlled to flow gases from gas sources 116, 118, 120, 122 into the processing chamber 102 via the gas inlet 112. The flow control hardware 114 may include one or more valves that may be controlled to place a selected gas source in fluid connection with the gas inlet 112. For example, in a first configuration, the flow control hardware 114 may place an oxide film precursor gas source 116 in fluid connection with the gas inlet 112 to allow the oxide film precursor to flow into the processing chamber 102. In a second configuration, the flow control hardware 114 may place an oxygen-containing gas source 118 in fluid connection with the gas inlet 112 to allow the oxygen-containing gas to flow into the processing chamber 102. In a third configuration, the flow control hardware 114 may place a carbon-containing inhibitor source 120 in fluid connection with the gas inlet 112 to allow the carbon-containing inhibitor to flow into the processing chamber 102. In a fourth configuration, the flow control hardware 114 may place a purge gas source 122 in fluid connection with the gas inlet 112 to allow the purge gas to flow into the processing chamber 102. In further configurations, the flow control hardware 114 may place two or more such gas sources in fluid connection with the gas inlet 112 .

[0116] The processing tool 100 further includes an exhaust system 124. The exhaust system 124 is configured to receive gases flowing out of the processing chamber 102. In some examples, the exhaust system 124 is configured to actively remove gases and / or apply a partial vacuum from the processing chamber 102. The exhaust system 124 can include any suitable hardware, including a pump.

[0117] The processing tool 100 further includes an RF power source 128 electrically connected to the substrate support 104. The RF power source 128 is configured to form a plasma containing an oxygen-containing gas. In this example, the showerhead 110 is configured as an electrode opposite to ground. In other examples, the RF power source 128 can supply RF power to the showerhead 110, or to other suitable electrode structures. The processing tool 100 may include a matching network 129 for impedance matching of the RF power source 128. The RF power source 128 can be configured for any suitable frequency and power. Examples of suitable frequencies include 400kHz and 13.56MHz. Examples of suitable powers include powers between 0 watts and 7000 watts. In some examples, the RF power source 128 is configured to operate at a plurality of different frequencies and / or powers.

[0118] The controller 130 is operably coupled to the substrate heater 108, the flow control hardware 114, the exhaust system 124, and the RF power source 128. The controller 130 is configured to control various functions of the processing tool 100 to perform a thin film deposition process such as an ALD process. For example, the controller 130 is configured to operate the substrate heater 108 to heat the substrate to a desired temperature. The controller 130 is also configured to operate the flow control hardware 114 to cause a selected gas or mixture of gases to flow into the processing chamber 102 at a selected rate. The controller 130 is further configured to operate the exhaust system 124 to remove gas from the processing chamber 102. In addition, the controller 130 is configured to operate the RF power source 128 to form a plasma containing an oxygen-containing gas, as well as to control any other suitable function of the processing tool 100. The controller 130 may include any suitable computing system, and reference is made below to Fig.13 Describe an example of a computing system.

[0119] Figure 2 A flow chart is shown of an exemplary method 200 for performing a deposition process, such as a PEALD process using a carbon-containing inhibitor to produce a non-conformal oxide film. For example, the method 200 may be performed using the processing tool 100. The method 200 includes, at 202, placing a substrate including one or more gaps in a processing chamber. Any suitable substrate may be used. Examples include semiconductor wafers. The gaps on the substrate may include any suitable intermediate structure in an integrated circuit manufacturing process. For example, the gaps may include channel gaps for a 3D NAND manufacturing process. In some examples, the method 200 may include heating the substrate via a substrate heater. In other examples, the substrate may include a mandrel for forming an oxide spacer, and / or any other suitable structure, instead of or in addition to the gaps.

[0120] The non-conformal oxide film growth may include multiple deposition cycles, at least some of which include a carbon-containing inhibitor. Thus, method 200 further includes, at 204, determining whether to perform a deposition cycle that includes a carbon-containing inhibitor, or to omit a deposition cycle that includes a carbon-containing inhibitor. This determination may be based on a recipe for the particular process being performed. The term "first deposition cycle" is used herein to refer to a deposition cycle that omits the introduction of a carbon-containing precursor. Figure 3 An exemplary first deposition cycle is described in more detail. The term "second deposition cycle" is used herein to refer to a deposition cycle that includes the introduction of a carbon-containing precursor. Figure 4An exemplary second deposition cycle is described in more detail. As described in more detail below, the ratio of the first deposition cycle to the second deposition cycle can be varied to control the magnitude of film non-conformality. In addition, the duration of exposure to the carbon-containing inhibitor in the deposition cycle can also be varied to control the magnitude of non-conformality. In certain gap filling examples, the magnitude of non-conformality of the deposited film can be controlled based on the characteristics of the gap. Exemplary gap characteristics include the aspect ratio of the gap, and whether the gap has a concave feature.

[0121] Figure 3 A flow chart depicting an exemplary first deposition cycle 300 for forming an oxide film is shown. The first deposition cycle 300 omits the introduction of a carbon-containing inhibitor. As shown at 301, the first deposition cycle 300 may be preceded by a previous cycle. The previous cycle may be a previous first deposition cycle 300 or a previous second deposition cycle 400 as part of a non-conformal oxide film growth process.

[0122] The first deposition cycle 300 includes, at 302, introducing an oxide film precursor into a process chamber. The oxide film precursor may be optionally deposited conformally on the substrate. For example, the oxide film precursor may form a monolayer of adsorbed oxide film precursor on the surface of the substrate including the inner surface of the gap. In the case of depositing a silicon-containing oxide film, exemplary oxide film precursors include polysilanes, siloxanes, aminosilanes, halosilanes, and organosilanes. As mentioned above, examples of silicon-containing precursors include materials having the following general structure: Wherein R1, R2 and R3 can be the same or different substituents and can include silane, siloxy, amine, halide, hydrogen, or organic groups, such as alkylamine, alkoxy, alkyl, alkenyl, alkynyl and aromatic groups.

[0123] Exemplary silicon-containing precursors include polysilanes (H3Si-(SiH2)n-SiH3), where n≥1, such as silane, disilane, trisilane, tetrasilane, and trisilylamine.

[0124] In some examples, the silicon-containing precursor is an alkoxysilane. Useful alkoxysilanes include the following: x -Si-(OR) y , wherein x=1 to 3, x+y=4, and each R is a substituted or unsubstituted alkyl, alkenyl, alkynyl or aromatic group; and H x (RO) y ,-Si-Si-(OR) y H x , is a substituted or unsubstituted alkyl, alkenyl, alkynyl or aromatic group.

[0125] Examples of silicon-containing precursors include tetraethylorthosilicate (TEOS), tetramethoxysilane (TMOS), monosilane, trimethylsilane (3MS), disilane, butasilane, pentasilane, octasilane, heptsilane, hexasilane, cyclotetrasilane, cycloheptasilane, cyclohexasilane, cyclooctylsilane, cyclopentasilane, 1,4-dioxane-2,3,5,6-tetrasilcyclohexane, diethoxymethylsilane (DEMS), diethoxysilane (DES), dimethoxymethylsilane, dimethoxysilane (DMOS), methyldiethoxysilane (MDES), methyldimethoxysilane (MDMS), tert-butoxydisilane, triethoxysilane (TES), and trimethoxysilane (TMS or TriMOS).

[0126] In some examples, the silicon-containing precursor may be a siloxane. Exemplary siloxanes include octamethylcyclotetrasiloxane (OMCTS), octamethoxydodecylsiloxane (OMODDS), tetramethylcyclotetrasiloxane (TMCTS), triethoxysiloxane (TRIES), and tetraoxymethylcyclotetrasiloxane (TOMCTS).

