Group III-V compound semiconductor single crystal substrate and method for producing same

By adjusting the cross angle between the crystal solid and the melt interface during the vertical crystal boat method of the Group III-V compound semiconductor single crystal substrate and using photoetching treatment, the problem of high fracture failure rate in slice processing is solved, and the finished product is improved and reduce dislocation density and asymmetry.

CN119053733APending Publication Date: 2024-11-29SUMITOMO ELECTRIC INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094765.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-04-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing Group III-V compound semiconductor single crystal substrates are prone to failure in slicing process, resulting in low yield and the prior art is difficult to effectively reduce the failure rate of failure in rupture.

Method used

The vertical crystal boat method (VB method) is used to contact the seed crystal and the raw material melt, so that the crystal solid grows on the raw material melt side of the seed crystal, and the interface between the crystal solid and the raw material melt has less than 90° relative to the axis of the crucible. and a corrugated pattern is formed by etching the light to reduce dislocation density and asymmetry.

Benefits of technology

The failure rate of the III-V compound semiconductor single crystal substrate during slice processing is effectively reduced, the yield is improved, and the corrugated pattern shown by photoetching treatment reduces the dislocation density and asymmetry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053733A_ABST
    Figure CN119053733A_ABST
Patent Text Reader

Abstract

The group III-V compound semiconductor single crystal substrate is an indium phosphide single crystal substrate having a circular main surface, and has a corrugated pattern viewed on the main surface by performing the following treatment. The corrugated pattern is a pattern corresponding to a part of corrugations extending concentrically from a wave source, and the wave source is not located on the main surface. In the treatment step, the main surface is horizontally disposed at a position 10 mm downward from the liquid surface of the 25 DEG C mixed liquid in the depth direction, and the main surface is irradiated with light of a reflective incandescent lamp of 500 W for 1-2 hours at a position 20 cm upward from the liquid surface. The mixed solution is composed of 10 g of chromium oxide (VI), 10 mL of a hydrofluoric acid solution having a concentration of 50 mass%, and 400 mL of pure water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a III-V group compound semiconductor single crystal substrate and a method for manufacturing the same. Background Art

[0002] Japanese Patent Publication No. 2012-236770 (Patent Document 1) and International Publication No. 2004 / 106597 (Patent Document 2) disclose III-V compound semiconductor single crystal substrates such as indium phosphide single crystal substrates. Japanese Patent Publication No. 2019-043788 (Patent Document 3) discloses a method for growing a compound semiconductor single crystal as a raw material for a compound semiconductor single crystal substrate, etc., using a so-called VB method such as a vertical Bridgman method. Typically, the above-mentioned III-V compound semiconductor single crystal substrate is manufactured by cutting a III-V compound semiconductor single crystal such as an indium phosphide single crystal, a gallium arsenide single crystal, etc. into a disc shape (hereinafter, the above-mentioned cutting is also referred to as "slicing").

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2012-236770;

[0006] Patent document 2: International Publication No. 2004 / 106597;

[0007] Patent document 3: Japanese Patent Application Publication No. 2019-043788. Summary of the invention

[0008] The III-V compound semiconductor single crystal substrate of the present invention is a III-V compound semiconductor single crystal substrate having a circular main surface, and the above-mentioned III-V compound semiconductor single crystal substrate is an indium phosphide single crystal substrate. The above-mentioned indium phosphide single crystal substrate has a corrugated pattern observed on the above-mentioned main surface by implementing the following treatment, and the above-mentioned corrugated pattern is a pattern equivalent to a part of the corrugations extending concentrically from the wave source, and the above-mentioned wave source is not located on the above-mentioned main surface.

[0009] Treatment: The main surface is horizontally arranged at a position 10 mm downward in the depth direction from the liquid surface of a mixed liquid at 25°C, and the main surface is irradiated with light from a 500 W reflective incandescent lamp for more than 1 hour and less than 2 hours from a position 20 cm upward from the liquid surface. The mixed liquid is composed of 10 g of chromium (VI) oxide, 10 mL of 50 mass % concentration hydrofluoric acid solution and 400 mL of pure water.

[0010] The III-V compound semiconductor single crystal substrate of the present invention is a III-V compound semiconductor single crystal substrate having a circular main surface, and the above-mentioned III-V compound semiconductor single crystal substrate is a gallium arsenide single crystal substrate. The above-mentioned gallium arsenide single crystal substrate has a corrugated pattern observed on the above-mentioned main surface by implementing the following treatment, and the above-mentioned corrugated pattern is a pattern equivalent to a part of the corrugations extending concentrically from the wave source, and the above-mentioned wave source is not located on the above-mentioned main surface.

[0011] Treatment: The main surface is horizontally arranged at a position 10 mm downward in the depth direction from the liquid surface of a mixed liquid at 25°C, and the main surface is irradiated with light from a 500 W reflective incandescent lamp for more than 5 minutes and less than 20 minutes from a position 20 cm upward from the liquid surface. The mixed liquid is composed of 10 g of chromium (VI) oxide, 10 mL of 50 mass % concentration hydrofluoric acid solution and 400 mL of pure water.

[0012] The manufacturing method of the III-V compound semiconductor single crystal substrate of the present invention uses a crystal growth device to manufacture the III-V compound semiconductor single crystal substrate, and the above-mentioned manufacturing method includes: a process of bringing a seed crystal into contact with a raw material melt and growing a crystal solid on the raw material melt side of the above-mentioned seed crystal to obtain a III-V compound semiconductor single crystal; and a process of cutting out the above-mentioned III-V compound semiconductor single crystal to obtain a III-V compound semiconductor single crystal substrate with a circular main surface. The above-mentioned crystal growth device has at least a cylindrical crucible and a heating element for heating the above-mentioned crucible, the above-mentioned crucible accommodates the above-mentioned seed crystal at its bottom, and accommodates the above-mentioned raw material melt at a position above the above-mentioned seed crystal, and the interface between the above-mentioned crystal solid and the above-mentioned raw material melt has an intersection angle less than 90° relative to the axis of the above-mentioned crucible. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is an explanatory diagram for explaining a corrugated pattern observed on the main surface of the III-V compound semiconductor single crystal substrate of the present embodiment by etching the main surface thereof using light, and the position of the wave source of the corrugated pattern.

[0014] Figure 2 The present invention is an explanatory diagram for explaining a corrugated pattern observed on a main surface of a conventional III-V compound semiconductor single crystal substrate by etching the main surface thereof using light, and a wave source position of the corrugated pattern.

[0015] Figure 3The III-V compound semiconductor single crystal substrate involved in the present embodiment is an explanatory diagram showing the absolute value of the difference between the radial expansion and contraction strain of the main surface and the tangential expansion and contraction strain, i.e., the residual strain, in polar coordinates with the center of the main surface as the origin and an imaginary line segment extending from the center of the main surface toward the wave source to a point 15 mm away from the periphery of the III-V compound semiconductor single crystal substrate as the polar axis.

[0016] Figure 4 Concerning an existing III-V compound semiconductor single crystal substrate, the invention is an explanatory diagram showing the absolute value of the difference between the radial expansion and contraction strain of the main surface and the tangential expansion and contraction strain, i.e., the residual strain, in polar coordinates with the center of the main surface as the origin and an imaginary line segment extending from the center of the main surface toward the wave source to a point 15 mm away from the periphery of the III-V compound semiconductor single crystal substrate as the polar axis.

[0017] Figure 5 The III-V compound semiconductor single crystal substrate according to the present embodiment is an explanatory diagram for explaining 69 measurement points set on the main surface in order to obtain the dislocation density of the main surface.

[0018] Figure 6 The III-V compound semiconductor single crystal substrate according to the present embodiment is a substrate that is Figure 1 The corrugated pattern shown and Figure 5 1 is an explanatory diagram of a method for determining the asymmetry of dislocations existing on the main surface using 69 measurement points shown.

[0019] Figure 7 This is a schematic diagram schematically illustrating a crystal growth apparatus for growing a group III-V compound semiconductor single crystal that is a raw material of a group III-V compound semiconductor single crystal substrate according to the present embodiment.

[0020] Figure 8 1 is a flowchart showing an example of a method for manufacturing a III-V compound semiconductor single crystal substrate according to the present embodiment. DETAILED DESCRIPTION

[0021] [Problems to be Solved by the Invention]

[0022] In the process of obtaining the compound semiconductor single crystal substrate disclosed in Patent Documents 1 to 2 by slicing, a more stringent yield rate is sometimes required. Specifically, when the compound semiconductor single crystal is sliced, the substrate may be broken or damaged, so-called cracking failure, and it is required to reduce the probability of the occurrence of the above-mentioned cracking failure (hereinafter also referred to as "crack failure rate"). In this case, the III-V compound semiconductor single crystal substrate disclosed in Patent Documents 1 to 2 has room for improvement from the perspective of reducing the crack failure rate.

[0023] In view of the above-mentioned actual situation, an object of the present invention is to provide a III-V compound semiconductor single crystal substrate having a reduced crack defect rate and a method for manufacturing the same.

[0024] [Effects of the Invention]

[0025] According to the present invention, it is possible to provide a III-V compound semiconductor single crystal substrate having a reduced cracking defect rate and a method for manufacturing the same.

[0026] [Overview of Embodiments]

[0027] First, an overview of the embodiments of the present invention is described. The inventors of the present invention have repeatedly conducted in-depth research to solve the above-mentioned problems, thereby completing the present invention. Specifically, as a method of growing a III-V compound semiconductor single crystal, which is a raw material for a III-V compound semiconductor single crystal substrate, in a crucible of a crystal growth device using a so-called VB method such as a vertical crystal boat method, the following method is adopted. That is, the interface between the crystal solid grown by the seed crystal on the raw material melt side and the above-mentioned raw material melt is not horizontal as in the past, but has an intersection angle of less than 90° relative to the axis of the above-mentioned crucible. The inventors found that when this method is used, the crack defect rate is reduced when the above-mentioned III-V compound semiconductor single crystal substrate is obtained by slicing. Furthermore, the inventors found that the wave source of the corrugated pattern obtained by subjecting the main surface of the III-V compound semiconductor single crystal substrate obtained by the above-mentioned method to a prescribed etching treatment is different from the existing ones and is not located on the main surface, thereby realizing the present invention.

[0028] Next, embodiments of the present invention are listed for explanation.

[0029] [1] A III-V compound semiconductor single crystal substrate according to one embodiment of the present invention has a circular main surface, and the III-V compound semiconductor single crystal substrate is an indium phosphide single crystal substrate. The indium phosphide single crystal substrate has a corrugated pattern observed on the main surface by performing the following treatment, and the corrugated pattern is a pattern corresponding to a portion of corrugations extending concentrically from a wave source, and the wave source is not located on the main surface.

[0030] Treatment: The main surface is horizontally arranged at a position 10 mm downward in the depth direction from the liquid surface of a mixed liquid at 25°C, and the main surface is irradiated with light from a 500 W reflective incandescent lamp for more than 1 hour and less than 2 hours from a position 20 cm upward from the liquid surface. The mixed liquid is composed of 10 g of chromium (VI) oxide, 10 mL of 50 mass % concentration hydrofluoric acid solution and 400 mL of pure water.

[0031] The indium phosphide single crystal substrate as the III-V compound semiconductor single crystal substrate having such characteristics can reduce the cracking defect rate during slicing.

[0032] [2] The diameter of the indium phosphide single crystal substrate is preferably 50 mm to 155 mm. Thus, for an indium phosphide single crystal substrate having a diameter of 50 mm to 155 mm, the cracking defect rate during slicing can be reduced.

[0033] [3] It is preferred that the dislocation density of the main surface is 0 cm -2 Above and 2000cm -2 As a result, it is possible to provide an indium phosphide single crystal substrate having a further reduced dislocation density over the entire main surface.

[0034] [4] It is preferred that the asymmetry of the dislocations present in the main surface is 1.8 or more, and the asymmetry is calculated as follows: the main surface is divided into a first region and a second region by an imaginary first straight line, the imaginary first straight line perpendicularly intersects an imaginary straight line extending in a direction from the wave source to the center of the main surface, and passes through the center of the main surface, and in the first region and the second region, two or more dislocations having a dislocation size of 1 mm are set at intervals of 5 mm or more in a direction away from the center of the main surface on an imaginary second straight line passing through the center of the main surface and perpendicularly intersecting the first straight line. 2 The number of dislocations is measured at the measuring points, and the number of dislocations is converted into a value per 1 cm based on the measurement results. 2 The area conversion value is obtained by subtracting the average value of the conversion value obtained from all the measurement points in the second region from the average value of the conversion value obtained from all the measurement points in the first region, and dividing the absolute value of the value obtained by the average value of the conversion value obtained from all the measurement points in the first region and the second region. In this way, the crack defect rate during slicing can be further reduced.

[0035] [5] A III-V compound semiconductor single crystal substrate according to one embodiment of the present invention has a circular main surface, and the III-V compound semiconductor single crystal substrate is a gallium arsenide single crystal substrate. The gallium arsenide single crystal substrate has a corrugated pattern observed on the main surface by performing the following treatment, and the corrugated pattern is a pattern corresponding to a portion of corrugations extending concentrically from a wave source, and the wave source is not located on the main surface.

[0036] Treatment: The main surface is horizontally arranged at a position 10 mm downward in the depth direction from the liquid surface of a mixed liquid at 25°C, and the main surface is irradiated with light from a 500 W reflective incandescent lamp for more than 5 minutes and less than 20 minutes from a position 20 cm upward from the liquid surface. The mixed liquid is composed of 10 g of chromium (VI) oxide, 10 mL of 50 mass % concentration hydrofluoric acid solution and 400 mL of pure water.

[0037] The gallium arsenide single crystal substrate as the III-V group compound semiconductor single crystal substrate having such characteristics can reduce the cracking defect rate during slicing.

[0038] [6] The diameter of the gallium arsenide single crystal substrate is preferably 75 mm to 205 mm. Thus, for a gallium arsenide single crystal substrate having a diameter of 75 mm to 205 mm, the cracking defect rate during slicing can be reduced.

