Method for improving etch rate and improving feature critical size and mask selectivity

By applying non-sine continuous wave voltage and dual-voltage pulse sequence on the electrostatic chuck, adjusting the voltage and frequency of the plasma sheath, the problem of insufficient ion energy and angular spread control in inductively coupled plasma etching technology is solved, and the etching is improved The consistency of rate and feature size improves the quality of semiconductor equipment manufacturing.

CN119054042APending Publication Date: 2024-11-29LAM RES CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035394.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-25
Filing Date
2023-04-06
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing inductively coupled plasma etching technology has shortcomings in controlling ion energy and angular spread, resulting in inconsistency between etching rate and characteristic size, affecting the manufacturing quality of semiconductor equipment.

Method used

By applying a non-sine continuous wave voltage (NSCWV) signal on the electrostatic chuck, the voltage and frequency of the plasma sheath are adjusted to control ion energy distribution and angular spread, combined with a dual voltage pulse sequence, etching parameters are optimized to improve etching rate and Feature accuracy.

Benefits of technology

It effectively improves the consistency of etching rate and feature size, reduces mask damage, and improves the quality and accuracy of semiconductor equipment manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119054042A_ABST
    Figure CN119054042A_ABST
Patent Text Reader

Abstract

A method of generating a voltage pulse includes generating a first non-sinusoidal continuous wave voltage (NSCWV) waveform for a first duration of a clock cycle. The first NSCWV signal includes a first base voltage and a first frequency. The method further includes performing a first transition to change from the first NSCWV signal to the second NSCWV signal. A second NSCWV signal is generated for a second duration of the clock cycle. The second NSCWV signal includes a second base voltage and a second frequency. The method further includes performing a second transition to transition from the second NSCWV signal back to the first NSCWV signal. The first transition and the second transition are repeated within a clock cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Priority claim

[0001] This application is a continuation of U.S. patent application No. 63 / 363,558, filed on April 25, 2022, entitled “METHOD TO ENHANCE ETCH RATE AND IMPROVE CRITICAL DIMENSION OF FEATURES AND MASK SELECTIVITY,” and claims the benefit of priority. The entire contents of the U.S. patent application are incorporated by reference. Background Art

[0002] Etching and deposition processes are an integral part of modern semiconductor processing. Although various plasma processing techniques can be used, inductively coupled plasma provides advantageous features, such as a way to control ion energy and ion angular spread. Controlling ion energy and ion angular spread can provide many advantages for etching and deposition processes based on inductively coupled plasma. Ion behavior can be controlled by changing parameters that affect the bulk plasma properties and by changing electrical parameters (e.g., bias voltage) on an electrostatic chuck. Of these two control methods, methods for changing electrical parameters on an electrostatic chuck are continually being developed to address various problems in semiconductor device manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0003] The materials described herein are provided as examples only and are not intended to limit the drawings in any way. For simplicity and clarity of description, the elements shown in the drawings are not necessarily drawn to scale. For example, for clarity, the sizes of some elements are exaggerated compared to the sizes of other elements. In addition, for clarity of discussion, various physical features can be presented in their simplified "ideal" form and geometric features, but it should not be understood that the actual situation can only be close to the ideal type shown. For example, smooth surfaces and square intersections can be drawn without considering the limited roughness, rounded corners and non-ideal corner intersections of the structure formed by nanofabrication technology. In addition, where deemed appropriate, the figure marks are repeated in the drawings to indicate corresponding or similar elements.

[0004] Figure 1 A schematic diagram of an apparatus according to at least one embodiment of the present disclosure is shown, comprising an electrostatic chuck coupled to a non-sinusoidal continuous wave voltage source.

[0005] Figure 2 The relationship between ion temperature, electric field, and angular spread in the sheath region of a plasma according to at least one embodiment of the present disclosure is shown.

[0006] Figure 3A graph showing a voltage generated by a non-sinusoidal continuous wave voltage (NSCWV) source, wherein the voltage level varies between a first level and a second level, according to at least one embodiment of the present disclosure.

[0007] Figure 4 According to at least one embodiment of the present disclosure, Figure 3 A diagram of the first portion of the voltage produced by a non-sinusoidal continuous wave voltage source.

[0008] Figure 5 According to at least one embodiment of the present disclosure, Figure 3 FIG. 1 is a diagram of the second portion of the voltage produced by a non-sinusoidal continuous wave voltage source.