[0127] As mentioned above, in some examples, the silicon-containing precursor may be an aminosilane having hydrogen atoms, such as bisdiethylaminosilane, diisopropylaminosilane, bis(tert-butylamino)silane (BTBAS), or tris(dimethylamino)silane (3DMAS), di-sec-butylaminosilane. Aminosilane precursors include the following: x -Si-(NR) y , wherein x=1 to 3, x+y=4, and R is a substituted or unsubstituted alkyl, alkenyl, alkynyl or aromatic group or a hydride group.

[0128] In some examples, a halogen-containing silane may be used such that the silane includes at least one hydrogen atom. Such a silane may have a chemical formula of SiX a H y , wherein X is a halogen and y ≥ 1. For example, dichlorosilane (H2SiCl2) may be used in some examples.

[0129] In the case of depositing a metal oxide film, exemplary oxide film precursors include HfCl4, Hf(N(C2H5)2)4, Hf(OC(CH3)3)4, TCl4, Ti(OCH(CH3)2)4, WF6, WCl6, W(CO)6, SnCl4, (CH3)4Sn, (C2H5)4Sn, (CH3)2SnCl2, Bu2Sn(OMe)2, Sn(NMe2)4, Me2Sn(NMe2)2, Me3Sn(NMe2), MoCl5, MoO2Cl 2、 MoOCl4, and Mo(CO)6.

[0130] Next, at 304, the first deposition cycle 300 includes purging the process chamber to remove at least some residual oxide film precursor. As mentioned above, an inert gas such as argon may be used to purge the chamber. At 306, the first deposition cycle 300 further includes introducing an oxygen-containing gas (e.g., oxygen, ozone, water vapor) into the process chamber.

[0131] At 308, the first deposition cycle 300 includes reacting the oxide film precursor with an oxygen-containing gas. In addition, at 308, any carbon-containing inhibitor deposited in the previous cycle 301 may also react with the oxygen-containing gas. Here, the carbon-containing inhibitor may compete with the oxide film precursor for oxygen, thereby inhibiting the growth of the oxide film. On surfaces with relatively more absorption of the carbon-containing inhibitor, the inhibition may be more pronounced.

[0132] A radio frequency power source may be used to form a plasma containing an oxygen-containing gas to perform the reaction. For example, the radio frequency power source may be operated at any suitable frequency (e.g., 400 kHz, 13.56 MHz) and power (e.g., between 0 watts and 7000 watts). The oxygen-containing gas may be converted to an oxygen-containing reactive species via a plasma. The oxygen-containing reactive species may then react with a monolayer of the adsorbed oxide film precursor to form a layer of an oxide film on the substrate. Exemplary oxide films include silicon dioxide, silicon oxynitride, silicon oxycarbide, hafnium oxide, titanium oxide, tungsten oxide, tin oxide, and molybdenum oxide. In other examples, thermal energy, and / or any other suitable energy source may be used to perform the reaction. In some examples, an optional sweep is performed after 308. When a radio frequency power source is used to form a plasma, an optional sweep may be performed after the plasma is extinguished. In some examples, the substrate is heated via a substrate heater during processing. In some examples, the substrate heater may be heated to a temperature in the range of 25° C. to 700° C. In a more specific example, the substrate heater may be heated to a temperature in the range of 25° C. to 75° C. In other examples, temperatures outside of these ranges may be used.

[0133] In other examples, the first deposition cycle 300 may be performed using TALD. In such examples, the reaction at 308 may be performed using thermal energy. Furthermore, in other examples, the first deposition cycle 300 may be performed via CVD by introducing an oxide film precursor with an oxygen-containing gas.

[0134] The first deposition cycle 300 may be performed zero or more times during processing of the substrate. The first deposition cycle may precede a subsequent cycle 314, which may be the first deposition cycle 300 or the second deposition cycle 400 as part of a non-conformal oxide film growth process. This is accomplished by Figure 2The "yes" branch at 212 indicates that the first deposition cycles may be interspersed with second deposition cycles, such as the exemplary second deposition cycle 400, in any suitable order and at any suitable frequency.

[0135] As described above, the non-conformal oxide film deposition process includes one or more deposition cycles in which a carbon-containing inhibitor is introduced. Figure 4 A flow chart depicting an exemplary second deposition cycle 400 is shown. The second deposition cycle 400 includes introducing a carbon-containing inhibitor. The case of the second deposition cycle 400 may be subsequent to a previous cycle 401, which may be a first deposition cycle (e.g., exemplary first deposition cycle 300) or a second deposition cycle (e.g., exemplary second deposition cycle 400). At 402, the second deposition cycle 400 includes introducing an oxide film precursor into a processing chamber. As described above, the oxide film precursor may be optionally conformally adsorbed onto surface features of a substrate placed in the processing chamber. In the case of depositing a silicon-containing oxide film, exemplary oxide film precursors include polysilanes, siloxanes, aminosilanes, halosilanes, and organosilanes. In the case of depositing a metal oxide film, exemplary oxide film precursors include HfCl4, Hf(N(C2H5)2)4, Hf(OC(CH3)3)4, TCl4, Ti(OCH(CH3)2)4, WF6, WCl6, W(CO)6, SnCl4, (CH3)4Sn, (C2H5)4Sn, (CH3)2SnCl2, Bu2Sn(OMe)2, Sn(NMe2)4, Me2Sn(NMe2)2, Me3Sn(NMe2), MoCl5, MoO2Cl 2、 MoOCl4, and Mo(CO)6. At 404, the second deposition cycle 400 includes purging the process chamber to remove at least some residual oxide film precursor gas. At 406, the second deposition cycle 400 further includes introducing an oxygen-containing gas into the process chamber. Exemplary oxygen-containing gases include oxygen, ozone, and water vapor. At 408, the second deposition cycle 400 includes reacting the oxygen-containing gas with the adsorbed oxide film precursor. The deposition cycle 400 may include operating the RF power source at any suitable frequency (e.g., 400kHz, 13.56MHz) and any suitable power (e.g., between 0 watts and 6500 watts). In some examples, at 408, the method may also include reacting the oxygen-containing gas with a carbon-containing inhibitor that was non-conformally deposited in a previous cycle (e.g., a previous second deposition cycle 400). In some examples, the process chamber is optionally purged after the reaction in 408. In addition, in some examples, the substrate heater is heated for the second deposition cycle 400.