[0039] [7] It is preferred that the dislocation density of the main surface is 0 cm -2 Over and 50cm -2 As a result, it is possible to provide a gallium arsenide single crystal substrate having a further reduced dislocation density over the entire main surface.

[0040] [8] It is preferred that the asymmetry of the dislocations present in the main surface is greater than or equal to 2.0, and the asymmetry is calculated as follows: the main surface is divided into a first region and a second region by an imaginary first straight line, the imaginary first straight line intersects perpendicularly with an imaginary straight line extending in a direction from the wave source to the center of the main surface, and passes through the center of the main surface, and in the first region and the second region, two or more dislocations having a dislocation size of 1 mm are set at intervals of at least 5 mm in a direction away from the center of the main surface on an imaginary second straight line passing through the center of the main surface and intersecting perpendicularly with the first straight line. 2 The number of dislocations is measured at the measuring points, and the number of dislocations is converted into a value per 1 cm based on the measurement results. 2The area conversion value is obtained by subtracting the average value of the conversion value obtained from all the measurement points in the second region from the average value of the conversion value obtained from all the measurement points in the first region, and dividing the absolute value of the value obtained by the average value of the conversion value obtained from all the measurement points in the first region and the second region. In this way, the crack defect rate during slicing can be further reduced.

[0041] [9] The main surface is preferably a surface having an off-angle of 0° or more and 15° or less relative to the {100} plane. Thus, the main surface can be a surface having excellent electrical and optical properties. Therefore, in a III-V compound semiconductor single crystal substrate having a surface having excellent electrical and optical properties as a main surface, the cracking defect rate during slicing can be reduced.

[0042]

[10] It is preferred that the absolute value of the difference between the tensile strain in the radial direction and the tensile strain in the tangential direction of the main surface, i.e., the average value of the residual strain, is 3.5×10 -5 As a result, the failure rate of cracking during slicing can be further reduced.

[0043]

[11] Preferably, in polar coordinates with the center of the main surface as the origin and an imaginary line segment extending from the center of the main surface toward the wave source to a point 15 mm away from the periphery of the III-V compound semiconductor single crystal substrate as the polar axis, the absolute value of the difference between the tensile strain in the radial direction and the tensile strain in the tangential direction of the main surface, i.e., the residual strain, does not have an n-fold symmetric distribution centered at the origin, wherein n is an integer greater than 2. Thus, the cracking defect rate during slicing can be more substantially reduced.

[0044]

[12] Preferably, the conductivity type of the III-V compound semiconductor single crystal substrate is electron-withdrawing type. Thus, in the electron-withdrawing type (hereinafter also referred to as "n-type") III-V compound semiconductor single crystal substrate, the cracking defect rate during slicing can be reduced.

[0045]

[13] Preferably, the III-V compound semiconductor single crystal substrate contains tin or sulfur as an impurity atom in the case of the indium phosphide single crystal substrate, and the III-V compound semiconductor single crystal substrate contains silicon as an impurity atom in the case of the gallium arsenide single crystal substrate. Thus, the cracking defect rate during slicing can be reduced in both the indium phosphide single crystal substrate containing tin or sulfur as an impurity atom and the gallium arsenide single crystal substrate containing silicon as an impurity atom.

[0046]

[14] It is preferred that the atomic concentration of the impurity atoms is 1×10 16 cm -3 Above and 1×10 19cm -3 As a result, it is possible to provide a III-V compound semiconductor single crystal substrate containing impurity atoms that change the conductivity type to n-type at an appropriate concentration.

[0047]

[15] Preferably, the impurity atoms in the III-V compound semiconductor single crystal substrate show a concentration distribution that changes in the same manner in the direction from the wave source toward the center of the main surface. Thus, in the III-V compound semiconductor single crystal substrate of n-type conductivity, the cracking defect rate during slicing can be further reduced.

[0048]

[16] A method for manufacturing a III-V compound semiconductor single crystal substrate according to one embodiment of the present invention uses a crystal growth device to manufacture a III-V compound semiconductor single crystal substrate, the method comprising: a step of bringing a seed crystal into contact with a raw material melt and growing a crystal solid on the raw material melt side of the seed crystal to obtain a III-V compound semiconductor single crystal; and a step of slicing the III-V compound semiconductor single crystal to obtain a III-V compound semiconductor single crystal substrate having a circular main surface, the crystal growth device having at least a cylindrical crucible and a heating element for heating the crucible, the crucible containing the seed crystal at its bottom and the raw material melt at a position above the seed crystal, the interface between the crystal solid and the raw material melt having an intersection angle of less than 90° relative to the axis of the crucible. By using the method for manufacturing a III-V compound semiconductor single crystal substrate having such a feature, a III-V compound semiconductor single crystal substrate having a reduced cracking defect rate during slicing can be obtained.

[0049] [Details of implementation method]

[0050] Hereinafter, one embodiment of the present invention (hereinafter, also referred to as "this embodiment") will be described in further detail, but the present invention is not limited thereto. Figure 1 The same or corresponding elements in this specification and the drawings are marked with the same symbols, and the same description is not repeated for them. In addition, in the drawings, in order to facilitate the understanding of each component, the scale is appropriately adjusted for representation, and the scale of each component shown in the drawings is not necessarily consistent with the scale of the actual component.

[0051] In this specification, expressions in the form of "A to B" refer to the upper and lower limits of a range (i.e., greater than A and less than B). When A has no unit but only B has a unit, the unit of A is the same as the unit of B. Furthermore, when compounds are represented by chemical formulas in this specification, when the atomic ratio is not particularly limited, all conventionally known atomic ratios are included and are not necessarily limited to the stoichiometric range.

[0052] In this specification, the "main surface" of the III-V compound semiconductor single crystal substrate refers to both of the two circular surfaces in the above-mentioned substrate. In the III-V compound semiconductor single crystal substrate, when at least one of the two surfaces meets the scope of the claims of the present invention, it belongs to the scope of the present invention. Furthermore, when the diameter of the III-V compound semiconductor single crystal substrate is recorded as "50mm", it means that the above-mentioned diameter is about 50mm (about 50 to 50.8mm), or it means 2 inches. When the above-mentioned diameter is recorded as "75mm", it means that the above-mentioned diameter is about 75mm (about 75 to 76.5mm), or it means 3 inches. When the above-mentioned diameter is recorded as "100mm", it means that the above-mentioned diameter is about 100mm (about 95 to 105mm), or it means 4 inches. When the above-mentioned diameter is recorded as "150mm", it means that the above-mentioned diameter is about 150mm (about 145 to 155mm), or it means 6 inches. When the diameter is expressed as "200 mm", it means that the diameter is about 200 mm (about 195 to 205 mm), or 8 inches. The diameter can be measured by using a conventionally known outer diameter measuring instrument such as a vernier caliper.

[0053] The above-mentioned III-V compound semiconductor single crystal substrate has a "circular" main surface as described below. In this specification, the "circle" representing the shape of the main surface includes not only a geometric circle, but also a shape in which the main surface does not form a geometric circle due to the formation of at least any one of a groove, a positioning edge (hereinafter, also referred to as "OF") or an index flat (hereinafter, also referred to as "IF") . That is, "the shape in which the main surface does not form a geometric circle" refers to a shape in which the length of a line segment extending from an arbitrary point on the periphery of the main surface to the center of the above-mentioned main surface, which extends from an arbitrary point on the above-mentioned groove, OF and IF to the center of the main surface, becomes shorter. In other words, in this specification, the shape of the main surface is referred to as "circular" based on the shape before the above-mentioned groove, OF and IF are formed. Therefore, with respect to the center of the main surface and the diameter of the above-mentioned substrate, its position and size (length) are calculated based on the circle before the above-mentioned groove, OF and IF are formed. It should be noted that “the shape in which the main surface does not form a geometric circle” also includes a shape in which the lengths of all line segments extending from any point on the periphery of the main surface to the center of the above-mentioned main surface are not necessarily the same due to the shape of the III-V compound semiconductor single crystal before the III-V compound semiconductor single crystal substrate is cut out. In this case, the center of the main surface refers to the position of the center of gravity, and the diameter of the above-mentioned substrate refers to the length of the longest line segment among the line segments extending from any point on the periphery of the above-mentioned substrate to the above-mentioned center of the above-mentioned main surface.

[0054] In the crystallographic description in this specification, [] is used to represent individual orientation, <> is used to represent collective orientation, () is used to represent individual planes, and {} is used to represent collective planes. In addition, negative crystallographic indices are usually expressed by marking "- (bar)" above the numbers. When marking them in this specification, a minus sign is marked before the numbers.

[0055] [III-V compound semiconductor single crystal substrate]

[0056] <First Embodiment: Indium Phosphide Single Crystal Substrate (InP Substrate)>

[0057] The III-V compound semiconductor single crystal substrate of the present embodiment, for example, the first embodiment, has a circular main surface. In particular, the III-V compound semiconductor single crystal substrate is an indium phosphide single crystal substrate (hereinafter, also referred to as "InP substrate"). The InP substrate has a corrugated pattern observed on the main surface by performing the following treatment. The corrugated pattern is a pattern corresponding to a portion of corrugations extending concentrically from a wave source. Furthermore, the wave source is not located on the main surface.

[0058] Treatment: The main surface is horizontally arranged at a position 10 mm downward in the depth direction from the liquid surface of a mixed liquid at 25°C, and the main surface is irradiated with light from a 500 W reflective incandescent lamp for more than 1 hour and less than 2 hours from a position 20 cm upward from the liquid surface. The mixed liquid is composed of 10 g of chromium (VI) oxide, 10 mL of 50 mass % concentration hydrofluoric acid solution and 400 mL of pure water.

[0059] In the InP substrate as the III-V compound semiconductor single crystal substrate having such characteristics, the wave source of the above-mentioned corrugated pattern is not located on the main surface, and therefore the crack defect rate in the slicing process can be reduced.

[0060] The diameter of above-mentioned InP substrate is preferably more than 50mm and below 155mm.Thus, for the InP substrate with a diameter more than 50mm and below 155mm, the rupture defective rate during the slicing process can be reduced.About the InP substrate with a diameter more than 50mm and below 155mm, specifically, preferably refer to an InP substrate with a diameter of 50mm, 75mm, 100mm or 150mm, in other words preferably refer to an InP substrate with a diameter of 2 inches, 3 inches, 4 inches or 6 inches.In addition, as mentioned above, the diameter of the InP substrate can be measured by using a known external diameter measuring instrument such as a vernier caliper.

[0061] <Second Embodiment: Gallium Arsenide Single Crystal Substrate (GaAs Substrate)>

[0062] The III-V compound semiconductor single crystal substrate of the present embodiment, for example, the second embodiment, has a circular main surface. In particular, the III-V compound semiconductor single crystal substrate is a gallium arsenide single crystal substrate (hereinafter, also referred to as a "GaAs substrate"). The GaAs substrate has a corrugated pattern observed on the main surface by performing the following treatment. The corrugated pattern is a pattern corresponding to a portion of corrugations extending concentrically from a wave source. Furthermore, the wave source is not located on the main surface.

[0063] Treatment: The main surface is horizontally arranged at a position 10 mm downward in the depth direction from the liquid surface of a mixed liquid at 25°C, and the main surface is irradiated with light from a 500 W reflective incandescent lamp for more than 5 minutes and less than 20 minutes from a position 20 cm upward from the liquid surface. The mixed liquid is composed of 10 g of chromium (VI) oxide, 10 mL of 50 mass % concentration hydrofluoric acid solution and 400 mL of pure water.

[0064] In the GaAs substrate which is a III-V compound semiconductor single crystal substrate having such characteristics, the wave source of the corrugated pattern is not located on the main surface, and therefore the crack defect rate in the slicing process can be reduced.

[0065] The diameter of the above-mentioned GaAs substrate is preferably more than 75mm and less than 205mm. Thus, for GaAs substrates with a diameter of more than 75mm and less than 205mm, the failure rate of fracture during slicing can be reduced. About GaAs substrates with a diameter of more than 75mm and less than 205mm, specifically, preferably refer to GaAs substrates with a diameter of 75mm, 100mm, 150mm or 200mm, in other words, preferably refer to GaAs substrates with a diameter of 3 inches, 4 inches, 6 inches or 8 inches. In addition, as mentioned above, the diameter of the GaAs substrate can be measured by using a known outer diameter measuring instrument such as a vernier caliper.

[0066] <Main surface>

[0067] The III-V compound semiconductor single crystal substrate of the present embodiment has a circular main surface as described above. Furthermore, the III-V compound semiconductor single crystal substrate (InP substrate and GaAs substrate) has a corrugated pattern observed on the main surface by performing the following treatment. Specifically, the corrugated pattern is observed on the main surface by performing the following treatment (hereinafter also referred to as "etching treatment using light"), wherein the main surface is horizontally arranged at a position 10 mm downward in the depth direction from the liquid surface of a mixed liquid at 25°C, and the main surface is irradiated with light from a 500W reflective incandescent lamp at a position 20 cm upward from the liquid surface, and the light is irradiated for more than 1 hour and less than 2 hours when the III-V compound semiconductor single crystal substrate is the indium phosphide single crystal substrate, and for more than 10 minutes and less than 20 minutes when the III-V compound semiconductor single crystal substrate is the gallium arsenide single crystal substrate, wherein the mixed liquid is composed of 10 g of chromium (VI) oxide, 10 mL of a 50% by mass hydrofluoric acid solution, and 400 mL of pure water. That is, the wavy pattern is a pattern that appears on the main surface for the first time by etching the main surface with light.