[0009] Figure 6 According to at least one embodiment of the present disclosure, Figure 3 A graph of a portion of the applied voltage generated by a non-sinusoidal continuous wave voltage source in FIG. 1 overlaid with a graph of the induced voltage generated on the substrate surface.

[0010] Figure 7 A flow chart of a method for increasing ion energy and reducing mask erosion in a patterned substrate placed in an inductively coupled plasma processing tool is shown in accordance with at least one embodiment of the present disclosure.

[0011] Fig. 8A A cross-sectional view of a mask formed over a substrate according to at least one embodiment of the present disclosure is shown.

[0012] Figure 8B A cross-sectional view of a groove profile of a high aspect ratio groove formed in a substrate according to at least one embodiment of the present disclosure is shown.

[0013] Figures 9A to 9D A graph of ion energy distribution functions in a plasma sheath resulting from single and dual voltage level discharges produced by a non-sinusoidal continuous wave voltage source is shown in accordance with at least one embodiment of the present disclosure.

[0014] Figures 10A to 10D is a cross-sectional view of a simulation of a groove formed in a silicon substrate corresponding to different voltage bias conditions on an electrostatic chuck according to at least one embodiment of the present disclosure.

[0015] Figures 11A to 11D is a cross-sectional view of simulated mask profiles corresponding to different voltage bias conditions on an electrostatic chuck after a process of etching recesses according to at least one embodiment of the present disclosure.

[0016] Fig.12A processor system having a machine-readable storage medium having instructions that, when executed, cause a processor to control a scaling of ion energies is shown in accordance with at least one embodiment of the present disclosure. DETAILED DESCRIPTION

[0017] A method for increasing etch rates and improving critical dimensions and mask selectivity of features in an inductively coupled plasma is described. Throughout this document, numerous specific details, such as structural schemes, are set forth to provide a thorough understanding of at least one embodiment. It will be apparent to one skilled in the art that at least one embodiment may be practiced without these specific details. In other instances, well-known features, such as radio frequency sources, are not described in detail to avoid unnecessarily obscuring at least one embodiment. Furthermore, it should be understood that at least one embodiment shown in the figures is an illustrative representation and is not necessarily drawn to scale.

[0018] In some cases, well-known methods and devices are represented in the form of block diagrams rather than in the form of details to avoid obscuring at least one embodiment. Reference to "an embodiment" or "some embodiments" or "one embodiment" or "at least one embodiment" throughout this specification refers to the specific features, structures, functions or characteristics described in conjunction with the embodiments being included in at least one embodiment. Therefore, the phrases "in one embodiment" or "in one embodiment" or "at least one embodiment" or "some embodiments" appearing in various places in this specification do not necessarily refer to the same embodiment. In addition, specific features, structures, functions or characteristics can be combined in any suitable manner in at least one embodiment. For example, the first embodiment can be combined with the second embodiment anywhere where the specific features, structures, functions or characteristics associated with the first embodiment and the second embodiment are not mutually exclusive.

[0019] In this article, "coupling" and "connection" together with their derivatives can be used to describe the functional or structural relationship between parts in this article. These terms are not intended to be synonymous with each other. Relatively speaking, in a particular embodiment, "connection" can be used to refer to two or more elements directly physically, optically or electrically contacting each other. "Coupling" can be used to refer to two or more elements directly or indirectly (with other intermediate elements therebetween) physically, electrically or magnetically contacting each other, and / or two or more elements co-operate or act on each other (e.g., in a causal relationship).

[0020] Here, "above," "below," "between," and "on" as used herein refer to the relative position of one component or material with respect to other components or materials, where such physical relationship is noted. Unless these terms are modified by "directly" or "directly," one or more intervening components or materials may be present. Similar distinctions will apply in the case of an assembly of components. As used throughout the specification and claims, a list of items linked with "at least one" or "one or more" may mean any combination of the listed terms.

[0021] As used herein, "adjacent" generally refers to a position where one thing is immediately adjacent to (eg, next to or close to, with one or more things in between) or next to (eg, adjacent to) another thing.

[0022] Unless otherwise expressly specified when used, the terms "substantially equal", "about equal" and "approximately equal" generally mean that there is no accidental variation between the two things described. In at least one embodiment, such variation does not exceed + / -10% of the reference value.