[0136] At 412, the second deposition cycle 400 further includes introducing a carbon-containing inhibitor into the process chamber. In some examples, the carbon-containing inhibitor may be introduced at 402 along with the oxide film precursor. The carbon-containing inhibitor may be selected to be non-conformally deposited on surface features of a substrate placed in the process chamber. The carbon-containing inhibitor is selected to form a gas-phase oxidized carbon species (e.g., CO and / or CO2, and other oxides, such as nitrogen oxides, depending on the constituent atoms of the carbon-containing inhibitor) when adsorbed to the substrate surface and exposed to a reactive oxygen-containing species. Any suitable carbon-containing inhibitor may be used. In some examples, the carbon-containing inhibitor may include a carbon-containing inhibitor having the general formula C n H 2n+2 alkane, wherein n is equal to 1 to 10. Examples of suitable alkanes may include methane, ethane, propane, butane, pentane, hexane, and substituted linear alkanes. Other examples of carbon-containing inhibitors may include olefins, alkynes, cyclic hydrocarbons, aromatics, alcohols, diols, aldehydes, esters, ethers, ketones, alkyl halides, alkylamines, or alkyl diamines. In still other examples, the carbon-containing inhibitor may include a mixture of carbon-containing inhibitors. Suitable olefins (for olefins having a single carbon-carbon double bond, wherein n is equal to 2 to 10 C n H 2n Examples of suitable alkynes (for alkynes having a single carbon-carbon triple bond, wherein n is equal to a C of 2 to 10) may include ethylene, propylene and butene. n H 2n-2 Examples of suitable hydrocarbons may include acetylene, propyne and butyne. Examples of suitable cyclic hydrocarbons may include cyclobutene, cyclopentane and cyclohexane. Examples of suitable aromatics may include benzene, toluene, pyridine and pyrimidine. Examples of suitable alcohols may include methanol, ethanol and propanol. Examples of suitable diols may include ethylene glycol, propylene glycol and hydroquinone. Examples of suitable aldehydes may include formaldehyde and acetaldehyde. Examples of suitable esters may include ethyl formate, methyl acetate and ethyl acetate. Examples of suitable ethers may include ethyl ether, methyl phenyl ether and aryl ethers such as furan. Examples of suitable ketones may include acetone and methyl ethyl ketone. Examples of suitable alkyl halides may include ethyl fluoride, isopropyl bromide and tert-butyl chloride. Examples of suitable alkylamines may include methylamine, dimethylamine, trimethylamine and piperidine. Examples of suitable alkyldiamines may include ethylenediamine and 1,3-diaminopropane.

[0137] The second deposition cycle 400 may be performed any suitable number of times during processing of the substrate. The second deposition cycle 400 may follow the previous deposition cycle 401 and may precede the subsequent deposition cycle 414, each of which may include the first deposition cycle 300 or the second deposition cycle 400. In the subsequent deposition cycle 414, the oxygen-containing gas may react with the adsorbed carbon-containing inhibitor to consume the oxygen-containing gas, thereby inhibiting the precursor reaction. When the carbon-containing precursor is non-conformally adsorbed to the substrate, the inhibition of oxide film formation may be more intense where more carbon-containing inhibitor is deposited.

[0138] In some examples, the substrate is heated via a substrate heater during the second deposition cycle. In some examples, the substrate heater may be heated to a temperature in the range of 25°C to 700°C, or to a higher temperature in some examples. Further, in some examples, the substrate heater may be heated to a temperature in the range of 25°C to 75°C. In other examples, temperatures outside of these ranges may be used. The temperature may be determined based at least on the properties of the carbon-containing inhibitor, such as the boiling point, vapor pressure, and / or adhesion coefficient of the carbon-containing inhibitor at a selected temperature and pressure.

[0139] In other examples, the second deposition cycle 400 may be performed using TALD. In such examples, the reaction at 408 may be performed using thermal energy. Furthermore, in other examples, the second deposition cycle 400 may be performed via CVD by introducing an oxide film precursor together with an oxygen-containing gas.

[0140] Back to Figure 2 When it is determined at 204 that the oxide film deposition cycle is run without a carbon-containing inhibitor, method 200 includes performing a first deposition cycle at 208. As mentioned above, Figure 3 The deposition cycle 300 is an example of the first deposition cycle 208. Likewise, when it is determined at 204 that the oxide film deposition cycle is run with a carbon-containing inhibitor, the method 200 includes performing a second deposition cycle 210. As mentioned above, Figure 4 The deposition cycle 400 is an example of the second deposition cycle 210. The relative proportion of deposition cycles with the carbon-containing inhibitor may be varied based on the desired amount of non-conformality of the oxide film. As described below, additional second deposition cycles may result in greater differences in thickness on different substrate features on different surfaces and / or at different aspect ratios within the gap. As such, when a greater amount of non-conformality is desired, the method 200 may include more second deposition cycles. Additionally or alternatively, when a greater amount of non-conformality is desired, the method 200 may include one or more second deposition cycles that expose the substrate to the carbon-containing inhibitor for a relatively longer duration.

[0141] As discussed below, various factors including the ratio of the first deposition cycle 208 to the second deposition cycle 210 may be adjusted to control the degree of non-conformal growth. At 212, the method 200 may perform additional deposition cycles, for example, depending on the overall treatment of the desired film. If additional deposition cycles are to be performed, the method returns to 204. Additional cycles result in thicker oxide film growth. A greater proportion of cycles including the introduction of carbon-containing inhibitors results in higher non-conformality. Any suitable number of deposition cycles may be performed. When the oxide film reaches a suitable thickness, the method may continue from 212 to 214 and terminate.

[0142] In certain examples, a low temperature SiO2 blanket oxide deposited according to the present disclosure may include to In some examples, the thickness may vary by ≤0.2% (R / 2). In addition, in some examples, the thickness may vary by ≤0.70% from substrate to substrate (range of average value of 25 substrates run continuously). In some examples, the SiO2 blanket oxide may include an adjustable wet etch rate and / or dry etch rate. In some examples, the SiO2 blanket oxide may include adder defects of ≤10 at 30nm. In some examples, the SiO2 blanket oxide may include a bulk modulus in the range of 70GPa to 80GPa. In some examples, the SiO2 blanket oxide may include 2.1 to 2.2g / cm 3 In some examples, the density can be within the range of ≤ In some examples, the SiO2 blanket oxide may include a carbon concentration of ≤0.5% and / or a nitrogen concentration of ≤0.5%. In other examples, the oxide film may have one or more values ​​outside of these ranges.

[0143] The oxide film deposition processes described herein may be used to fill any suitable gap in any suitable substrate. Figures 5A to 5B An exemplary substrate comprising a gap is shown. Figure 5A An example of an intermediate structure 500 including a substrate 502 with a gap 504 is schematically shown. More specifically, the intermediate structure 500 includes a stack 505 of alternating layers 506, 508. In some examples, the layers 506, 508 may include alternating oxide / nitride layers or alternating oxide / polysilicon layers. The intermediate structure 500 may represent an intermediate structure in a 3D NAND flash memory manufacturing process. In such an example, the gap 504 may represent a channel gap used to form a channel in a 3D NAND flash memory device. In other examples, the intermediate structure 500 may represent a structure formed during a 3D dynamic random access memory (DRAM) manufacturing process.

[0144] The gap 504 has a relatively high aspect ratio. For example, the gap 504 may have an aspect ratio in the range of 40: 1 to 100: 1. It should be understood that the gaps and other substrate features depicted herein may not be drawn to scale.

[0145] Figure 5BAn intermediate structure 510 is schematically shown including a substrate 512 having a concave gap 514. Substrate 512 is a generalization of substrate 502. In this example, the concave gap 514 includes a concave profile with negatively sloped sidewalls. The term "negatively sloped sidewalls" indicates sidewalls that extend below the edge of the opening of the gap. The opening of the gap 514 at the substrate surface is narrower than the width of the bottom of the gap. In other examples, the gap may include other types of concave features besides sloped sidewalls. Intermediate structure 510 represents any suitable concave intermediate structure in an integrated circuit manufacturing process.

[0146] As discussed above, using PEALD to fill a recessed gap or a high aspect ratio gap with an oxide film while avoiding the formation of voids can be challenging. For example, with respect to a high aspect ratio structure, the oxide film precursor and / or oxygen-containing gas may have a higher in-gap deposition rate at a location closer to the gap opening than at a location deeper within the gap. Furthermore, even with a uniform growth rate throughout the gap depth, conformal film growth may pinch off the recessed gap before completely filling the deeper portion of the gap because the narrower portion of the gap may close before the wider portion deeper within the gap.