[0068] (Wave-like pattern and wave source position of the wave-like pattern)

[0069] The III-V compound semiconductor single crystal substrate has a corrugated pattern as described above. The corrugated pattern is a pattern observed on the main surface when the main surface is subjected to the etching process using light as described above. Figure 1This is an explanatory diagram for explaining the wavy pattern observed on the main surface of the III-V compound semiconductor single crystal substrate of the present embodiment by etching the main surface thereof using light, and the position of the wave source of the wavy pattern. In this specification, the "wavy pattern" refers to a pattern that can be likened to a pattern of waves that spread out in multiple circles (so-called ripples) that appears when an object falls on a water surface. Furthermore, the "wave source" of the wavy pattern refers to the starting point or source of the waves that generate the wavy pattern. Figure 1 As shown in FIG. 1 , the corrugated pattern P appearing on the main surface S of the III-V compound semiconductor single crystal substrate 100 of the present embodiment is a pattern corresponding to a portion of the corrugations extending concentrically from the wave source O, that is, a pattern formed by a plurality of continuous arcs bent in the same direction. Figure 1 As shown, the wave source O of the above-mentioned corrugated pattern P is not located on the main surface S.

[0070] The reason why the cracking defect rate during slicing is reduced in the III-V compound semiconductor single crystal substrate 100 having such a corrugated pattern P is not clear in detail, but it is presumed to be based on the following main reasons. First, it is considered that the corrugated pattern P observed on the main surface by the etching process using light as described above is a pattern corresponding to the concentration of impurity atoms added to the III-V compound semiconductor single crystal substrate 100 as a dopant or the like. In other words, the corrugated pattern P can be considered to be an image that visualizes the impurity atoms contained in the III-V compound semiconductor single crystal substrate 100.

[0071] Figure 2 This is an explanatory diagram for explaining a corrugated pattern observed on a main surface of a conventional III-V compound semiconductor single crystal substrate by etching the main surface thereof using light and the position of the wave source of the corrugated pattern. Figure 2As shown, in the conventional III-V compound semiconductor single crystal substrate 101, the wavy pattern P observed on the main surface S by etching with light usually has a wave source O located at the center or near the center of the main surface S, and is a pattern equivalent to ripples extending in concentric circles from the wave source O. This III-V compound semiconductor single crystal substrate 101 is achieved by making the interface between the crystal solid grown on the raw material melt side of the seed crystal and the above-mentioned raw material melt horizontal (or approximately horizontal) during the process of growing the III-V compound semiconductor single crystal as its raw material in the crucible of the crystal growth device. In this case, the impurity atoms contained in the III-V compound semiconductor single crystal substrate 101 correspond to the wavy pattern P as described above, and show a distribution extending in concentric circles from the center or near the center of the main surface S. At this time, the strain (hereinafter also referred to as "residual strain") generated in the III-V compound semiconductor single crystal substrate 101 due to the impurity atoms is expressed in polar coordinates with the wave source O as the origin, showing a point-symmetric (specifically, four-fold symmetric) distribution centered on the wave source (see Figure 4 ). Therefore, it can be understood that it is difficult for the existing III-V compound semiconductor single crystal substrate 101 to release the stress of the residual strain on the substrate. Therefore, it can be considered that since the stress of the residual strain is easily released during the slicing process for obtaining the III-V compound semiconductor single crystal substrate 101 from the III-V compound semiconductor single crystal, the cracking of the substrate will occur at a certain ratio.

[0072] On the other hand, Figure 1As shown, in the III-V compound semiconductor single crystal substrate 100 of the present embodiment, the corrugated pattern P has a corrugation source O outside the main surface S. That is, the corrugated source O is not located on the main surface S. Therefore, the corrugated pattern P of the III-V compound semiconductor single crystal substrate of the present embodiment is a pattern corresponding to a portion of the corrugations extending concentrically from the corrugation source O, that is, a pattern formed by a plurality of continuous arcs bent in the same direction. Such a III-V compound semiconductor single crystal substrate 100 is achieved by making the interface between the crystal solid grown on the raw material melt side of the seed crystal and the raw material melt not horizontal but having a crossing angle of less than 90° with respect to the axis of the crucible in a process of growing a III-V compound semiconductor single crystal as a raw material in a crucible of a crystal growth apparatus, as exemplified in the item [Method for Manufacturing III-V Compound Semiconductor Single Crystal Substrate] described later. In this case, the impurity atoms contained in the III-V compound semiconductor single crystal substrate 100 correspond to the above-mentioned corrugated pattern P, and show a distribution formed by multiple layers of arcs that are bent in the same direction on the main surface S. At this time, when the residual strain generated in the III-V compound semiconductor single crystal substrate 100 due to the impurity atoms is expressed in polar coordinates with the center of the main surface S as the origin, it does not show an n-fold symmetric (where n is an integer greater than 2) distribution centered on the origin, but can only show a one-fold symmetric distribution, especially a roughly mirror-symmetric distribution (see Figure 3 ). Thus, it can be understood that the III-V compound semiconductor single crystal substrate 100 of the present embodiment is easy to release the stress of the residual strain on the substrate (for example, it is easy to release the stress at the intersection of the outer periphery of the main surface and the left and right ends of the arc). Therefore, it can be considered that since the stress of the residual strain does not need to be released during the slicing process for obtaining the III-V compound semiconductor single crystal substrate 100 from the III-V compound semiconductor single crystal, the crack defect rate of the substrate is reduced.

[0073] Here, the details of the etching process using light are described. First, at least one of the two surfaces as the main surface is polished to an arithmetic average roughness Ra of 0.1 nm or more and 0.5 nm or less, thereby preparing a III-V compound semiconductor single crystal substrate with a polished surface. Furthermore, with the polished surface as the upper surface, the substrate is horizontally arranged at a position 10 mm downward in the depth direction from the liquid surface of a mixed liquid at 25°C, wherein the mixed liquid is composed of 10 g of chromium (VI) oxide, 10 mL of a 50% by mass concentration hydrofluoric acid solution, and 400 mL of pure water. Next, in the case where the substrate is, for example, an indium phosphide single crystal substrate, the polished surface is irradiated with light from a 500W reflective incandescent lamp (for example, trade name: "EYELAMP (registered trademark)", Iwasaki Electric Co., Ltd.) for 1 to 2 hours from a position 20 cm above the liquid surface, thereby etching the polished surface. Thus, a pattern can be formed on the polished surface. On the other hand, when the substrate is, for example, a gallium arsenide single crystal substrate, the light is irradiated to the polished surface for 5 to 20 minutes from a position 20 cm above the liquid surface, thereby etching the polished surface. Thus, a pattern can be formed on the polished surface. Finally, by visually observing the pattern formed on the polished surface, it can be determined whether the pattern is a wavy pattern, and if the pattern is a wavy pattern, it can be determined whether the wave source is located on the main surface.

[0074] In the case where the above-mentioned III-V compound semiconductor single crystal substrate is an indium phosphide single crystal substrate and in the case where it is a gallium arsenide single crystal substrate, the time for irradiating the main surface with the light of the reflective incandescent lamp (hereinafter also referred to as "etching time") is different and the reason why the above-mentioned etching time has a range is to make the pattern (corrugated pattern) formed on the polished surface clearer. Therefore, in the present invention, whether the above-mentioned III-V compound semiconductor single crystal substrate is an indium phosphide single crystal substrate or a gallium arsenide single crystal substrate, in order to make the pattern formed on the polished surface clearer, the above-mentioned etching time can be extended or shortened within the above-mentioned range. Furthermore, fine adjustments such as increasing or decreasing the intensity of light can also be made. It should be noted that the temperature of the mixed solution (25°C) refers to the temperature at the beginning of the etching process using light. Therefore, the temperature of the mixed solution sometimes fluctuates up and down during the above-mentioned etching process due to the thermal energy of the light of the reflective incandescent lamp, etc. In addition, in the above-mentioned etching process, in order to make the pattern formed on the polished surface clearer, it is preferred to shake the above-mentioned substrate in the mixed solution at predetermined intervals (for example, every 1 minute).

[0075] (Residual strain)

[0076] In the III-V compound semiconductor single crystal substrate of the present embodiment, the absolute value of the difference between the tensile strain in the radial direction and the tensile strain in the tangential direction of the main surface, that is, the average value of the residual strain, is preferably 3.5×10 -5 By setting the average value of the residual strain to 3.5×10 -5 Since the stress does not need to be released during the slicing process for obtaining the III-V compound semiconductor single crystal substrate, the crack defect rate of the substrate can be reduced. In addition, the lower limit of the average value of the residual strain is not particularly limited, but is usually 1.0×10 -6 Here, in this specification, the expansion and contraction strain in the radial direction of the main surface is sometimes represented by "Sr", and the expansion and contraction strain in the tangential direction of the main surface is sometimes represented by "St".

[0077] In particular, the average value of the residual strain can have a more preferred value depending on whether the III-V compound semiconductor single crystal substrate is an InP substrate or a GaAs substrate, or the type of impurity atoms contained in the substrate, the size of the diameter of the substrate, etc. For example, in the case of an InP substrate with a diameter of 50 mm containing tin as an impurity atom, the average value of the residual strain is more preferably 5.9×10 -6 In the case of an InP substrate having a diameter of 50 mm and containing sulfur as an impurity atom, the average value of the residual strain is more preferably 5.4×10 -6 the following.

[0078] In the case of an InP substrate having a diameter of 75 mm and containing tin as an impurity atom, the average value of the residual strain is more preferably 1.1×10 -5 In the case of an InP substrate having a diameter of 75 mm and containing sulfur as an impurity atom, the average value of the residual strain is more preferably 9.5×10 -6 In the case of an InP substrate having a diameter of 100 mm and containing tin as an impurity atom, the average value of the residual strain is more preferably 2.2×10 -5 In the case of an InP substrate having a diameter of 100 mm and containing sulfur as an impurity atom, the average value of the residual strain is more preferably 2.0×10 -5 In the case of an InP substrate with a diameter of 150 mm containing tin as an impurity atom, the average value of the residual strain is more preferably 3.9×10 -5 In the case of an InP substrate having a diameter of 150 mm and containing sulfur as an impurity atom, the average value of the residual strain is more preferably 3.4×10 -6 the following.

[0079] In the case of a GaAs substrate having a diameter of 75 mm and containing silicon as an impurity atom, the average value of the residual strain is more preferably 8.2×10 -6 In the case of a GaAs substrate having a diameter of 100 mm and containing silicon as an impurity atom, the average value of the residual strain is more preferably 1.0×10 -5 In the case of a GaAs substrate having a diameter of 150 mm and containing silicon as an impurity atom, the average value of the residual strain is more preferably 2.0×10 -5 In the case of a GaAs substrate having a diameter of 200 mm and containing silicon as an impurity atom, the average value of the residual strain is more preferably 3.5×10 -5 the following.

[0080] The absolute value of the difference between the tensile strain in the radial direction and the tensile strain in the tangential direction of the main surface, i.e., the residual strain, is expressed in polar coordinates with the center of the main surface as the origin and an imaginary line segment extending from the center of the main surface toward the wave source to a point 15 mm away from the periphery of the III-V compound semiconductor single crystal substrate as the polar axis. This is convenient for determining the amount and distribution of the residual strain contained in the III-V compound semiconductor single crystal substrate. This is because: through the polar coordinates, the distribution of the residual strain in the III-V compound semiconductor single crystal substrate can be visually understood, so that the ease of release of the residual strain during the slicing process for obtaining the substrate, i.e., the ease of occurrence of cracking defects (how much cracking defects) can be easily grasped. In this case, it is preferred that the residual strain in the III-V compound semiconductor single crystal substrate of the present embodiment does not have an n-fold symmetric distribution centered on the origin in the polar coordinates, and the n is an integer greater than 2. Specifically, it is preferred that the residual strain shows a single-fold symmetric distribution centered on the origin in the polar coordinates. In particular, from the viewpoint of further reducing the crack defect rate of the substrate, it is preferred that the residual strain shows a distribution having a symmetry close to mirror symmetry (hereinafter also referred to as "substantially mirror symmetry") with an imaginary straight line from the center of the main surface to the wave source as the central axis. It should be noted that in this specification, "n-fold symmetry" centered on the origin refers to a symmetry characterized as rotational symmetry centered on the origin, specifically, a symmetry that overlaps with itself when rotated (360 / n)° around the origin. The above n is an integer greater than 2, for example, "three-fold symmetry" refers to a symmetry that overlaps with itself when n=3 and rotates 120°.

[0081] The absolute value of the difference between the tensile strain in the radial direction and the tensile strain in the tangential direction of the above-mentioned main surface, that is, the residual strain (hereinafter also referred to as "|Sr-St|") can be measured based on the photoelastic method described in Appl. Phys. Lett. 47 (1985) pp. 365-367. First, in the same manner as the step of performing the above-mentioned etching process using light, at least one of the two surfaces of the main surface is polished to an arithmetic mean roughness Ra of 0.1 nm or more and 0.5 nm or less, thereby preparing a III-V compound semiconductor single crystal substrate with a polished surface. Next, by applying the above-mentioned photoelastic method to the polished surface, the residual strain existing on the entire surface of the above-mentioned polished surface can be measured. In particular, in the above-mentioned photoelastic method, the residual strain can be obtained in the form of an absolute value |Sr-St|. In the above-mentioned photoelastic method, the residual strain (|Sr-St|) is defined as follows in the following formula (1).

[0082] [Mathematical formula 1]

[0083]

[0084] In formula (1), k = (λπdn0 3 ).

[0085] In the above formula (1), λ represents the wavelength of the light used for measurement, d represents the thickness of the III-V compound semiconductor single crystal substrate used for measurement, n0 represents the refractive index, δ represents the phase difference caused by the birefringence of the sample to be measured, φ represents the main vibration azimuth, and p 11 、p 12 、p 44 represents the photoelastic constant.

[0086] According to the photoelasticity method, the residual strain (|Sr-St|) in the entire main surface of the substrate can be obtained by measuring only the phase difference δ and the main vibration azimuth φ caused by the birefringence of the sample to be measured.

[0087] Furthermore, based on the residual strain (|Sr-St|) in the entire main surface of the above-mentioned substrate, as for example Figure 3 and Figure 4 As shown, it can be represented in polar coordinates with the center of the above-mentioned main surface as the origin and an imaginary line segment extending from the center of the above-mentioned main surface toward the above-mentioned wave source to a point 15 mm long away from the outer periphery of the above-mentioned III-V compound semiconductor single crystal substrate as the polar axis.