[0023] Plasma etching is essential to modern semiconductor device manufacturing. "Plasma etching" herein generally refers to a process of removing material from a surface by charged particles and / or reactive species generated by a plasma. In at least one embodiment, during the manufacture of semiconductor devices, plasma can be used to etch masked materials and maskless structures. In at least one embodiment, etching the masked material includes forming a photoresist mask over the material and using a pattern in the mask to selectively etch the underlying material relative to the mask. In at least one embodiment, etching the maskless structure includes selectively removing some or all of the material formed in a pocket relative to the surrounding material, or forming a spacer on the sidewall of a gate electrode in a transistor.

[0024] There are various types of tools that generate and maintain plasma, which are called plasma etching processing tools. "Plasma etching processing tool" herein generally refers to a device that uses plasma to generate ions and reactive species to etch materials. "Plasma" herein generally refers to a collection of electrically neutral ionized gases. In at least one embodiment, the plasma etching processing tool can generate plasma by transformer action, electron cyclotron resonance, or capacitive methods. In at least one embodiment, a wafer including the material to be etched is transferred to an electrostatic chuck contained in a plasma processing chamber or plasma chamber under vacuum conditions. In this article, "wafer" generally refers to a conductive or insulating substrate, and includes one or more materials in dielectrics, insulation, metals or semiconductors. In this article, "electrostatic chuck" generally refers to a support structure that utilizes electrostatic clamping between the uppermost surface of the wafer and the chuck.

[0025] In at least one embodiment, a gas mixture flows into the chamber and a plasma is started by one of the methods described above. In at least one embodiment, a plasma is formed near a wafer placed on an electrostatic chuck. In at least one embodiment, energetic electrons generated after ignition of the plasma generate reactive free radical species and ions by dissociation of a gas mixture (referred to as a feedstock gas). In at least one embodiment, the plasma used for processing is weakly ionized because the density of ions and electrons is a fractional portion of the neutral atoms in the plasma. In at least one embodiment, the plasma is quasi neutral, where the electron density is approximately equal to the ion density. In at least one embodiment, of the ions and electrons generated in the plasma, electrons are more mobile and escape from the edge of the plasma to the chamber walls and wafer surface. Electron losses at the edge of the plasma result in the formation of a plasma sheath at the edge. As used herein, "plasma sheath or sheath" may generally refer to an area of ​​net positive charge density at the edge of the plasma.

[0026] In at least one embodiment, the plasma can have three regions: a bulk region, where the potential can be positive but small, such as less than 50V; and a pre-sheath region, between the bulk and sheath regions. In at least one embodiment, the plasma potential at the pre-sheath / sheath boundary is close to zero and drops to negative values ​​near the wall or wafer surface. In at least one embodiment, the sheath region acts as a potential hill for electrons and a potential valley for ions. In at least one embodiment, ions enter the sheath at the sheath / pre-sheath boundary at a speed that is defined by the ion temperature in the bulk plasma. In at least one embodiment, the ions are accelerated toward the wafer surface, which is at a lower potential relative to the sheath / pre-sheath boundary.

[0027] In at least one embodiment, ions striking a wafer surface are used in a treatment plasma to etch feature profiles in semiconductors, dielectrics, and conductive materials that may be deposited on the wafer surface. In at least one embodiment, understanding and controlling the ion energy at the wafer surface facilitates precise control of the process for etching various features used to manufacture semiconductor devices. In at least one embodiment, a relatively thin sheath (e.g., less than 10 mm) and a low pressure discharge (e.g., less than 0.1 Pa) result in a collisionless sheath that can be used to reduce the ion angular spread at the wafer surface. In at least one embodiment, a collisionless sheath is one in which the sheath thickness is significantly less than the ion mean free path in the sheath. In this context, "ion angular spread" may generally refer to the spread of angles that ions of a given energy have at the wafer surface. In at least one embodiment, ions that pass through the plasma sheath on the way to the wafer surface have an ion energy distribution that may be small but not zero. In this context, "ion energy distribution" may generally refer to the distribution of ions that arrive at the wafer surface after leaving the plasma.

[0028] The ion energy distribution may arise from oscillations in the plasma and from oscillations of the sheath potential and is affected by the frequency of the oscillations. In at least one embodiment, the ion energy distribution may be adjusted by applying an externally driven, time-varying voltage at the electrostatic chuck.