[0147] Thus, non-conformal film growth according to the present disclosure can be used to address such challenges. As mentioned above, various process variables can be adjusted to affect the degree of film conformality. As an example, varying the time of exposure to a carbon-containing inhibitor in an oxide deposition cycle can change the conformality of the oxide film. In such an example, a longer exposure time can result in higher non-conformality. As another example, the ratio of the first oxide deposition cycle to the second oxide deposition cycle can be varied to change the conformality of the resulting oxide film.

[0148] Fig. 6A and 6B An exemplary gap fill process performed on intermediate structure 510 under different processing conditions is schematically shown. Process 600 may represent an ALD oxide film deposition process performed without the use of a carbon-containing inhibitor. Figures 6A to 6B 5. Film deposition on a substrate region 604 adjacent to the gap 514 is not shown in FIG. At 600a, conformal growth of a partial thickness of the oxide film 602 results in conformal narrowing of the gap 514. At 600b, continued conformal growth of the oxide film 602 further narrows the opening of the gap, as shown at 606. At 600c, the opening of the gap has been completely pinched off, as shown at 608. Thus, a pore 609 surrounded by the oxide film 602 is formed.

[0149] To avoid the formation of such pores, process 610 utilizes one or more oxide film deposition cycles including the introduction of a carbon-containing inhibitor, as described above, to grow the film non-conformally. Process 610 includes introducing a first, smaller amount of a carbon-containing gas to the process chamber. As shown at 610a, an oxide film 612 has grown relatively thicker at 614 at the bottom of the gap than at 616 of the sidewalls near the opening. At 610b, continued film growth narrows the gap 514 relatively uniformly across the depth of the gap. Finally, at 610c, the gap 514 is almost completely filled without pore formation.

[0150] The duration and frequency of exposure to the carbon-containing gas can be controlled by adjusting a number of parameters in the PEALD process. For example, an oxide film deposition process may include performing n first deposition cycles 300 followed by m second deposition cycles 400. The numbers n and m may be any suitable integers. These steps may be repeated any suitable number of times. In such an example, the proportion P of oxide film deposition cycles that include the introduction of a carbon-containing inhibitor may be determined by the following formula: In some examples, n and m may be changed during processing of the substrate. In addition, in some examples, the ratio P may be between 5% and 50%. In some such examples, the ratio P may be between 10% and 20%.

[0151] Figure 6B shows an intermediate structure formed by exemplary process 630, compared to Fig. 6A 6, process 630 uses a second deposition cycle with a larger ratio of P, and / or a longer exposure to a carbon-containing inhibitor. Although gap 514 is substantially uniformly narrowed in process 610, process 630 results in the bottom of gap 514 being filled well before the top of gap 514 is filled. For example, at 630a, oxide film 632 is relatively thick on the sidewalls of the gap in the bottom of the gap at 634, and relatively thin on the sidewalls in the upper portion of the gap at 636. The intermediate structures shown at 630b and 630c show oxide film 632 in further stages of growth, and depict gap filling from the bottom to the opening without void formation.

[0152] Oxide film 632 exhibits a relatively higher degree of non-conformal growth compared to oxide film 612. Thus, exposing the gap to a carbon-containing inhibitor for a relatively longer duration and / or a greater number of cycles including the carbon-containing inhibitor may provide a higher degree of non-conformal growth.

[0153] Figure 7An exemplary gap filling process performed on an intermediate structure 510 under different processing conditions is schematically shown. In this figure, the layers of the intermediate structure 500 are omitted for clarity. In addition, the intermediate structure 500 represents any relatively high aspect ratio intermediate structure in the substrate other than the layer structure and the via gap of FIG. 5 .

[0154] Process 700 may represent an ALD oxide film deposition process performed without the use of a carbon-containing inhibitor. Figure 7 504. In the figure, film deposition on the substrate region 704 adjacent to the gap 504 is not shown. At 700a, the growth of a partial thickness of the oxide film 702 results in a narrowing of the gap 504. The oxide film 702 grows slower at the bottom of the gap and grows faster near the opening of the gap outside of the saturation state. At 700b, continued growth of the oxide film 702 further narrows the opening of the gap, as shown at 706. At 700c, the opening of the gap has been completely pinched off, as shown at 708 to form a pore 709 surrounded by the oxide film 702.

[0155] Figure 7 Further shown is an intermediate structure formed by an exemplary process 720 that uses a carbon-containing inhibitor during an ALD cycle. As shown at 720a, an oxide film 722 has grown relatively thicker at 724 at the bottom of the gap 504 compared to 726 at the sidewalls near the opening. At 720b, continued film growth narrows the gap 504 as the bottom of the gap continues to fill. Finally, at 720c, the gap 504 is completely filled without void formation.

[0156] As mentioned above, for example Figures 6A to 6B In the context of these depicted at 610 or 630, the ratio of the number of oxide film deposition cycles that include a carbon-containing inhibitor to the number of cycles that omit the carbon-containing inhibitor may be selected to achieve a desired degree of non-conformal film growth to avoid the formation of voids. Additionally or alternatively, the duration of carbon-containing gas exposure in one or more cycles that include a carbon-containing inhibitor may be selected to achieve a desired degree of non-conformal oxide film growth.

[0157] In some examples, an oxide film structure having a seam depth ≥ 1 μm can be formed. In some examples, the seam non-uniformity within the substrate is between + / - 5 nm. In some examples, the oxide film structure may warp and have a variable of ≤ 80 μm. In some examples, the bottom fill percentage of the oxide film structure is ≥ 70%. In some examples, a blanket oxide can be formed with a wet etching rate ratio of ≤ 6. In some examples, the blanket oxide may have a non-uniformity of ≤ 2% within the substrate. In some examples, the blanket oxide may have a substrate-to-substrate non-uniformity of ≤ 0.5%. In some examples, the blanket oxide may have a defect of ≤ 10 at 60 nm. In other examples, the oxide film structure may have one or more values ​​outside these exemplary ranges.

[0158] Figure 8 A flow chart depicting an exemplary method 800 for performing atomic layer deposition to fill a gap on a substrate placed in a processing chamber is shown. At 802, method 800 includes performing at least one oxide film deposition cycle. In some examples, multiple oxide film deposition cycles are performed. The first deposition cycle 300 and the second deposition cycle 400 are examples of oxide film deposition cycles.

[0159] At 804, the oxide film deposition cycle 802 includes exposing the substrate to an oxide film precursor to adsorb the oxide film precursor to the substrate within the gap. In some examples, the gap is formed in alternating layers of materials. For example, the substrate may include a stack of alternating layers of different materials (e.g., 3D NAND or 3D DRAM). In other examples, the substrate may include any other suitable structure. Any suitable oxide film precursor may be used. In the case of silicon-containing oxide films, exemplary oxide film precursors include polysilanes, siloxanes, aminosilanes, halosilanes, and organosilanes, such as those described in more detail above. Exemplary oxide film precursors for metal oxide films include HfCl4, Hf(N(C2H5)2)4, Hf(OC(CH3)3)4, TCl4, Ti(OCH(CH3)2)4, WF6, WCl6, W(CO)6, SnCl4, (CH3)4Sn, (C2H5)4Sn, (CH3)2SnCl2, Bu2Sn(OMe)2, Sn(NMe2)4, Me2Sn(NMe2)2, Me3Sn(NMe2), MoCl5, MoO2Cl 2、 MoOCl4 and Mo(CO)6.