[0088] Figure 3The III-V compound semiconductor single crystal substrate involved in the present embodiment is an explanatory diagram showing the absolute value of the difference between the radial expansion and contraction strain of the main surface and the tangential expansion and contraction strain, i.e., the residual strain, in polar coordinates with the center of the main surface as the origin and an imaginary line segment extending from the center of the main surface toward the wave source to a point 15 mm away from the periphery of the III-V compound semiconductor single crystal substrate as the polar axis. Figure 4 Concerning an existing III-V compound semiconductor single crystal substrate, the invention is an explanatory diagram showing the absolute value of the difference between the radial expansion and contraction strain of the main surface and the tangential expansion and contraction strain, i.e., the residual strain, in polar coordinates with the center of the main surface as the origin and an imaginary line segment extending from the center of the main surface toward the wave source to a point 15 mm away from the periphery of the III-V compound semiconductor single crystal substrate as the polar axis.

[0089] according to Figure 3 and Figure 4 It can be understood from the comparison that the residual strain in the main surface of the III-V compound semiconductor single crystal substrate of the present embodiment does not have an n-fold symmetric distribution (where n is an integer greater than 2) in the polar coordinates, but shows a 1-fold symmetric distribution centered at the origin. In particular, according to Figure 3 It can be understood that the residual strain of the III-V compound semiconductor single crystal substrate of the present embodiment shows a distribution that is roughly mirror-symmetrical with the imaginary straight line from the center of the main surface to the wave source as the central axis. It can be understood that since the polar coordinates show a one-fold symmetry, especially a roughly mirror-symmetrical distribution with the origin as the center, the III-V compound semiconductor single crystal substrate of the present embodiment has a portion on the substrate that is easy to release the stress of the residual strain. On the other hand, it can be understood that since the conventional III-V compound semiconductor single crystal substrate shows a four-fold symmetric distribution with the origin as the center in the polar coordinates, there is no portion on the substrate that is easy to release the stress of the residual strain.

[0090] In addition, in the III-V compound semiconductor single crystal substrate of the present embodiment, when the above-mentioned residual strain is measured, the measurement can be performed before the dislocation density of the main surface described later is obtained, or the measurement can be performed after the dislocation density of the main surface is obtained. When the above-mentioned residual strain is measured after the dislocation density of the main surface is obtained, since etching pits corresponding to dislocations (etching pits) are formed on the main surface, in order to remove the etching pits and to make the main surface the above-mentioned polished surface, both sides of the above-mentioned main surface can be polished.

[0091] (Declination angle)

[0092] Preferably, the above-mentioned main surface is a surface having an off-angle of 0° or more and 15° or less relative to the {100} plane. In the case where the above-mentioned main surface has an off-angle of 0° or more and 15° or less relative to the {100} plane, the main surface of the III-V compound semiconductor single crystal substrate is a surface having an orientation with excellent electrical and optical properties. Therefore, this embodiment can reduce the crack defect rate in the III-V compound semiconductor single crystal substrate having a surface with excellent electrical and optical properties as the main surface.

[0093] This III-V compound semiconductor single crystal substrate can be obtained by slicing a III-V compound semiconductor single crystal, which is a raw material of the III-V compound semiconductor single crystal substrate, with the {100} just plane having no off-angle as the main surface. Alternatively, it can be obtained by subjecting the above-mentioned III-V compound semiconductor single crystal to a previously known inclined slicing method in a manner in which a plane having an off-angle greater than 0° and less than 15° relative to the {100} plane is the main surface. In the case of obtaining such a raw material (III-V compound semiconductor single crystal), the growth direction of the III-V compound semiconductor single crystal is preferably in the <100> direction. Here, the above-mentioned "off-angle" in the present invention has an accuracy error of ±0.5°. For example, in the case where the main surface is a {100} just plane, the above-mentioned main surface may have an off-angle of -0.5 to 0.5° relative to the {100} plane. Furthermore, for example, when the main surface has an off angle of 15° with respect to the {100} plane, the main surface may have an off angle of 14.5 to 15.5° with respect to the {100} plane.

[0094] The off angle of the main surface of the III-V compound semiconductor single crystal with respect to the {100} plane can be measured using a conventionally known crystal orientation measuring apparatus (for example, trade name (model): “2991G2”, manufactured by Rigaku Corporation).

[0095] (Dislocation density)

[0096] When the III-V compound semiconductor single crystal substrate is an InP substrate, the dislocation density of the main surface is preferably 0 cm -2 Above and 2000cm -2 The dislocation density of the main surface is more preferably 0 cm -2 Over 1500cm -2 On the other hand, when the III-V compound semiconductor single crystal substrate is a GaAs substrate, the dislocation density of the main surface is preferably 0 cm -2 Over 50cm -2 The dislocation density of the main surface is more preferably 0 cm -2Over and 30cm -2 As a result, it is possible to provide a III-V compound semiconductor single crystal substrate (InP substrate and GaAs substrate) with a further reduced dislocation density over the entire surface of the main surface. Therefore, in this embodiment, for a III-V compound semiconductor single crystal substrate with a reduced dislocation density over the entire surface of the main surface, the crack defect rate can be reduced.

[0097] In particular, the dislocation density of the main surface can have a more preferred value depending on whether the III-V compound semiconductor single crystal substrate is an InP substrate or a GaAs substrate, or the type of impurity atoms contained in the substrate, the size of the diameter of the substrate, etc. For example, in the case of an InP substrate with a diameter of 50 mm containing tin as an impurity atom, the dislocation density of the main surface is more preferably 1000 cm -2 In the case of an InP substrate having a diameter of 50 mm containing sulfur as an impurity atom, the diameter is preferably 200 cm -2 .

[0098] In the case of an InP substrate having a diameter of 75 mm and containing tin as an impurity atom, the dislocation density of the main surface is more preferably 2000 cm -2 In the case of an InP substrate having a diameter of 75 mm and containing sulfur as an impurity atom, the dislocation density of the main surface is more preferably 350 cm -2 In the case of an InP substrate having a diameter of 100 mm and containing tin as an impurity atom, the dislocation density of the main surface is more preferably 2000 cm -2 In the case of an InP substrate having a diameter of 100 mm and containing sulfur as an impurity atom, the dislocation density of the main surface is more preferably 600 cm -2 In the case of an InP substrate having a diameter of 150 mm and containing tin as an impurity atom, the dislocation density of the main surface is more preferably 2000 cm -2 In the case of an InP substrate having a diameter of 150 mm and containing sulfur as an impurity atom, the dislocation density of the main surface is more preferably 700 cm -2 the following.

[0099] In the case of a GaAs substrate having a diameter of 75 mm and containing silicon as an impurity atom, the dislocation density of the main surface is more preferably 25 cm -2 In the case of a GaAs substrate having a diameter of 100 mm and containing silicon as an impurity atom, the dislocation density of the main surface is more preferably 35 cm -2In the case of a GaAs substrate having a diameter of 150 mm and containing silicon as an impurity atom, the dislocation density of the main surface is more preferably 35 cm -2 In the case of a GaAs substrate having a diameter of 200 mm and containing silicon as an impurity atom, the dislocation density of the main surface is more preferably 90 cm -2 the following.

[0100] In this specification, "dislocation" and "dislocation density" of the main surface refer to "etch pits" and "etch pit density (EtchPit Density, hereinafter also referred to as "EPD")", respectively. "Etch pits" refer to corrosion pits formed on the surface of a III-V compound semiconductor single crystal substrate by treating the surface with chemicals. Specifically, in the case where the III-V compound semiconductor single crystal substrate is an indium phosphide single crystal substrate, "etch pits" refer to corrosion pits formed on the above main surface when the above substrate is immersed in a 25°C solution composed of hydrogen bromide and phosphoric acid in a mass ratio of hydrogen bromide:phosphoric acid of 1:2 for 1 to 5 minutes. Furthermore, in the case where the III-V compound semiconductor single crystal substrate is a gallium arsenide single crystal substrate, "etch pits" refer to corrosion pits formed on the above main surface when the above substrate is immersed in molten potassium hydroxide at 600°C for 45 minutes. In addition, when the main surface of the III-V compound semiconductor single crystal substrate is a polished surface after polishing, before immersing the above-mentioned substrate in a chemical solution, the above-mentioned polished surface of, for example, an indium phosphide single crystal substrate can be pre-treated with reverse aqua regia, and the above-mentioned polished surface of, for example, a gallium arsenide single crystal substrate can be pre-treated with sulfuric acid and hydrogen peroxide. In this way, the corrosion pits on the above-mentioned main surface can be made clearer. When the main surface of the III-V compound semiconductor single crystal substrate is observed through an optical microscope, the above-mentioned corrosion pits appear as white spots. Academically, the corrosion pits are not synonymous with dislocations, but can be regarded as equivalent to dislocations in this technical field.

[0101] The following is a method for measuring the etch pits formed on the main surface of the III-V compound semiconductor single crystal substrate and a method for calculating the EPD, referring to Figure 5 , the case where the III-V compound semiconductor single crystal substrate is a GaAs substrate with a diameter of 150 mm is used as an example for explanation. Figure 5 The III-V compound semiconductor single crystal substrate according to the present embodiment is an explanatory diagram for explaining 69 measurement points set on the main surface in order to obtain the dislocation density of the main surface.

[0102] First, the main surface of the III-V compound semiconductor single crystal substrate (GaAs substrate) 100 is immersed in molten potassium hydroxide at 600° C. for 45 minutes. As for the immersion method, a conventionally known method can be used. Then, the III-V compound semiconductor single crystal substrate 100 is taken out from the molten potassium hydroxide. Next, as Figure 5 As shown, 69 measuring points M are set in the main surface S of the III-V compound semiconductor single crystal substrate 100 (one measuring point M is a 1 mm 2 The 69 measurement points M are used as the object, and the number of etch pits is measured at a magnification of 100 times using a known optical microscope (e.g., trade name: "ECLIPSE (registered trademark) LV150N", manufactured by Nikon Corporation). Finally, the number of etch pits measured at the above 69 measurement points M is converted into a square per 1 cm 2 Thus, we can get the area value of 69 pits per 1cm 2 Since the numerical value of the area is obtained, the average value of the 69 numerical values ​​can be calculated as the EPD.

[0103] According to the above method, the number of etch pits can be measured by making one field of view (size of 1 mm×1 mm) correspond to one measuring point. In addition, when the III-V compound semiconductor single crystal substrate 100 is an InP substrate, the method for measuring the etch pits formed on its main surface S and the method for calculating the EPD can be obtained by the same method as the method for measuring the etch pits in the above GaAs substrate and the method for calculating the EPD except that the main surface is immersed in the above-mentioned solution of hydrogen bromide:phosphoric acid at a mass ratio of 1:2 at 25°C for 1 to 5 minutes.

[0104] Here, in Figure 5 In the substrate shown in FIG. 1 , the 69 measurement points M are arranged in the order of 5, 7, 9, 9, 9, 9, 9, 7, and 5 from the right side in the direction of the perpendicular line relative to the positioning edge OF provided at the upper portion. These measurement points M are provided at intervals I of 15 mm from each other. That is, when the diameter of the III-V compound semiconductor single crystal substrate is 150 mm, the measurement points M can be set at 69 points within the plane of the main surface S by setting the interval I between one measurement point M and the other measurement points M most adjacent to the measurement point M to 15 mm.

[0105] When the diameter of the III-V compound semiconductor single crystal substrate is 50 mm, the measurement points M can be set at 69 locations within the plane of the main surface S by setting the interval I between one measurement point M and the other measurement points M that are most adjacent to the measurement point M to 5 mm. Similarly, when the diameter of the III-V compound semiconductor single crystal substrate is 75 mm, the measurement points M can be set at 69 locations within the plane of the main surface S by setting the interval I between one measurement point M and the other measurement points M that are most adjacent to the measurement point M to 7.5 mm. When the diameter of the III-V compound semiconductor single crystal substrate is 100 mm, the measurement points M can be set at 69 locations within the plane of the main surface S by setting the interval I between one measurement point M and the other measurement points M that are most adjacent to the measurement point M to 10 mm. When the diameter of the III-V compound semiconductor single crystal substrate is 200 mm, the above-mentioned measurement points M can be set at 69 locations within the plane of the main surface S by setting the interval I between one measurement point M and another measurement point M most adjacent to the measurement point M to 20 mm.

[0106] (Dislocation asymmetry)

[0107] In the case where the above-mentioned III-V compound semiconductor single crystal substrate is an InP substrate, the asymmetry of the dislocations existing in the above-mentioned main surface is preferably greater than 1.8, and more preferably greater than 2.0. Furthermore, in the case where the above-mentioned III-V compound semiconductor single crystal substrate is a GaAs substrate, the asymmetry of the above-mentioned dislocations is preferably greater than 2.0, and more preferably greater than 2.3. The above-mentioned asymmetry is calculated as follows: the above-mentioned main surface is divided into a first region and a second region by an imaginary first straight line, and the above-mentioned imaginary first straight line intersects perpendicularly with an imaginary straight line extending in a direction from the above-mentioned wave source to the center of the above-mentioned main surface, and passes through the center of the above-mentioned main surface. In the first region and the second region, on an imaginary second straight line passing through the center of the above-mentioned main surface and intersecting perpendicularly with the above-mentioned first straight line, two or more dislocations with a diameter of 1 mm are set at intervals of more than 5 mm in a direction away from the center of the above-mentioned main surface. 2 The number of dislocations is measured at the measuring points, and the number of dislocations is converted into a value per 1 cm based on the measurement results. 2 The converted value of the area is obtained by subtracting the average value of the conversion values ​​obtained based on all the above-mentioned measurement points in the above-mentioned second area from the average value of the above-mentioned conversion values ​​obtained based on all the above-mentioned measurement points in the above-mentioned first area, and dividing the absolute value of the thus obtained value by the average value of the above-mentioned conversion values ​​obtained based on all the above-mentioned measurement points in the above-mentioned first area and the above-mentioned second area.