[0160] In some examples, as shown at 808, the gap includes a relatively high aspect ratio, such as in the range of 40: 1 to 100: 1. In other examples, the gap may include an aspect ratio outside of this range. In addition, in some examples, as shown at 810, the gap includes a concave structure.

[0161] Continuing, at 812, performing the oxide film deposition cycle 802 may optionally include purging the process chamber after introducing the oxide film precursor into the process chamber. Purging the process chamber may be performed to remove at least some residual oxide film precursor.

[0162] At 814, performing the oxide film deposition cycle 802 includes exposing an oxygen-containing gas to the substrate. Any suitable oxygen-containing gas may be used. Examples include oxygen, ozone, and water vapor. At 816, the oxide film deposition cycle 802 further includes reacting the oxide film precursor with the oxygen-containing gas. At 818, in the case of performing the oxide film deposition cycle using PEALD, the method 800 includes forming a plasma containing an oxygen-containing gas to form an oxygen-containing reactive species. In such an example, at 819, the method 800 further includes oxidizing the oxide film precursor by reacting the oxide film precursor with the oxygen-containing reactive species to form an oxide film. In some examples, at 820, at least some of the oxygen-containing reactive species in the plasma react with the adsorbed carbon-containing inhibitor that was non-conformally deposited in the previous oxide film deposition cycle, thereby reducing the availability of the oxygen-containing reactive species for reacting with the oxide film precursor and thus inhibiting oxide film growth. In some examples, at 822, the method includes sweeping the processing chamber after extinguishing the plasma.

[0163] In at least some deposition cycles, at 824, method 800 includes exposing the substrate to a carbon-containing inhibitor. As described above, any suitable carbon-containing inhibitor may be used. In some examples, the carbon-containing inhibitor includes a carbon-containing inhibitor having the general formula C n H 2n+2 alkane, wherein n is equal to 1 to 10. In some examples, the alkane comprises one or more of methane, ethane, propane, butane, pentane, or hexane. In addition, in some examples, the carbon-containing inhibitor comprises one or more of olefins, alkynes, cyclic hydrocarbons, aromatics, alcohols, diols, aldehydes, esters, ethers, ketones, alkyl halides, alkylamines, or alkyl diamines. In some examples, the alkane comprises a substituted straight chain alkane. In still other examples, the carbon-containing inhibitor may comprise a mixture of carbon-containing inhibitors. Suitable olefins (for olefins having a single carbon-carbon double bond, wherein n is equal to 2 to 10 C n H 2n Examples of suitable alkynes (for alkynes having a single carbon-carbon triple bond, wherein n is C in the range of 2 to 10) may include ethylene, propylene and butene. n H 2n-2Examples of suitable hydrocarbons may include acetylene, propyne and butyne. Examples of suitable cyclic hydrocarbons may include cyclobutene, cyclopentane and cyclohexane. Examples of suitable aromatics may include benzene, toluene, pyridine and pyrimidine. Examples of suitable alcohols may include methanol, ethanol and propanol. Examples of suitable diols may include ethylene glycol, propylene glycol and hydroquinone. Examples of suitable aldehydes may include formaldehyde and acetaldehyde. Examples of suitable esters may include ethyl formate, methyl acetate and ethyl acetate. Examples of suitable ethers may include ethyl ether, methyl phenyl ether and aryl ethers such as furan. Examples of suitable ketones may include acetone and methyl ethyl ketone. Examples of suitable alkyl halides may include ethyl fluoride, isopropyl bromide and tert-butyl chloride. Examples of suitable alkylamines may include methylamine, dimethylamine, trimethylamine and piperidine. Examples of suitable alkyldiamines may include ethylenediamine and 1,3-diaminopropane.

[0164] At 826, method 800 may further include performing one or more subsequent oxide film deposition cycles. In some examples, at 827, the subsequent oxide film deposition cycle may include introducing a carbon-containing inhibitor (e.g., second deposition cycle 400). Further, in some examples, at 828, the subsequent oxide film deposition cycle omits introducing a carbon-containing inhibitor (e.g., first deposition cycle 300). Further, at 830, in some examples, the subsequent oxide film deposition cycle includes reacting the carbon-containing inhibitor introduced at 824 with an oxygen-containing gas.

[0165] Thus, examples disclosed herein may provide for filling one or more gaps on a substrate in a manner that may avoid the formation of voids.Although disclosed in the context of gaps having relatively high aspect ratios or concave features, the disclosed examples may be used to fill any suitable gaps.

[0166] In some examples, a substrate having an initial critical dimension spacing imbalance uniformity (3 standard deviations) ≤ In some examples, the spacers may be formed to have a squareness of ≥ 90%. In some examples, the maximum spacing imbalance may be ≤ In some examples, the as-deposited critical dimension stability, as measured as an average of 6 substrate runs, may be ≤ In some examples, the structure may contain ≤ In some examples, the structure may include ≤ In some examples, the structure may include ≤ In other examples, the structure may have one or more values ​​outside of these exemplary ranges.

[0167] The examples described herein can provide efficient formation of films and / or structures on substrates with a relatively high degree of control over feature size, film thickness, uniformity, and other characteristics. In some examples, the throughput of forming low temperature oxide type films can be ≥125 substrates per chamber per hour. In some examples, the throughput of forming low temperature hard mask type films can be ≥90 substrates per chamber per hour. In some examples, a SiO2 blanket oxide can be formed using a chemical dosage of ≤2.6 mg per cycle. In some examples, the SiO2 blanket oxide can include a cumulative limit of ≥3.0 μm. In other examples, the film can have one or more values ​​outside of these exemplary ranges.

[0168] As another example, Fig. 9 Schematically showing oxide film growth on intermediate structure 900 under different processing conditions. Intermediate structure 900 may represent any suitable intermediate structure in an integrated circuit manufacturing process. Intermediate structure 900, shown here in a schematic cross-sectional view, includes substrate 902. Intermediate structure 900 further includes surface features, which in this example are mandrels 904A-B for a patterning process (e.g., SADP). Substrate 902 represents any suitable structure on which mandrels 904A-B may be formed. Mandrels 904A-B may have any suitable size. In some examples, mandrels 904A-B may have a cross-sectional width of 10 to 100 nm. Mandrels may include any suitable material. Examples include polycrystalline silicon, amorphous silicon, silicon oxide, silicon nitride, or carbon. Mandrels 904A-B may be formed on substrate 902 via any suitable process. For example, mandrels 904A-B may be formed via application of spin-on carbon followed by photolithographic patterning. Each mandrel includes a top horizontal surface 906 and sidewall surfaces 908, with a lower horizontal substrate surface 910 between mandrels 904A and 904B.

[0169] Fig. 9 Also shown are three processed intermediate structures after the growth of the oxide film. Processed intermediate structure 920 represents the growth of a conformal oxide film using a carbon-free PEALD process 922 that omits the use of a carbon-containing inhibitor. As shown, the thickness 924 of the oxide film 921 at the top horizontal surface of mandrel 904A is substantially equal to the thickness 926 along the vertical surface of mandrel 904A, and the thickness 928 of the oxide film deposited on the underlying substrate surface between the two mandrels 904A and 904B. The uniform thickness of the conformal oxide film 921 indicates uncontrolled growth of oxide films on different surfaces in the absence of a carbon-containing inhibitor.