[0108] In this specification, "dislocation asymmetry" refers to the following index: when the above-mentioned main surface is divided into a first region and a second region by an imaginary first straight line, the above-mentioned imaginary first straight line intersects perpendicularly with an imaginary straight line extending in the direction from the above-mentioned wave source to the center of the above-mentioned main surface, and the number of dislocations respectively existing in the first region and the second region through the center of the above-mentioned main surface is compared to indicate the degree of difference between them. Although the detailed reason is unknown, the larger the value of the "dislocation asymmetry", the more it can further reduce the crack defect rate during slicing. The "dislocation asymmetry" of the III-V compound semiconductor single crystal substrate of this embodiment can show a larger value than that of the existing III-V compound semiconductor single crystal substrate based on the following reasons.

[0109] This is because, as described above, when the main surface of the III-V compound semiconductor single crystal substrate of the present embodiment is subjected to an etching process using light, a corrugated pattern in which the wave source is not located on the main surface can be observed on the above main surface. On the other hand, when the main surface of the conventional III-V compound semiconductor single crystal substrate is subjected to an etching process using light, a corrugated pattern in which the wave source is located at the center or near the center of the main surface can be observed on the above main surface. At this time, it can be considered that the above-mentioned corrugated pattern in the conventional III-V compound semiconductor single crystal substrate becomes a pattern equivalent to corrugations extending concentrically from the wave source located at the center or near the center of the main surface as described above, so the number of dislocations existing in the first region and the second region is the same or similar, so the "dislocation asymmetry" becomes small. On the other hand, it can be considered that the above-mentioned corrugated pattern in the III-V compound semiconductor single crystal substrate of the present embodiment becomes a pattern formed by multiple layers of arcs bent in the same direction as described above, so the number of dislocations existing in the first region and the second region is different, so the "dislocation asymmetry" becomes large. Furthermore, it is considered that the larger the value of the "dislocation asymmetry", the more strain-low orientation will appear in the III-V compound semiconductor single crystal. Therefore, if the substrate is obtained by slicing the single crystal along this orientation, the cracking defect rate can be further reduced.

[0110] In the case of the III-V compound semiconductor single crystal substrate of the present embodiment, in the case of an InP substrate, the asymmetry of the dislocation can be greater than 1.8. In contrast, in the existing InP substrate, the asymmetry is usually less than 1.8. In the case of the III-V compound semiconductor single crystal substrate of the present embodiment is a GaAs substrate, the asymmetry of the dislocation can be greater than 2.0. In contrast, in the existing GaAs substrate, the asymmetry is usually less than 2.0.

[0111] The following is a method for calculating the "asymmetry of dislocations" existing on the above-mentioned main surface, referring to Figure 6 Provide specific instructions. Figure 6 The III-V compound semiconductor single crystal substrate according to the present embodiment is a substrate that is Figure 1 The corrugated pattern shown and Figure 5 1 is an explanatory diagram of a method for determining the asymmetry of dislocations existing on the main surface using 69 measurement points shown.

[0112] First, the main surface S of the III-V compound semiconductor single crystal substrate 100 is subjected to the above-mentioned etching process using light, thereby forming a corrugated pattern P on the main surface S. After the position of the wave source is determined based on the above-mentioned corrugated pattern P, an imaginary straight line extending in the direction from the above-mentioned wave source to the center of the main surface S is set on the main surface S. Next, the position of an imaginary first straight line L1 on the main surface S that intersects the above-mentioned imaginary straight line perpendicularly and passes through the center of the above-mentioned main surface is determined. Furthermore, the position of the imaginary first straight line L1 is recorded on the main surface S by methods such as making the periphery of the III-V compound semiconductor single crystal substrate 100 defective or marking a mark on the main surface S. Then, the above-mentioned corrugated pattern is removed from the main surface S by polishing the main surface S.

[0113] Next, 69 measurement points M are set on the main surface S in the same manner as the above-mentioned method for measuring the dislocation density. Furthermore, the main surface S is divided into a first region R1 and a second region R2 based on an imaginary first straight line L1 recorded on the main surface S. Next, an imaginary second straight line L2 is set that passes through the center of the main surface S and intersects the first straight line L1 perpendicularly, and measurement points M that overlap with the second straight line L2 are selected in the first region R1 and the second region R2, respectively.

[0114] Next, the number of dislocations (etching pits) is measured at the measurement points M selected in each of the first region R1 and the second region R2, and the number of dislocations is converted into a value per 1 cm based on the measurement results. 2 The converted value of the area. Furthermore, the average value of the converted value obtained from all the measurement points M selected in the second region R2 is subtracted from the average value of the converted value obtained from all the measurement points M selected in the first region R1. Finally, the absolute value of the value obtained by the subtraction operation is divided by the average value of the converted value obtained from all the measurement points M selected in each of the first region R1 and the second region R2. The "dislocation asymmetry" can be obtained by the above method.

[0115] Here, in each of the first region R1 and the second region R2, when the imaginary second straight line L2 and the measurement point M do not overlap at two or more locations, the average value of the conversion value for obtaining the "asymmetry of dislocation" may not be calculated. In this case, in each of the first region R1 and the second region R2, the measurement point M closest to the imaginary second straight line L2 and the second closest measurement point M are regarded as measurement points M overlapping the second straight line L2, and the number of dislocations in the measurement points M is measured, so that the average value of the above-mentioned conversion value can be calculated. Furthermore, when the diameter of the III-V compound semiconductor single crystal substrate 100 is 50 mm, the interval I between one measurement point M and the other measurement point M most adjacent to the measurement point M is 5 mm. Therefore, when the diameter of the III-V compound semiconductor single crystal substrate 100 for obtaining the "asymmetry of dislocation" is 50 mm or more, the interval I (pitch) between the measurement points M overlapping the imaginary second straight line L2 must be 5 mm or more.

[0116] <Conductive type>

[0117] The III-V compound semiconductor single crystal substrate of this embodiment can be endowed with electron-withdrawing (n-type) conductivity by adding impurity atoms to the seed crystal as its raw material. That is, the conductivity type of the above-mentioned III-V compound semiconductor single crystal substrate is preferably n-type. In particular, the above-mentioned III-V compound semiconductor single crystal substrate preferably contains tin or sulfur as impurity atoms in the case of an indium phosphide single crystal substrate, and preferably contains silicon in the case of a gallium arsenide single crystal substrate. As a result, in the III-V compound semiconductor single crystal substrate whose conductivity type is n-type, the cracking defect rate during slicing can be reduced.

[0118] For example, an InP substrate can contain both or either S (sulfur) atoms and Sn (tin) atoms to impart n-type conductivity. A conductive InP substrate containing both or either S (sulfur) atoms and Sn (tin) atoms can, for example, have a resistivity of less than 1Ω·cm. A GaAs substrate can contain Si (silicon) atoms to impart n-type conductivity.

[0119] The atomic concentration of the impurity atoms (S, Sn or Si) is preferably 1×10 16 cm -3 Above and 1×10 19 cm -3 The atomic concentration of the impurity atoms is more preferably 1×10 18 cm -3 Above and 1×10 19 cm -3 The atomic concentration of the impurity atoms can be measured by using GDMS (glow discharge mass spectrometry).

[0120] Preferably, the impurity atoms in the III-V compound semiconductor single crystal substrate have a concentration distribution that changes uniformly in the direction from the wave source toward the center of the main surface. Figure 1 In the III-V compound semiconductor single crystal substrate 100 shown as having a pattern (corrugated pattern P) formed by a plurality of continuous arcs having a wave source O on the outside of the main surface S and bending in the same direction, the impurity atoms can show a concentration distribution that changes in the same manner in the direction from the wave source O toward the center of the main surface S. More preferably, the impurity atoms show a concentration distribution that increases in the same manner in the direction from the wave source O toward the center of the main surface S in the III-V compound semiconductor single crystal substrate 100. In this case, when the strain (residual strain) generated in the III-V compound semiconductor single crystal substrate 100 based on the impurity atoms is expressed in polar coordinates with the center of the main surface S as the origin, the residual strain does not show a distribution with n-fold symmetry (where n is an integer greater than 2) centered at the origin, but only shows a distribution with one-fold symmetry (see FIG. 1 ). Figure 3 ), so it is easy to release the stress of the residual strain on the substrate. Therefore, the stress of the residual strain does not need to be released during slicing, so the crack defect rate of the substrate can be reduced.

[0121] Specifically, the concentration distribution of the impurity atoms can be obtained by the following method. First, the III-V compound semiconductor single crystal substrate is cleaved with the (100) plane at each position on the main surface where an imaginary straight line passing through the center of the main surface and extending in the direction from the wave source to the center of the main surface overlaps with the periphery on the wave source side of the center of the main surface, the center of the main surface, and the periphery on the opposite side of the wave source of the center of the main surface. Thus, a measurement sample having a thickness of 300 to 1000 μm and a square surface with a side length of 10 mm is prepared, and the GDMS is performed using the measurement sample. Thus, it is possible to clarify what concentration distribution the impurity atoms show in the III-V compound semiconductor single crystal substrate in the direction from the wave source to the center of the main surface.

[0122] [Method for manufacturing III-V compound semiconductor single crystal substrate]

[0123] The manufacturing method of the III-V compound semiconductor single crystal substrate of the present embodiment is preferably, for example, the following manufacturing method. That is, the manufacturing method is a manufacturing method of a III-V compound semiconductor single crystal substrate using a crystal growth device, comprising: a step (first step) of bringing a seed crystal into contact with a raw material melt and growing a crystal solid on the raw material melt side of the seed crystal to obtain a III-V compound semiconductor single crystal; and a step (second step) of cutting out the III-V compound semiconductor single crystal to obtain a III-V compound semiconductor single crystal substrate having a circular main surface. The crystal growth device has at least a cylindrical crucible and a heating element for heating the crucible. The crucible accommodates the seed crystal at its bottom, and accommodates the raw material melt at a position above the seed crystal in the crucible. The interface between the crystal solid and the raw material melt has an intersection angle of less than 90° relative to the axis of the crucible.

[0124] The present inventors studied the structure of the heating element, etc., as described later, when growing a III-V compound semiconductor single crystal, which is a raw material of a III-V compound semiconductor single crystal substrate, in a crucible of a crystal growth apparatus using the VB method, so that the interface between the crystal solid grown on the raw material melt side of the seed crystal and the raw material melt is not horizontal as in the past, but has an intersection angle of less than 90° with respect to the axis of the crucible. In this case, the present inventors found that the cracking defect rate when obtaining a III-V compound semiconductor single crystal substrate by slicing the III-V compound semiconductor single crystal grown from the crystal is reduced compared with the prior art.

[0125] In this specification, "fracture defect rate" refers to the proportion of fractures of a III-V compound semiconductor single crystal substrate in a series of processes for manufacturing a III-V compound semiconductor single crystal substrate. Specifically, it refers to the proportion of fracture defects such as defects in addition to fractures in a series of processes of growing a III-V compound semiconductor single crystal, grinding the periphery, forming an OF or groove, slicing to a desired thickness, thereby obtaining a III-V compound semiconductor single crystal substrate precursor, and then grinding the periphery of the above-mentioned III-V compound semiconductor single crystal substrate precursor, etching the back and polishing the surface, as well as cleaning and drying to obtain a III-V compound semiconductor single crystal substrate. On the other hand, in this specification, "slicing processing yield rate" refers to the proportion of good III-V compound semiconductor single crystal substrates that do not have the above-mentioned fracture defects.

[0126] Below, by referring to Figure 7, an example of a method for manufacturing a III-V compound semiconductor single crystal substrate of the present embodiment using a so-called VB method using a crucible, such as a vertical Bridgman method and a vertical temperature gradient solidification method included in a vertical boat method, is described. The method for manufacturing a III-V compound semiconductor single crystal substrate of the present embodiment sequentially implements: a seed crystal loading step, a raw material loading step, a sealant configuration step, a crystal growth step as a first step, a cutting step as a second step, and a peripheral grinding step. When implementing the above-mentioned manufacturing method, it is possible to use, for example Figure 7 A crystal growing apparatus is shown having a crucible 1 and a heating element 2 . Figure 7 This is a schematic diagram schematically illustrating a crystal growth apparatus for growing a group III-V compound semiconductor single crystal that is a raw material of a group III-V compound semiconductor single crystal substrate according to the present embodiment.

[0127] In the crystal growth device, the crucible 1 is cylindrical and has a seed crystal holding part and a crystal growth part connected to the seed crystal holding part. The crystal growth part also includes a conical part and a straight part. The seed crystal holding part is a cylindrical area having a cylindrical hollow part, and the cylindrical hollow part is open on the side connected to the crystal growth part and forms a bottom wall on the side opposite to it. The seed crystal holding part can hold a seed crystal 31 in the hollow part. The conical part of the crystal growth part has a conical shape and is connected to the seed crystal holding part on the small diameter side. The straight part has a hollow cylindrical shape and is connected to the large diameter side of the conical part. The crystal growth part of the crucible 1 has the function of holding a solid III-V compound semiconductor raw material inside it. Furthermore, the crystal growth part of the crucible 1 has the following function: by solidifying the raw material melt 33 as a raw material heated to a molten state, a III-V compound semiconductor single crystal as a crystal solid 32 is grown. The crucible 1 can use various materials that can withstand the temperature at which the III-V compound semiconductor raw material melts as its material. For example, it is convenient to use pyrolytic boron nitride (pBN) as the material of the crucible 1. Furthermore, the crystal growth apparatus can include a crucible holding table 4 for holding the crucible 1. As the material of the crucible holding table 4, for example, silicon carbide can be used.

[0128] In the crystal growth device, the heating elements 2 are arranged in a manner that two heating elements surround the outer circumference of the cylindrical crucible 1. Furthermore, each heating element 2 is divided into a plurality of parts in a direction perpendicular to the axis of the crucible, thereby forming a multi-stage structure. As a result, the output power of the heating element 2 can be independently controlled in each heating element and each part. For example, the output power of the heating element 2 can be easily reduced gradually along the axial direction of the crucible 1. Furthermore, by gradually reducing the output power of the heating element 2 along the axial direction of the crucible 1, the interface between the crystal solid grown on the raw material melt side of the seed crystal and the above-mentioned raw material melt can have an intersection angle of less than 90° relative to the axis of the crucible 1. Below, with regard to each step of the above-mentioned manufacturing method, refer to Figure 8 , and the manufacturing methods of InP substrate and GaAs substrate, which are III-V group compound semiconductor single crystal substrates, are described in detail respectively. Figure 8 1 is a flowchart showing an example of a method for manufacturing a III-V compound semiconductor single crystal substrate according to the present embodiment.

[0129] <Method for manufacturing InP substrate>

[0130] (Seed Crystal Loading Step S10)

[0131] In the method for manufacturing an InP substrate, a seed crystal loading step S10 is first performed. In the seed crystal loading step S10, a seed crystal 31 (InP seed crystal) is loaded into the hollow portion of the seed crystal holding portion of the crucible 1. The method for loading the seed crystal 31 into the seed crystal holding portion can use a conventionally known method. Here, with respect to the seed crystal 31, its cross-sectional area is preferably 15% or more, and more preferably 50% or more relative to the cross-sectional area of ​​the straight tube portion of the crucible 1. The average dislocation density of the seed crystal 31 is preferably 5000cm -2 , more preferably 2000cm -2 It is also preferable to add a small amount of impurity atoms (S, Sn) to the seed crystal 31. Furthermore, the inclination angle of the conical portion of the crucible 1 with respect to the straight portion is preferably 40° or less, and more preferably 20° or less.

[0132] (Raw material charging step S20)

[0133] Next, a raw material charging step S20 is performed. In the raw material charging step S20, a plurality of blocks composed of polycrystals (InP polycrystals) of a group III-V compound semiconductor raw material are charged and stacked in the crystal growth part (conical part and straight part) in the crucible 1. Furthermore, in this step, a predetermined amount of impurity atoms (S, Sn) can be added.

[0134] (Sealing Agent Arrangement Step S30)

[0135] Next, a sealing agent disposing step S30 is performed. In the sealing agent disposing step S30, a sealing agent known in the art in the VB method (for example, a solid sealing agent composed of B2O3 (boron oxide)) is disposed on the above-mentioned block.

[0136] (Crystal Growth Step S40: First Step)

[0137] Next, a crystal growth step S40 is implemented as the first step. That is, in the first step, as the crystal growth step S40, in order to obtain a III-V compound semiconductor single crystal (InP single crystal), the seed crystal 31 is brought into contact with the raw material melt 33, and the crystal solid 32 is grown on the raw material melt 33 side of the seed crystal 31. Specifically, a crucible 1 having a seed crystal 31, a block of raw material for the III-V compound semiconductor single crystal, and a solid sealant arranged therein is loaded on the crucible holding table 4 of the crystal growth device. Then, an electric current is supplied to the heating element 2 to heat the crucible 1. As a result, the solid sealant melts to become a liquid sealant 5, and the block of the above-mentioned raw material melts to become the raw material melt 33. Next, a portion of the seed crystal 31 is also melted, and contacts the raw material melt 33 at its interface. Furthermore, by slowly lowering the crucible 1 downward (toward the seed crystal holding portion) along the axis of the crucible relative to the heating element 2, a temperature gradient is formed in the crucible 1 in such a manner that the temperature on the seed crystal 31 side is low and the temperature on the raw material melt 33 side is high, so that the raw material melt 33 in contact with the seed crystal 31 is solidified, and the crystal solid 32 is grown on the raw material melt 33 side of the seed crystal 31. The speed at which the crucible 1 is lowered downward along its axis is preferably 10 mm / hour or less, and more preferably 5 mm / hour or less. Furthermore, when the crucible 1 is lowered downward along its axis, it is preferred that the crucible 1 is rotated at about 5 rpm with its axis as the center.

[0138] Here, two (one group) of heating elements 2 are arranged every half circumference in a manner covering the outer circumference of the crucible 1 as described above. Furthermore, the output power of the heating element 2 is controlled to gradually decrease along the axial direction of the crucible 1. Thus, in the first step, when the crystalline solid 32 is grown on the raw material melt 33 side of the seed crystal 31, the interface 3a between the crystalline solid 32 and the raw material melt 33 is not horizontal, but has an intersection angle of less than 90° relative to the axis of the crucible 1. For example, the interface 3a preferably has an intersection angle of 10 to 70° relative to the axis of the crucible 1.

[0139] In the first step, the crucible 1 is then lowered relative to the heating element 2 along the axis of the crucible, and the non-horizontal interface 3a between the crystalline solid 32 and the raw material melt 33 is raised toward the liquid sealant 5 side, thereby solidifying the raw material melt 33, and the crystalline solid 32 can be grown along the axis of the crucible 1. The growth of the crystalline solid 32 continues until the solidification of the raw material melt 33 remaining in the crystal growth portion of the crucible 1 is completed. In this way, a III-V group compound semiconductor single crystal (InP single crystal) composed of the crystalline solid 32 can be obtained.

[0140] (Cutting Step and Outer Periphery Grinding Step S50: Second Step)

[0141] The cutting step is a step of obtaining a III-V compound semiconductor substrate precursor by cutting out the III-V compound semiconductor crystal (InP single crystal) taken out from the crucible 1. Furthermore, the peripheral grinding step is a step of obtaining a III-V compound semiconductor substrate (InP substrate) having a circular main surface by grinding the periphery of the III-V compound semiconductor substrate precursor. That is, the cutting step and the peripheral grinding step S50 (second step) are steps of slicing the above-mentioned InP single crystal. In the manufacturing method of the InP substrate using the VB method, the cutting step and the peripheral grinding step S50 can be respectively implemented by using the cutting method and the peripheral grinding method known in the past.

[0142] <Method for manufacturing GaAs substrate>

[0143] (Seed Crystal Loading Step S10)

[0144] In the method for manufacturing a GaAs substrate, a seed crystal loading step S10 is first performed. In the seed crystal loading step S10, a seed crystal 31 (GaAs seed crystal) is loaded into the hollow portion of the seed crystal holding portion of the crucible 1. A conventionally known method can be used to load the seed crystal 31 into the seed crystal holding portion.

[0145] (Raw material charging step S20)

[0146] Next, a raw material charging step S20 is performed. In the raw material charging step S20, a plurality of blocks composed of polycrystals (GaAs polycrystals) of a group III-V compound semiconductor raw material are charged and stacked in the crystal growth part (conical part and straight part) in the crucible 1. Furthermore, in this step, a predetermined amount of impurity atoms (Si) can be added.

[0147] (Sealing Agent Arrangement Step S30)

[0148] Next, a sealing agent disposing step S30 is performed. In the sealing agent disposing step S30, a sealing agent known in the art in the VB method (for example, a solid sealing agent composed of B2O3 (boron oxide)) is disposed on the above-mentioned block.

[0149] (Crystal Growth Step S40: First Step)

[0150] Next, a crystal growth step S40 is implemented as the first step. That is, in the first step, as the crystal growth step S40, in order to obtain a III-V compound semiconductor single crystal (GaAs single crystal), the seed crystal 31 is brought into contact with the raw material melt 33, and the crystal solid 32 is grown on the raw material melt 33 side of the seed crystal 31. Specifically, a crucible 1 having a seed crystal 31, a block of raw material for the III-V compound semiconductor single crystal, and a solid sealant arranged therein is loaded on the crucible holding table 4 of the crystal growth device. Then, an electric current is supplied to the heating element 2 to heat the crucible 1. As a result, the solid sealant melts to become a liquid sealant 5, and the block of the above-mentioned raw material melts to become the raw material melt 33. Next, a portion of the seed crystal 31 is also melted, and contacts the raw material melt 33 at its interface. Furthermore, by slowly lowering the crucible 1 downward (toward the seed crystal holding portion) along the axis of the crucible relative to the heating element 2, a temperature gradient is formed in the crucible 1 in such a manner that the temperature on the seed crystal 31 side is low and the temperature on the raw material melt 33 side is high, so that the raw material melt 33 in contact with the seed crystal 31 is solidified, and the crystalline solid 32 is grown on the raw material melt 33 side of the seed crystal 31. The speed at which the crucible 1 is lowered downward along its axis is not particularly limited, and can be, for example, 2 to 10 mm / hour.

[0151] As for the heating element 2, two (a group of) heating elements are arranged every half circumference in a manner covering the outer circumference of the crucible 1 as described above. Furthermore, the output power of the heating element 2 is controlled to gradually decrease along the axial direction of the crucible 1. Thus, in the first step, when the crystalline solid 32 is grown on the raw material melt 33 side of the seed crystal 31, the interface 3a between the crystalline solid 32 and the raw material melt 33 is not horizontal, but has an intersection angle of less than 90° relative to the axis of the crucible 1. For example, the interface 3a preferably has an intersection angle of 10 to 70° relative to the axis of the crucible 1.

[0152] In the first step, the crucible 1 is then lowered relative to the heating element 2 along the axis of the crucible, and the non-horizontal interface 3a between the crystalline solid 32 and the raw material melt 33 is raised toward the liquid sealant 5 side, thereby solidifying the raw material melt 33, and the crystalline solid 32 can be grown along the axis of the crucible 1. The growth of the crystalline solid 32 continues until the solidification of the raw material melt 33 remaining in the crystal growth portion of the crucible 1 is completed. In this way, a III-V group compound semiconductor single crystal (GaAs single crystal) composed of the crystalline solid 32 can be obtained.

[0153] (Cutting Step and Outer Periphery Grinding Step S50: Second Step)

[0154] The cutting step is a step of obtaining a III-V compound semiconductor substrate precursor by cutting out the III-V compound semiconductor crystal (GaAs single crystal) taken out from the crucible 1. Furthermore, the peripheral grinding step is a step of obtaining a III-V compound semiconductor substrate (GaAs substrate) having a circular main surface by grinding the periphery of the III-V compound semiconductor substrate precursor. That is, the cutting step and the peripheral grinding step S50 (second step) are steps of slicing the above-mentioned GaAs single crystal. In the manufacturing method of the GaAs substrate using the VB method, the cutting step and the peripheral grinding step S50 can be respectively implemented by using the cutting method and the peripheral grinding method known in the past.

[0155] <Effects>

[0156] By implementing the above-mentioned steps, a III-V compound semiconductor single crystal substrate having a circular main surface can be manufactured. Regarding the manufacturing method of the III-V compound semiconductor single crystal substrate of the present embodiment, in particular, in the first step, the interface 3a between the crystal solid 32 and the raw material melt 33 is made to have a crossing angle of less than 90° relative to the axis of the crucible 1, so that the crystal solid 32 grows on the raw material melt 33 side of the seed crystal 31. As a result, during the slicing process implemented in the second step, the cracking defect rate of the III-V compound semiconductor single crystal substrate is reduced. Therefore, by the above-mentioned manufacturing method, a III-V compound semiconductor single crystal substrate with a reduced cracking defect rate can be obtained.

[0157] In the above-mentioned manufacturing method, the growth direction of the III-V compound semiconductor single crystal (crystalline solid 32) is preferably the <100> direction. Furthermore, the III-V compound semiconductor single crystal substrate of the present embodiment is preferably obtained by cutting out from the III-V compound semiconductor single crystal with the {100} just plane as the main surface. Furthermore, the III-V compound semiconductor single crystal substrate having an off-angle greater than 0° and less than 15° relative to the {100} plane can be obtained by oblique slicing of the III-V compound semiconductor single crystal with the <100> direction as the growth direction using a conventionally known method.

[0158] Example

[0159] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited thereto. Figure 7The crystal growth apparatus shown uses the VB method to grow a III-V compound semiconductor single crystal in the <100> direction as the growth direction, and obtains an InP substrate (Examples 1 to 8) whose main surface orientation is a (100) just plane and a GaAs substrate (Examples 11 to 17) whose main surface orientation is a plane with an angle of 0 to 15° relative to the (100) plane. On the other hand, in the comparative example described later, a III-V compound semiconductor crystal (InP substrate and GaAs substrate) is grown by using an existing crystal growth apparatus having a heating element configured to cover the entire circumference of the side of the crucible. In each embodiment and comparative example, 1000 InP substrates or GaAs substrates are manufactured respectively.

[0160] <<First Test>>

[0161] [Manufacturing of III-V compound semiconductor single crystal substrate]

[0162] <Example 1: InP substrate>

[0163] (Seed Crystal Loading Step S10)

[0164] A seed crystal 31 made of InP manufactured by a conventionally known method is loaded into the hollow portion of the seed crystal holding portion of the crucible 1 of the crystal growth apparatus by using a conventionally known method. Tin (Sn) is added as an impurity element in a small amount to the seed crystal 31. The cross-sectional area of ​​the seed crystal 31 is 50% of the cross-sectional area of ​​the straight tube portion of the crucible 1. Furthermore, the inclination angle of the conical portion of the crucible 1 relative to the straight tube portion is set to 20°.

[0165] (Raw Material Charging Step S20 and Sealing Agent Disposing Step S30)

[0166] A plurality of blocks made of polycrystalline InP are placed in the crystal growth part of the crucible 1 and stacked. A predetermined amount of tin (Sn) is then added. A solid sealant made of B2O3 is then placed on the raw material of the blocks. The inner diameter of the crystal growth part of the crucible 1 used in this embodiment is 60 mm.

[0167] (Crystal Growth Step S40: First Step)

[0168] Current is supplied to the heating element 2 to heat the crucible 1, thereby turning the solid sealant into the liquid sealant 5 and turning the lumps in the crucible 1 into the raw material melt 33. Furthermore, the lumps located at the interface with the seed crystal 31 also turn into the raw material melt 33, making them contact with a part of the seed crystal 31. Next, the crucible 1 is lowered downward along the axis of the crucible (toward the seed crystal holding portion) relative to the heating element 2, so that the crystalline solid 32 grows on the raw material melt 33 side of the seed crystal 31.