[0170] The processed intermediate structure 930 represents a non-conformal oxide film 931 formed using a PEALD process 932 utilizing a carbon-containing inhibitor. The carbon-inhibited PEALD process 932 includes introducing a carbon-containing inhibitor into the process chamber for a first, shorter duration during each second deposition cycle 400. As shown at thickness 934, the oxide film 931 on the upper horizontal surface of the mandrel 904A is significantly thinner than the thickness 936 on the vertical surface of the mandrel 904A. The thickness 934 on the upper horizontal surface of the mandrel 904A is substantially equal to the thickness 938 on the underlying substrate surface. Such non-conformal growth results from the non-conformal adsorption of the carbon-containing inhibitor onto surfaces of different orientations, thereby providing relatively more inhibition on the horizontal surfaces 906, 910 and relatively less inhibition on the vertical surface 908.

[0171] The processed intermediate structure 940 schematically shows the result of growing an oxide film 941 when a carbon-containing inhibitor is introduced into the process chamber for a second longer duration during each second deposition cycle 400. The increase in exposure time to the carbon-containing inhibitor results in a relatively greater degree of non-conformality in the PEALD process 942 compared to the PEALD process 932. Fig. 9 , the thickness 944 of the film 941 at the upper horizontal surface is less than the thickness 934 of the film 931 on a similar horizontal surface. The thickness 948 on the lower horizontal substrate surface is similar to the thickness 944. In some examples, the top:sidewall ratio (thickness 944:thickness 946) ranges from 0.99 to 0.50, with smaller ratio values ​​associated with longer exposure durations of the carbon-containing inhibitor. In other examples, the top:sidewall ratio can have any other suitable value.

[0172] Fig.10 An example of non-conformal oxide film growth on an intermediate structure 900 in which the proportion of carbon-inhibiting deposition cycles is varied is schematically shown. In this example, the oxide film deposition process may include performing n first deposition cycles 300 (shown at 1002) followed by m second deposition cycles 400 (shown at 1004). The numbers n and m may be any suitable integers. These steps may be repeated at 1006 any suitable number of times. Thus, the proportion P of oxide film deposition cycles that include the introduction of a carbon-containing inhibitor may be determined by the following equation: In some examples, n and m may be changed during processing of the substrate. In addition, in some examples, the ratio P may be between 5% and 50%. In some such examples, the ratio P may be between 10% and 20%.

[0173] The processed intermediate structure 1020 includes an oxide film 1021 grown using a carbon-free PEALD process 1022. The carbon-free PEALD process 1022 includes a plurality of first deposition cycles 300, where m = 0. In this way, the oxide film 1021 is conformally deposited.

[0174] The processed intermediate structure 1030 schematically shows the result of growing an oxide film 1031 using a carbon inhibited PEALD process 1032. The carbon inhibited PEALD process 1032 includes performing n1 first deposition cycles 300, performing one second deposition cycle 400, and repeating, where n1 > 1. As shown, the oxide film 1031 is thinner at the upper horizontal surface (thickness 1034) than at the vertical surface (thickness 1036).

[0175] The processed intermediate structure 1040 schematically shows the result of growing an oxide film 1041 using a carbon inhibited PEALD process 1042, wherein the ratio of the second deposition cycle 400 performed is relatively higher than the PEALD process 1032. The carbon inhibited PEALD process 1042 includes performing n2 first deposition cycles 300, running one second deposition cycle 400 for a time t, and repeating, wherein n2>1 and n2<n1. Thus, the ratio P2 is greater than P1, wherein and The oxide film 1041 has a relatively smaller thickness 1044 at the upper horizontal surface than at the vertical surface 1046. In addition, due to the higher proportion of the second deposition cycles performed, the PEALD process 1042 produces a relatively thinner oxide film 1041 on the top of the mandrel (i.e., at thickness 1044) than the oxide film 1031 (i.e., at thickness 1034). Thus, a relatively higher proportion of carbon-inhibited deposition cycles can result in an oxide film having a higher degree of non-conformal growth.

[0176] As described above, controlled non-conformal growth of oxide films can have a variety of uses in device processing. Examples include patterning processes such as SADP processes. Fig.11A Schematically shows a cross-sectional view of an intermediate structure 1100 that includes an oxide film 1102 that has been non-conformally grown on a substrate 1104 and a mandrel 1106 by a PEALD process (e.g., via PEALD process 932 or PEALD process 1032) utilizing a first, relatively small amount of a carbon-containing inhibitor gas. Fig. 11B The intermediate structure 1110 includes an oxide film 1112 that has been non-conformally grown on a substrate 1114 and a mandrel 1116 using a second, larger amount of a carbon-containing inhibitor gas (eg, PEALD process 942 or PEALD process 1042 ).

[0177] The oxide film on top of and between the mandrels is removed via dry etching. Fig.11A , the result of performing a dry etch on the intermediate structure 1100 is shown at 1120. Mandrel 1106 has been removed, leaving spacers 1102a-1102d. As seen at 1122, spacer 1102d is tapered at the top. Such tapering of the spacer may have a negative impact on transfer etch performance. Such tapering may be more pronounced for longer etch times. In addition, longer etch times and tapering may be associated with the use of relatively small amounts of carbon-containing inhibitor gas.

[0178] like Fig. 11B As depicted in , the result of performing a dry etch on the intermediate structure 1110 is shown at 1130. The top layer of the oxide film 1112 is etched away so as to remove the mandrel 1116. As a result of the dry etching, square spacers 1112a to 1112d remain. Because the top of the non-conformal oxide film 1112 is relatively thin compared to the oxide film 1102, the dry etching process can be performed for less time compared to the example at 1120. With the reduced dry etching time, the sidewalls of the oxide film 1112 are exposed to the dry etching chemistry for less time. Due to the reduction in dry etching time, the square spacers 1112a to 1112d include square tops (e.g., see 1132 for square spacer 1112d). In this way, the use of a carbon-containing inhibitor gas during PEALD to form a non-conformal oxide film can help avoid tapering compared to the use of a conformal oxide film. In this way, the square spacers can provide relatively good transfer etching performance. In some examples, structures such as these can be formed on a substrate with an as-deposited critical dimension spacing imbalance uniformity (3 standard deviations) ≤ In some examples, the spacers may be formed to have a verticality of ≥ 90%. In some examples, the maximum spacer imbalance may be ≤ In some examples, the as-deposited critical dimension stability, as measured as an average of 6 substrate runs, may be ≤ In some examples, the structure may contain ≤ In some examples, the structure may include ≤ In some examples, the structure may include ≤ Sidewall roughness. In some examples, an oxide film structure having a seam depth ≥1 μm can be formed. In some examples, the seam non-uniformity within the substrate is between + / -5 nm. In some examples, the oxide film structure may warp and have a difference of ≤80 μm. In some examples, the bottom fill percentage of the oxide film structure is ≥70%. In some examples, a blanket oxide can be formed with a wet etch rate ratio of ≤6. In some examples, the blanket oxide may have a non-uniformity of ≤2% within the wafer. In some examples, the blanket oxide may have a wafer-to-wafer non-uniformity of ≤0.5%. In some examples, the blanket oxide may have a defect of ≤10 at 60 nm. In other examples, the oxide film structure may have one or more values ​​outside these exemplary ranges. In other examples, the structure may have one or more values ​​outside these exemplary ranges.

[0179] Fig.12 A flow chart of an exemplary method 1200 for performing atomic layer deposition to non-conformally grow an oxide film is shown. At 1202, the method 1200 includes performing at least one oxide film deposition cycle. In some examples, multiple oxide film deposition cycles are performed. The first deposition cycle 300 and the second deposition cycle 400 are examples of oxide film deposition cycles.