[0169] Here, regarding the heating elements 2, as described above, two heating elements are arranged so as to surround the outer circumference of the cylindrical crucible 1. Furthermore, each heating element 2 is divided into a plurality of parts in a direction perpendicular to the axis of the crucible 1, thereby forming a multi-stage structure. With such a structure, the output power of the heating element 2 is gradually reduced along the axial direction of the crucible 1. Thus, in the first step, the interface 3a between the crystalline solid 32 and the raw material melt 33 has a crossing angle of 30° relative to the axis of the crucible 1.

[0170] Next, the heating element 2 is lowered downward along the axis of the crucible 1, so that the interface 3a between the crystal solid 32 and the raw material melt 33 is raised upward along the axis of the crucible 1, and the crystal solid 32 is grown upward along the axis of the crucible 1. This process is continued until the solidification of the raw material melt 33 remaining in the crystal growth portion of the crucible 1 is completed. According to the above steps, an InP single crystal is manufactured in the crucible 1. Then, the InP single crystal is taken out from the crucible 1 using a conventionally known method.

[0171] (Cutting Step and Outer Periphery Grinding Step S50: Second Step)

[0172] The InP single crystal taken out from the crucible 1 was cut out using a conventionally known cutting method and a peripheral grinding method to obtain an InP substrate precursor, and the peripheral surface of the InP substrate precursor was further ground to produce an InP substrate having a circular main surface. According to the above process, an InP substrate having a diameter of 50 mm and a thickness of 350 μm was obtained as Example 1.

[0173] <Example 2: InP substrate>

[0174] In the seed crystal loading step, a seed crystal 31 to which a small amount of sulfur (S) was added was prepared, and an InP substrate having a diameter of 50 mm and a thickness of 350 μm was obtained by using the same method as in Example 1. In the crystal growth step (first step) of Example 2, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° with respect to the axis of the crucible 1.

[0175] <Example 3: InP substrate>

[0176] The inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 85 mm, and an InP substrate having a diameter of 75 mm and a thickness of 600 μm was obtained by using the same method as in Example 1. In the crystal growth step (first step) of Example 3, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° with respect to the axis of the crucible 1.

[0177] <Example 4: InP substrate>

[0178] The inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 85 mm, and an InP substrate having a diameter of 75 mm and a thickness of 600 μm was obtained by using the same method as in Example 2. In the crystal growth step (first step) of Example 4, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° relative to the axis of the crucible 1.

[0179] <Example 5: InP substrate>

[0180] The inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 110 mm, and an InP substrate having a diameter of 100 mm and a thickness of 625 μm was obtained by using the same method as in Example 1. In the crystal growth step (first step) of Example 5, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° relative to the axis of the crucible 1.

[0181] <Example 6: InP substrate>

[0182] The inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 110 mm, and an InP substrate having a diameter of 100 mm and a thickness of 625 μm was obtained by using the same method as in Example 2. In the crystal growth step (first step) of Example 6, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° relative to the axis of the crucible 1.

[0183] <Example 7: InP substrate>

[0184] The inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 160 mm, and an InP substrate having a diameter of 150 mm and a thickness of 675 μm was obtained by using the same method as in Example 1. In the crystal growth step (first step) of Example 7, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° relative to the axis of the crucible 1.

[0185] <Example 8: InP substrate>

[0186] The inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 160 mm, and an InP substrate having a diameter of 150 mm and a thickness of 675 μm was obtained by using the same method as in Example 2. In the crystal growth step (first step) of Example 8, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° relative to the axis of the crucible 1.

[0187] <Comparative Example 1: InP substrate>

[0188] By using an existing crystal growth device, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 in the crystal growth process (first process) has a crossing angle of 90° (i.e., horizontal) relative to the axis of the crucible 1. In addition, by using the same method as in Example 1, an InP substrate with a diameter of 50 mm and a thickness of 350 μm is obtained.

[0189] <Comparative Example 2: InP substrate>

[0190] By using an existing crystal growth device, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 in the crystal growth process (first process) has a crossing angle of 90° (i.e., horizontal) relative to the axis of the crucible 1. In addition, by using the same method as in Example 2, an InP substrate with a diameter of 50 mm and a thickness of 350 μm is obtained.

[0191] <Comparative Example 3: InP substrate>

[0192] By using the same method as in Comparative Example 1 except that the inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was 85 mm, an InP substrate having a diameter of 75 mm and a thickness of 600 μm was obtained.

[0193] <Comparative Example 4: InP substrate>

[0194] By using the same method as in Comparative Example 2 except that the inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was 85 mm, an InP substrate having a diameter of 75 mm and a thickness of 600 μm was obtained.

[0195] <Comparative Example 5: InP substrate>

[0196] By using the same method as in Comparative Example 1 except that the inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was 110 mm, an InP substrate having a diameter of 100 mm and a thickness of 625 μm was obtained.

[0197] <Comparative Example 6: InP substrate>

[0198] By using the same method as in Comparative Example 2 except that the inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was 110 mm, an InP substrate having a diameter of 100 mm and a thickness of 625 μm was obtained.

[0199] <Comparative Example 7: InP substrate>

[0200] By using the same method as in Comparative Example 1 except that the inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was 160 mm, an InP substrate having a diameter of 150 mm and a thickness of 675 μm was obtained.

[0201] <Comparative Example 8: InP substrate>

[0202] By using the same method as in Comparative Example 2 except that the inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was 160 mm, an InP substrate having a diameter of 150 mm and a thickness of 675 μm was obtained.

[0203] <Example 11: GaAs substrate>

[0204] (Seed Crystal Loading Step S10)

[0205] A seed crystal 31 made of GaAs produced by a conventionally known method is placed in a hollow portion of a seed crystal holding portion of a crucible 1 provided in a crystal growth apparatus by using a conventionally known method. A small amount of silicon (Si) is added to the seed crystal 31 as an impurity element.

[0206] (Raw Material Charging Step S20 and Sealing Agent Disposing Step S30)

[0207] A plurality of blocks made of polycrystalline GaAs are placed in the crystal growth part of the crucible 1 and stacked. A predetermined amount of Si is then added. A solid sealant made of B2O3 is then placed on the raw material of the blocks. The inner diameter of the crystal growth part of the crucible 1 used in this embodiment is 80 mm.

[0208] (Crystal Growth Step S40: First Step)

[0209] Current is supplied to the heating element 2 to heat the crucible 1, thereby turning the solid sealant into the liquid sealant 5 and turning the lumps in the crucible 1 into the raw material melt 33. Furthermore, the lumps located at the interface with the seed crystal 31 also turn into the raw material melt 33, making them contact with a part of the seed crystal 31. Next, the crucible 1 is lowered downward along the axis of the crucible (toward the seed crystal holding portion) relative to the heating element 2, so that the crystalline solid 32 grows on the raw material melt 33 side of the seed crystal 31.

[0210] Here, regarding the heating elements 2, as described above, two heating elements are arranged so as to surround the outer circumference of the cylindrical crucible 1. Furthermore, each heating element 2 is divided into a plurality of parts in a direction perpendicular to the axis of the crucible 1, thereby forming a multi-stage structure. With such a structure, the output power of the heating element 2 is gradually reduced along the axial direction of the crucible 1. Thus, in the first step, the interface 3a between the crystalline solid 32 and the raw material melt 33 has a crossing angle of 30° relative to the axis of the crucible 1.

[0211] Next, the heating element 2 is lowered downward along the axis of the crucible 1, so that the interface 3a between the crystal solid 32 and the raw material melt 33 is raised upward along the axis of the crucible 1, and the crystal solid 32 is grown upward along the axis of the crucible 1. This process is continued until the solidification of the raw material melt 33 remaining in the crystal growth part of the crucible 1 is completed. According to the above steps, a GaAs single crystal is manufactured in the crucible 1. Then, the GaAs single crystal is taken out from the crucible 1 using a conventionally known method.

[0212] (Cutting Step and Outer Periphery Grinding Step S50: Second Step)

[0213] Using a conventionally known cutting method and a peripheral grinding method, the GaAs anti-crystal taken out from the crucible 1 is cut out using a known slicing method in a manner such that the main surface is a surface having a (100) just plane, thereby obtaining a GaAs substrate precursor, and then the periphery of the GaAs substrate precursor is ground to thereby manufacture a GaAs substrate having a circular main surface. According to the above process, a GaAs substrate having a diameter of 75 mm and a thickness of 600 μm is obtained as Example 11.

[0214] <Example 12: GaAs substrate>

[0215] In the cutting step and the peripheral grinding step (second step), the GaAs single crystal taken out from the crucible 1 was cut in such a way that the main surface was a plane having an off-angle of 10° relative to the (100) plane, thereby obtaining a GaAs substrate precursor, and a GaAs substrate having a diameter of 75 mm and a thickness of 600 μm was obtained by using the same method as in Example 11. In the crystal growth step (first step) of Example 12, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° relative to the axis of the crucible 1.

[0216] <Example 13: GaAs substrate>

[0217] A GaAs substrate having a diameter of 100 mm and a thickness of 625 μm was obtained by using the same method as in Example 11, except that the inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 110 mm. In the crystal growth step (first step) of Example 13, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° with respect to the axis of the crucible 1.

[0218] <Example 14: GaAs substrate>

[0219] The inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 160 mm, and in the cutting step and the peripheral grinding step S50, the GaAs single crystal taken out from the crucible 1 was cut in such a way that the main surface was a plane having an angle of 2° relative to the (100) plane, and a GaAs substrate having a diameter of 150 mm and a thickness of 760 μm was obtained by using the same method as in Example 11. In the crystal growth step (first step) of Example 14, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° relative to the axis of the crucible 1.

[0220] <Example 15: GaAs substrate>

[0221] The inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 160 mm, and in the cutting step and the peripheral grinding step S50, the GaAs single crystal taken out from the crucible 1 was cut in such a way that the main surface was a plane having an angle of 6° relative to the (100) plane, and a GaAs substrate having a diameter of 150 mm and a thickness of 760 μm was obtained by using the same method as in Example 11. In the crystal growth step (first step) of Example 15, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° relative to the axis of the crucible 1.

[0222] <Example 16: GaAs substrate>

[0223] The inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 160 mm, and in the cutting step and the peripheral grinding step S50, the GaAs single crystal taken out from the crucible 1 was cut so that the main surface was a plane having an angle of 15° relative to the (100) plane, and a GaAs substrate having a diameter of 150 mm and a thickness of 760 μm was obtained by using the same method as in Example 11. In the crystal growth step (first step) of Example 16, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° relative to the axis of the crucible 1.

[0224] <Example 17: GaAs substrate>

[0225] The inner diameter of the crystal growth portion in the crucible 1 of the crystal growth apparatus was set to 210 mm, and in the cutting step and the peripheral grinding step S50, the GaAs single crystal taken out from the crucible 1 was cut in such a way that the main surface was a plane having an angle of 6° relative to the (100) plane, and a GaAs substrate having a diameter of 200 mm and a thickness of 675 μm was obtained by using the same method as in Example 11. In the crystal growth step (first step) of Example 17, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 had a crossing angle of 30° relative to the axis of the crucible 1.

[0226] <Comparative Example 11: GaAs substrate>

[0227] By using an existing crystal growth device, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 in the crystal growth process (first process) has a crossing angle of 90° (i.e., horizontal) relative to the axis of the crucible 1. In addition, by using the same method as Example 11, a GaAs substrate with a diameter of 75 mm and a thickness of 600 μm is obtained.

[0228] <Comparative Example 12: GaAs substrate>

[0229] By using an existing crystal growth device, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 in the crystal growth process (first process) has a crossing angle of 90° (i.e., horizontal) relative to the axis of the crucible 1. In addition, by using the same method as Example 12, a GaAs substrate with a diameter of 75 mm and a thickness of 600 μm is obtained.

[0230] <Comparative Example 13: GaAs substrate>

[0231] By using an existing crystal growth device, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 in the crystal growth process (first process) has a crossing angle of 90° (i.e., horizontal) relative to the axis of the crucible 1. In addition, by using the same method as Example 13, a GaAs substrate with a diameter of 100 mm and a thickness of 625 μm is obtained.

[0232] <Comparative Example 14: GaAs substrate>

[0233] By using an existing crystal growth device, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 in the crystal growth process (first process) has a crossing angle of 90° (i.e., horizontal) relative to the axis of the crucible 1. In addition, by using the same method as Example 14, a GaAs substrate with a diameter of 150 mm and a thickness of 760 μm is obtained.

[0234] <Comparative Example 15: GaAs substrate>

[0235] By using an existing crystal growth device, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 in the crystal growth process (first process) has a crossing angle of 90° (i.e., horizontal) relative to the axis of the crucible 1. In addition, by using the same method as Example 15, a GaAs substrate with a diameter of 150 mm and a thickness of 760 μm is obtained.

[0236] <Comparative Example 16: GaAs substrate>

[0237] By using an existing crystal growth device, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 in the crystal growth process (first process) has a crossing angle of 90° (i.e., horizontal) relative to the axis of the crucible 1. In addition, by using the same method as Example 16, a GaAs substrate with a diameter of 150 mm and a thickness of 760 μm is obtained.

[0238] <Comparative Example 17: GaAs substrate>

[0239] By using an existing crystal growth device, the interface 3a between the crystal solid 32 grown in the crucible 1 and the raw material melt 33 in the crystal growth process (first process) has a crossing angle of 90° (i.e., horizontal) relative to the axis of the crucible 1. In addition, by using the same method as Example 17, a GaAs substrate with a diameter of 200 mm and a thickness of 675 μm is obtained.

[0240] [Evaluation of III-V compound semiconductor single crystals]

[0241] For the III-V compound semiconductor single crystal substrates of Examples 1 to 8, Examples 11 to 17, Comparative Examples 1 to 8, and Comparative Examples 11 to 17, the average concentration of impurity atoms in the substrate, the dislocation density of the main surface, and the asymmetry of the dislocations present on the main surface were determined by the above method. Furthermore, the average value of the residual strain and the distribution form of the residual strain in polar coordinates (whether it is n-fold symmetric, and whether it is mirror symmetric (including the case of approximately mirror symmetric)) were determined by the above method, and whether the wave source of the corrugated pattern observed on the main surface is located on the above main surface was also determined by the above method. The results are shown in Tables 1 to 4.

[0242] Furthermore, when 1000 III-V compound semiconductor single crystal substrates of Examples 1 to 8, Examples 11 to 17, Comparative Examples 1 to 8, and Comparative Examples 11 to 17 were manufactured, the ratio of good III-V compound semiconductor single crystal substrates without cracks, defects, etc. was obtained as the "slicing yield". The results are also shown in Tables 1 to 4. The "slicing yield" in Tables 1 to 4 was evaluated as good when 90% or more, and was evaluated as poor when less than 90%.

[0243] [Table 1]

[0244]

[0245] [Table 2]

[0246]

[0247] [Table 3]

[0248]

[0249] [Table 4]

[0250]

[0251] [Investigation]

[0252] According to Tables 1 to 4, the wave source of the corrugated pattern formed on the main surface of each III-V compound semiconductor single crystal substrate of Examples 1 to 8 and Examples 11 to 17 is not located on the above-mentioned main surface, and the "slicing process yield rate" is 90% or more, which can be evaluated as good. On the other hand, for each III-V compound semiconductor single crystal substrate of Comparative Examples 1 to 8 and Comparative Examples 11 to 17, the wave source of the corrugated pattern formed on the main surface is located on the above-mentioned main surface, and the "slicing process yield rate" is less than 90%, which cannot be evaluated as good.

[0253] <<Second Test>>

[0254] For the III-V compound semiconductor single crystal substrates (InP substrates) of Examples 4 and 6, and Comparative Examples 4 and 6, the concentration distribution of impurity atoms (S) on the main surface was measured by the above method. The results are shown in Table 5. In Table 5, the impurity atom (S) concentration indicated in the item "wave source side" refers to the concentration measured in the measurement sample obtained from the following position, which is a position on the main surface where an imaginary straight line extending from the wave source to the center of the main surface overlaps with the periphery on the wave source side of the center of the main surface. The impurity atom (S) concentration indicated in the item "center" refers to the concentration measured in the measurement sample obtained from the center of the main surface, and the impurity atom (S) concentration indicated in the item "ripple spread side" refers to the concentration measured in the measurement sample obtained from the following position, which is a position on the main surface where an imaginary straight line extending from the wave source to the center of the main surface overlaps with the periphery on the opposite side of the wave source than the center of the main surface.

[0255] [Table 5]

[0256] Table 5

[0257] Impurity atom (S) concentration Wave source side center Corrugated spread side Example 4 (3 inches) <![CDATA[2.9×10 18 ]]> <![CDATA[3.0×10 18 ]]> <![CDATA[3.1×10 18 ]]> Example 6 (4 inches) <![CDATA[2.8×10 18 ]]> <![CDATA[3.0×10 18 ]]> <![CDATA[3.2×10 18 ]]> Comparative Example 4 (3 inches) <![CDATA[3.0×10 18 ]]> <![CDATA[3.0×10 18 ]]> <![CDATA[3.0×10 18 ]]> Comparative Example 6 (4 inches) <![CDATA[3.1×10 18 ]]> <![CDATA[3.0×10 18 ]]> <![CDATA[3.1×10 18 ]]>

[0258] [Investigation]

[0259] According to Table 5, the impurity atoms present in the InP substrates of Examples 4 and 6 increase uniformly along the direction from the wave source to the center of the above-mentioned main surface, that is, from the "wave source side" to the "wave spreading side", and thus show a concentration distribution with a higher concentration on the "wave spreading side" than on the "wave source side". On the other hand, the impurity atoms present in the InP substrates of Comparative Examples 4 and 6 show a distribution with the same concentration on the "wave source side" and the "wave spreading side".

[0260] <<The Third Test>>

[0261] For the III-V compound semiconductor single crystal substrates (GaAs substrates) of Example 13 and Example 15, and Comparative Example 13 and Comparative Example 15, the concentration distribution of impurity atoms (Si) on the main surface was measured by the above method. The results are shown in Table 6. In Table 6, the impurity atom (Si) concentration indicated in the item "wave source side" refers to the concentration measured in the measurement sample obtained from the following position, which is a position on the main surface where an imaginary straight line extending from the wave source to the center of the main surface overlaps with the outer periphery on the wave source side of the center of the main surface. The impurity atom (Si) concentration indicated in the item "center" refers to the concentration measured in the measurement sample obtained from the center of the main surface, and the impurity atom (Si) concentration indicated in the item "ripple spread side" refers to the concentration measured in the measurement sample obtained from the following position, which is a position on the main surface where an imaginary straight line extending from the wave source to the center of the main surface overlaps with the outer periphery on the opposite side of the above wave source than the center of the main surface.

[0262] [Table 6]

[0263] Table 6

[0264] Impurity Atom (Si) Concentration Wave source side center Corrugated spread side Example 13 (4 inches) <![CDATA[1.7×10 18 ]]> <![CDATA[1.8×10 18 ]]> <![CDATA[1.9×10 18 ]]> Example 15 (6 inches) <![CDATA[1.6×10 18 ]]> <![CDATA[1.8×10 18 ]]> <![CDATA[2.0×10 18 ]]> Comparative Example 13 (4 inches) <![CDATA[1.9×10 18 ]]> <![CDATA[1.8×10 18 ]]> <![CDATA[1.9×10 18 ]]> Comparative Example 15 (6 inches) <![CDATA[2.0×10 18 ]]> <![CDATA[1.8×10 18 ]]> <![CDATA[2.0×10 18 ]]>

[0265] [Investigation]

[0266] According to Table 6, the impurity atoms present in the GaAs substrates of Examples 13 and 15 increase uniformly along the direction from the wave source to the center of the above-mentioned main surface, that is, from the "wave source side" to the "wave spread side", and thus show a concentration distribution with a higher concentration on the "wave spread side" than on the "wave source side". On the other hand, the impurity atoms present in the GaAs substrates of Comparative Examples 13 and 15 show a distribution with the same concentration on the "wave source side" and the "wave spread side".

[0267] Although the embodiments and examples of the present invention have been described above, it has been planned from the beginning to combine the above-described embodiments and examples as appropriate.

[0268] The embodiments and examples disclosed this time should be considered as illustrative in all aspects and not restrictive. The scope of the present invention is indicated by the claims rather than the embodiments and examples described above, and is intended to include all modifications within the meaning and scope equivalent to the claims.

[0269] Description of Reference Numerals

[0270] O wave source, P corrugated pattern, S main surface, 100 III-V group compound semiconductor single crystal substrate, 101 III-V group compound semiconductor single crystal substrate (existing), I interval, M measuring point, L1 imaginary first straight line, L2 imaginary second straight line, R1 first region, R2 second region, OF positioning edge, 1 crucible, 2 heating element, 3a interface, 31 seed crystal, 32 crystal solid, 33 raw material melt, 3a interface, 4 crucible holding table, 5 liquid sealant, S10 seed crystal loading process, S20 raw material loading process, S30 sealant configuration process, S40 crystal growth process, S50 cutting process and peripheral grinding process.

Claims

1. A III-V compound semiconductor single crystal substrate having a circular main surface, The III-V compound semiconductor single crystal substrate is an indium phosphide single crystal substrate, The indium phosphide single crystal substrate has a corrugated pattern observed on the main surface by performing the following treatment, The wavy pattern is a pattern corresponding to a portion of ripples extending concentrically from a wave source. The wave source is not located on the main surface, Treatment: The main surface is horizontally arranged at a position 10 mm downward in the depth direction from the liquid surface of a mixed liquid at 25°C, and the main surface is irradiated with light from a 500 W reflective incandescent lamp for more than 1 hour and less than 2 hours from a position 20 cm upward from the liquid surface. The mixed liquid is composed of 10 g of chromium (VI) oxide, 10 mL of 50 mass % concentration hydrofluoric acid solution and 400 mL of pure water.

2. The III-V compound semiconductor single crystal substrate according to claim 1, wherein: The diameter of the indium phosphide single crystal substrate is greater than or equal to 50 mm and less than or equal to 155 mm.

3. The III-V compound semiconductor single crystal substrate according to claim 1 or claim 2, wherein: The dislocation density of the main surface is 0 cm -2 Above and 2000cm -2 the following.

4. The III-V compound semiconductor single crystal substrate according to any one of claims 1 to 3, wherein The asymmetry of the dislocations present in the main surface is 1.8 or more, The asymmetry is calculated as follows: The main surface is divided into a first area and a second area by an imaginary first straight line, the imaginary first straight line perpendicularly intersecting an imaginary straight line extending in a direction from the wave source to the center of the main surface and passing through the center of the main surface, In the first area and the second area, two or more lines with a length of 1 mm are set at intervals of 5 mm or more in a direction away from the center of the main surface on an imaginary second straight line that passes through the center of the main surface and intersects the first straight line at right angles. 2 The number of dislocations is measured at the measuring point, and the number of dislocations is converted into per 1 cm based on the measurement result. 2 The converted value of area, The average value of the converted values ​​obtained based on all the measuring points in the second area is subtracted from the average value of the converted values ​​obtained based on all the measuring points in the first area, and the absolute value of the resulting value is divided by the average value of the converted values ​​obtained based on all the measuring points in the first area and the second area.

5. A III-V compound semiconductor single crystal substrate having a circular main surface, The III-V compound semiconductor single crystal substrate is a gallium arsenide single crystal substrate, The gallium arsenide single crystal substrate has a corrugated pattern observed on the main surface by performing the following treatment, The wavy pattern is a pattern corresponding to a portion of ripples extending concentrically from a wave source. The wave source is not located on the main surface, Treatment: The main surface is horizontally arranged at a position 10 mm downward in the depth direction from the liquid surface of a mixed liquid at 25°C, and the main surface is irradiated with light from a 500 W reflective incandescent lamp for more than 5 minutes and less than 20 minutes from a position 20 cm upward from the liquid surface. The mixed liquid is composed of 10 g of chromium (VI) oxide, 10 mL of 50 mass % concentration hydrofluoric acid solution and 400 mL of pure water.

6. The III-V compound semiconductor single crystal substrate according to claim 5, wherein: The diameter of the gallium arsenide single crystal substrate is greater than or equal to 75 mm and less than or equal to 205 mm.

7. The III-V compound semiconductor single crystal substrate according to claim 5 or claim 6, wherein: The dislocation density of the main surface is 0 cm -2 Over and 50cm -2 the following.

8. The III-V compound semiconductor single crystal substrate according to any one of claims 5 to 7, wherein The asymmetry of the dislocations present in the main surface is 2.0 or more, The asymmetry is calculated as follows: The main surface is divided into a first area and a second area by an imaginary first straight line, the imaginary first straight line perpendicularly intersecting an imaginary straight line extending in a direction from the wave source to the center of the main surface and passing through the center of the main surface, In the first area and the second area, two or more lines with a length of 1 mm are set at intervals of 5 mm or more in a direction away from the center of the main surface on an imaginary second straight line that passes through the center of the main surface and intersects the first straight line at right angles. 2 The number of dislocations is measured at the measuring point, and the number of dislocations is converted into per 1 cm based on the measurement result. 2 The converted value of area, The average value of the converted values ​​obtained based on all the measuring points in the second area is subtracted from the average value of the converted values ​​obtained based on all the measuring points in the first area, and the absolute value of the resulting value is divided by the average value of the converted values ​​obtained based on all the measuring points in the first area and the second area.

9. The III-V compound semiconductor single crystal substrate according to any one of claims 1 to 8, wherein The main surface is a plane having an off angle of 0° or more and 15° or less with respect to a {100} plane.

10. The III-V compound semiconductor single crystal substrate according to any one of claims 1 to 9, wherein The absolute value of the difference between the tensile strain in the radial direction and the tensile strain in the tangential direction of the main surface, i.e., the average value of the residual strain, is 3.5×10 -5 the following.

11. The III-V compound semiconductor single crystal substrate according to any one of claims 1 to 10, wherein In polar coordinates with the center of the main surface as the origin and an imaginary line segment extending from the center of the main surface toward the wave source to a point 15 mm long from the periphery of the III-V compound semiconductor single crystal substrate as the polar axis, the absolute value of the difference between the radial tensile strain and the tangential tensile strain of the main surface, i.e., the residual strain, does not have an n-fold symmetric distribution centered on the origin, where n is an integer greater than 2.

12. The III-V compound semiconductor single crystal substrate according to any one of claims 1 to 11, wherein The conductivity type of the III-V group compound semiconductor single crystal substrate is electron-withdrawing type.

13. The III-V compound semiconductor single crystal substrate according to any one of claims 1 to 12, wherein The III-V compound semiconductor single crystal substrate contains tin or sulfur as an impurity atom in the case of the indium phosphide single crystal substrate, The III-V compound semiconductor single crystal substrate contains silicon as an impurity atom in the case of the gallium arsenide single crystal substrate.

14. The III-V compound semiconductor single crystal substrate according to claim 13, wherein: The atomic concentration of the impurity atoms is 1×10 16 cm -3 Above and 1×10 19 cm -3 the following.

15. The III-V compound semiconductor single crystal substrate according to claim 13 or claim 14, wherein: The impurity atoms show a concentration distribution that changes uniformly in the direction from the wave source toward the center of the main surface in the III-V compound semiconductor single crystal substrate.

16. A method for manufacturing a III-V compound semiconductor single crystal substrate, comprising: using a crystal growth device to manufacture a III-V compound semiconductor single crystal substrate; The manufacturing method comprises: A step of bringing a seed crystal into contact with a raw material melt and growing a crystal solid on the raw material melt side of the seed crystal to obtain a III-V compound semiconductor single crystal; as well as a step of obtaining a III-V compound semiconductor single crystal substrate having a circular main surface by cutting out the III-V compound semiconductor single crystal; The crystal growth device at least comprises a cylindrical crucible and a heating element for heating the crucible. The crucible contains the seed crystal at its bottom, and contains the raw material melt at a position above the seed crystal in the crucible. An interface between the crystalline solid and the raw material melt has an intersection angle of less than 90° with respect to the axis of the crucible.