[0180] At 1204, the oxide deposition cycle 1202 includes exposing the substrate to an oxide film precursor. Any suitable oxide film precursor may be used. For example, when forming a silicon dioxide film, the oxide film precursor may include a polysilane, a siloxane, an aminosilane, a halosilane, or an organosilane, such as those described in more detail above. Exemplary oxide film precursors for metal oxide films include HfCl4, Hf(N(C2H5)2)4, Hf(OC(CH3)3)4, TCl4, Ti(OCH(CH3)2)4, WF6, WCl6, W(CO)6, SnCl4, (CH3)4Sn, (C2H5)4Sn, (CH3)2SnCl2, Bu2Sn(OMe)2, Sn(NMe2)4, Me2Sn(NMe2)2, Me3Sn(NMe2), MoCl5, MoO2Cl 2、 MoOCl4 and Mo(CO)6. In some examples, at 1206, the substrate includes a mandrel.

[0181] Continuing, the oxide deposition cycle 1202 may optionally include purging the process chamber at 1208. Purging the process chamber may be performed to remove at least some residual oxide film precursor.

[0182] At 1210, the oxide deposition cycle further includes introducing an oxygen-containing gas. Any suitable oxygen-containing gas may be used, such as oxygen, ozone, or water vapor. At 1212, the oxide deposition cycle 1202 further includes reacting the oxide film precursor with the oxygen-containing gas. In some examples, at 1214, the oxide deposition cycle 1202 includes forming a plasma containing the oxygen-containing gas to oxidize the oxide film precursor to form an oxide film. In some examples, the reactive oxygen-containing species in the plasma oxidizes adsorbed carbon-containing inhibitors that were non-conformally deposited in a previous cycle. In some examples, at 1216, the method includes purging the process chamber after extinguishing the plasma.

[0183] In at least some deposition cycles, at 1218, method 1200 includes exposing the substrate to a carbon-containing inhibitor. Any suitable carbon-containing inhibitor may be used. In some examples, at 1220, the carbon-containing inhibitor includes a carbon-containing inhibitor having the general formula C n H 2n+2 alkane, wherein n is equal to 1 to 10. In some examples, at 1222, the alkane comprises one or more of methane, ethane, propane, butane, pentane, or hexane. In some examples, the alkane comprises a substituted straight chain alkane. In some examples, the carbon-containing inhibitor comprises one or more of an olefin, an alkyne, a cyclic hydrocarbon, an aromatic, an alcohol, a diol, an aldehyde, an ester, an ether, a ketone, an alkyl halide, an alkylamine, or an alkyl diamine. In still other examples, the carbon-containing inhibitor may comprise a mixture of carbon-containing inhibitors. Suitable olefins (for olefins having a single carbon-carbon double bond, wherein n is equal to 2 to 10 C n H 2n Examples of suitable alkynes (for alkynes having a single carbon-carbon triple bond, wherein n is C in the range of 2 to 10) may include ethylene, propylene and butene. n H 2n-2 Examples of suitable hydrocarbons may include acetylene, propyne, and butyne. Examples of suitable cyclic hydrocarbons may include cyclobutene, cyclopentane, and cyclohexane. Examples of suitable aromatics may include benzene, toluene, pyridine, and pyrimidine. Examples of suitable alcohols may include methanol, ethanol, and propanol. Examples of suitable diols may include ethylene glycol, propylene glycol, and hydroquinone. Examples of suitable aldehydes may include formaldehyde and acetaldehyde. Examples of suitable esters may include ethyl formate, methyl acetate, and ethyl acetate. Examples of suitable ethers may include ethyl ether, methyl phenyl ether, or aryl ethers such as furan. Examples of suitable ketones may include acetone and methyl ethyl ketone. Examples of suitable alkyl halides may include ethyl fluoride, isopropyl bromide, and tert-butyl chloride. Examples of suitable alkylamines may include methylamine, dimethylamine, trimethylamine, and piperidine. Examples of suitable alkyl diamines may include ethylenediamine and 1,3-diaminopropane. In some examples, at 1228, a carbon-containing inhibitor is introduced in 5% to 25% of the deposition cycles.

[0184] In some examples, at 1230, the method 1200 further includes heating the substrate heater to a temperature in a range of 25°C to 75°C. In some examples, the method includes heating the substrate heater to a temperature in a range of 25°C to 650°C.

[0185] At 1240, the method 1200 may further include performing a subsequent oxide film deposition cycle. The subsequent oxide film deposition cycle may include introducing a carbon-containing inhibitor (e.g., the second deposition cycle 400). However, in some examples, at 1242, the subsequent oxide film deposition cycle omits introducing a carbon-containing inhibitor (e.g., the first deposition cycle 300). Furthermore, at 1244, the subsequent oxide film deposition cycle includes reacting the carbon-containing inhibitor introduced at 1218 with an oxygen-containing gas.

[0186] The examples described herein can provide efficient formation of films and / or structures on substrates with a relatively high degree of control over feature size, film thickness, uniformity, and other characteristics. In some examples, the throughput of forming low temperature oxide type films can be ≥125 substrates per chamber per hour. In some examples, the throughput of forming low temperature hard mask type films can be ≥90 substrates per chamber per hour. In some examples, a SiO2 blanket oxide can be formed using a chemical dosage of ≤2.6 mg per cycle. In some examples, the SiO2 blanket oxide can include a cumulative limit of ≥3.0 μm. In other examples, the film can have one or more values ​​outside of these exemplary ranges.

[0187] In some examples, the methods and processes described herein may be bound to a computing system of one or more computing devices. In particular, such methods and processes may be implemented as computer applications or services, application programming interfaces (APIs), libraries, and / or other computer program products.

[0188] Fig.13 Schematically illustrates a non-limiting example of a computing system 1300 that can implement one or more of the above methods and processes. The computing system 1300 is shown in simplified form. The computing system 1300 can take the form of one or more personal computers, workstations, computers integrated with substrate processing equipment, and / or network accessible server computers.

[0189] The computing system 1300 includes a logic machine 1302 and a storage machine 1304. The computing system 1300 may optionally include a display subsystem 1306, an input subsystem 1308, a communication subsystem 1310, and / or Fig.13 Controller 130 is an example of computing system 1300 .

[0190] Logic machine 1302 includes one or more physical devices configured to execute instructions. For example, the logic machine may be configured to execute instructions as part of one or more applications, services, programs, routines, libraries, objects, components, data structures, or other logical constructs. Such instructions may be implemented to perform a task, implement a data type, transform the state of one or more components, achieve a technical effect, or otherwise achieve a desired result.

[0191] The logic machine may include one or more processors configured to execute software instructions. Additionally or alternatively, the logic machine may include one or more hardware or firmware logic machines configured to execute hardware or firmware instructions. The processors of the logic machine may be single-core or multi-core, and the instructions executed thereon may be configured for sequential, parallel, and / or distributed processing. The various components of the logic machine may optionally be distributed between two or more separate devices that may be remotely located and / or configured for coordinated processing. Aspects of the logic machine may be virtualized and executed by a remotely accessible networked computing device configured for cloud computing.

[0192] The storage machine 1304 includes one or more physical devices configured to store instructions 1312 executable by a logic machine to implement the methods and processes described herein. When implementing such methods and processes, the state of the storage machine 1304 may be transformed—for example, to store different data.

[0193] The storage machine 1304 may include removable and / or built-in devices. The storage machine 1304 may include optical storage (e.g., CD, DVD, HD-DVD, Blu-ray disc, etc.), semiconductor storage (e.g., RAM, EPROM, EEPROM, etc.), and / or magnetic storage (e.g., hard disk drive, floppy disk drive, tape drive, MRAM, etc.), etc. The storage machine 1304 may include volatile, non-volatile, dynamic, static, read / write, read-only, random access, sequential access, location addressable, file addressable, and / or content addressable devices.

[0194] It should be understood that storage device 1304 includes one or more physical devices. However, various aspects of the instructions described herein may alternatively be propagated over a communication medium (eg, electromagnetic signals, optical signals, etc.) that is not retained for a limited duration by a physical device.

[0195] Aspects of the logic machine 1302 and the storage machine 1304 may be integrated together into one or more hardware logic components. Such hardware logic components may include, for example, field programmable gate arrays (FPGAs), program and application specific integrated circuits (PASIC / ASIC), program and application specific standard products (PSSP / ASSP), systems on chips (SOCs), and complex programmable logic devices (CPLDs).

[0196] When included, the display subsystem 1306 can be used to present a visual representation of the data stored by the storage machine 1304. The visual representation can take the form of a graphical user interface (GUI). Since the methods and processes described herein change the data stored by the storage machine and thus convert the state of the storage machine, the state of the display subsystem 1306 can also be converted to visually represent the changes in the underlying data. The display subsystem 1306 can include one or more display devices using almost any type of technology. Such a display device can be combined with the logic machine 1302 and / or the storage machine 1304 in a shared housing, or such a display device can be a peripheral display device.

[0197] When included, input subsystem 1308 may include or interface with one or more user input devices, such as a keyboard, mouse, or touch screen. In some examples, the input subsystem may include or interface with selected natural user input (NUI) components. Such components may be integrated or peripheral, and the conversion and / or processing of input actions may be handled on-board or off-board. Exemplary NUI components may include microphones for speech and / or voice recognition; and infrared, color, stereo, and / or depth cameras for machine vision and / or gesture recognition.

[0198] When included, the communication subsystem 1310 can be configured to communicatively couple the computing system 1300 with one or more other computing devices. The communication subsystem 1310 can include wired and / or wireless communication devices compatible with one or more different communication protocols. As non-limiting examples, the communication subsystem can be configured to communicate via a wireless telephone network or a wired or wireless local or wide area network. In some examples, the communication subsystem can allow the computing system 1300 to send and / or receive messages to and from other devices via a network such as the Internet.

[0199] It should be understood that the configuration and / or method described herein are exemplary in nature, and these specific embodiments or examples should not be considered to have limiting significance, because many variations are possible. The specific routine or scheme described herein can represent one or more of any number of processing strategies. Like this, the various actions shown and / or described can be performed in the order shown and / or described, in other orders, in parallel or omitted. Equally, the order of the above-mentioned processing can be changed.

[0200] The subject matter of the present disclosure includes all novel and nonobvious combinations and subcombinations of the various processes, systems and configurations, and other features, functions, acts, and / or properties disclosed herein, as well as any and all equivalents.

Claims

1. A method for forming an oxide film on a substrate, the method comprising: performing a plurality of oxide film deposition cycles, at least one oxide film deposition cycle of the plurality of oxide film deposition cycles comprising: exposing the substrate to an oxide film precursor to adsorb the oxide film precursor to the substrate, exposing the substrate to an oxygen-containing gas, reacting the oxide film precursor with the oxygen-containing gas, and The substrate is exposed to a carbon-containing inhibitor. The method of claim 1 , wherein the method comprises an atomic layer deposition process. 3 . The method of claim 1 , wherein a subsequent oxide film deposition cycle of the plurality of oxide film deposition cycles performed after the at least one oxide film deposition cycle omits exposing the substrate to the carbon-containing inhibitor. 4 . The method of claim 1 , wherein reacting the oxide film precursor with the oxygen-containing gas comprises forming a plasma comprising the oxygen-containing gas. 5 . The method of claim 4 , further comprising reacting the plasma with a carbon-containing suppressor deposited in a previous oxide film deposition cycle in the plurality of oxide film deposition cycles.

6. The method of claim 1, wherein the substrate comprises a stack of alternating layers of a first material and a second material, wherein a gap is formed in the stack of alternating layers of materials, and wherein the oxide film is deposited in the gap. 7 . The method of claim 6 , wherein the gap comprises an aspect ratio in a range of 40:1 to 100:

1. The method of claim 6 , wherein the gap comprises a concave structure.

9. The method of claim 1, wherein the carbon-containing inhibitor comprises one or more of an alkane, an alkene, an alkyne, a cyclic hydrocarbon, an aromatic, an alcohol, a diol, an aldehyde, an ester, an ether, a ketone, an alkyl halide, an alkylamine, or an alkyl diamine. 10 . The method according to claim 1 , wherein the oxide film comprises a silicon oxide film.

11. A processing tool comprising: Processing room; RF power source; one or more gas inlets leading into the processing chamber; flow control hardware configured to control the flow of gas through the one or more gas inlets; as well as A controller operably coupled to the flow control hardware and the RF power source, the controller configured to fill a gap in a substrate within the processing chamber by: operating the flow control hardware to introduce an oxide film precursor into the process chamber, operating the flow control hardware to introduce an oxygen-containing gas into the process chamber, operating the radio frequency power source to form a plasma comprising the oxygen-containing gas; as well as The flow control hardware is operated to introduce a carbon-containing suppressant into the processing chamber after the RF power source is operated to extinguish the plasma.

12. The processing tool of claim 11, wherein the controller is further configured to operate the flow control hardware to purge the processing chamber after the controller operates the RF power source to extinguish the plasma.

13. The processing tool of claim 11, further comprising a source of a carbon-containing inhibitor.

14. The processing tool of claim 13, wherein the carbon-containing inhibitor source comprises one or more of alkanes, alkenes, alkynes, cyclic hydrocarbons, aromatics, alcohols, diols, aldehydes, esters, ethers, ketones, alkyl halides, alkylamines, or alkyldiamines.

15. The processing tool of claim 11, wherein the controller is configured to operate the flow control hardware and the RF power source to perform a plurality of oxide film deposition cycles, at least some of the oxide film deposition cycles omitting operating the flow control hardware to introduce the carbon-containing suppressant.

16. The processing tool of claim 11, wherein the controller is configured to control the processing tool to fill a recessed gap in the substrate.

17. The processing tool of claim 11, further comprising a substrate heater operably coupled to the controller, and wherein the controller is configured to control the substrate heater to heat to a temperature in the range of 25°C to 75°C.

18. A computer-readable storage device comprising: Instructions executable by a computing device comprising a processor to control a substrate processing tool to fill a gap in a substrate, the instructions executable to: operating flow control hardware of the substrate processing tool to direct an oxide film precursor into a processing chamber to expose the gap to the oxide film precursor, operating the flow control hardware to introduce an oxygen-containing gas into the process chamber, operating a radio frequency power source to form a plasma comprising the oxygen-containing gas, and After extinguishing the plasma, the flow control hardware is operated to introduce a carbon-containing inhibitor into the processing chamber, thereby exposing the gap to the carbon-containing inhibitor.

19. The computer readable storage device of claim 18, wherein the instructions executable to operate the flow control hardware to introduce the carbon-containing inhibitor into the process chamber are executable to control the introduction of one or more of an alkane, an alkene, an alkyne, a cyclic hydrocarbon, an aromatic, an alcohol, a diol, an aldehyde, an ester, an ether, a ketone, an alkyl halide, an alkylamine, or an alkyldiamine into the process chamber.