[0029] In at least one embodiment, inductively coupled plasma can provide advantages over plasmas produced by other methods because the ion energy at the wafer surface can be controlled independently of the ion temperature in the plasma. In this article, "inductively coupled plasma" generally refers to a plasma generated and maintained by a transformer action outside the chamber. In at least one embodiment, the plasma potential and ion temperature are directly controlled by power, which is transmitted through the transformer action. In at least one embodiment, the ion temperature can be controlled by transformer coupling of an induced electric field in an etching chamber. In this article, "etching chamber" generally refers to a chamber where plasma is generated and plasma etching is performed on a wafer. In at least one embodiment, the induced electric field helps to excite and maintain the plasma and control global parameters, such as electron and ion temperature, density, etc. The plasma etching and deposition system includes an electrostatic chuck. In this article, "electrostatic chuck" generally refers to a support structure in the etching chamber on which a wafer or substrate for processing is placed. In at least one embodiment, the wafer contacts the plasma sheath at the edge of the plasma boundary during processing. In at least one embodiment, the ions leave the sheath with an expansion of ion energy and ion angular spread. In at least one embodiment, the ion energy is controlled by the bulk plasma potential, but may also be controlled by a biased electrostatic chuck.

[0030] In at least one embodiment, the electrostatic chuck includes a conductive electrode and an insulator layer on the conductive electrode, and the substrate is generally placed on the insulator layer. In at least one embodiment, the electrostatic chuck is generally voltage biased by a radio frequency (RF) voltage waveform to induce an RF voltage on the wafer. In at least one embodiment, the RF voltage induced on the wafer overcomes the capacitive effect of the insulator. In at least one embodiment, the RF voltage waveform is adjusted to overcome the steady rise in potential at the wafer due to a steady ion flux. In at least one embodiment, the RF biased electrostatic chuck can also change the sheath voltage. In at least one embodiment, the sheath of a low-pressure discharge (usually an inductively coupled plasma) can generally be considered to be collision-free and relatively narrow (e.g., on the order of a few millimeters). For example, when the bias voltage approaches the kV level, in the dielectric chamber, the sheath may collide. In at least one embodiment, the plasma potential in the body can also be considered to have a low level of voltage fluctuations.

[0031] In at least one embodiment, the ion energy, and more precisely, the ion energy distribution at the wafer depends on (a) the time-varying flux of ions entering the sheath, and (b) the time-varying sheath voltage. If (b) is more dominant, the voltage oscillation in the sheath may be mainly caused by the frequency of the RF voltage waveform that biases the electrostatic chuck. In at least one embodiment, the response of the ions to the RF voltage waveform affects the etching characteristics on the wafer surface. In at least one embodiment, in addition to the voltage amplitude, the oscillation frequency can also be used to affect the etching characteristics. In at least one embodiment, the voltage amplitude and the oscillation frequency can shape the ion energy distribution and the ion angular spread at the wafer surface. The former can control the etching rate, and the latter can affect the shape of different features of the etching. In at least one embodiment, the ions pass through the sheath in a limited time period. In at least one embodiment, this is determined by the initial ion velocity and the sheath thickness, wherein the initial ion velocity is determined by the ion temperature when the ions enter the sheath. In at least one embodiment, the sheath thickness also varies with the oscillation voltage amplitude and the oscillation frequency. In at least one embodiment, the ion energy distribution is highly dependent on the timescale of the voltage amplitude change.

[0032] In at least one embodiment, programming the time-varying voltage amplitude within the sheath region can advantageously provide a path to reduce the angular spread of ions leaving the plasma. In at least one embodiment, reducing the angular spread can positively affect etching parameters, such as etching anisotropy or the degree of vertical etching relative to lateral etching. In at least one embodiment, reducing the angular spread of ions is useful for anisotropic etching of high aspect ratio features during semiconductor device manufacturing. The aspect ratio is defined as the ratio of the depth of the feature to the width. In at least one embodiment, the high aspect ratio (e.g., aspect ratio greater than 20:1) feature includes a groove. In at least one embodiment, the groove can have a width ranging between 10nm and 20nm, and a depth of at least 200nm. In at least one embodiment, obtaining substantially vertical sidewalls in the groove can advantageously provide a structure to manufacture a capacitor with enhanced electrical characteristics, or to manufacture source and drain isolation regions in a transistor.

[0033] In at least one embodiment, the ion angular spread at the wafer surface can be proportional to the square root of the ion temperature in the bulk plasma and to the sheath voltage V s In at least one embodiment, one method of reducing the angular spread of the ions may be to increase the bias power on the electrostatic chuck. Increasing the bias voltage results in an increase in V s In at least one embodiment, a pulsed DC voltage waveform can be used to reduce the ion energy distribution to improve etching characteristics, such as uniformity and anisotropy. In at least one embodiment, the pulsed DC voltage signal is a non-sinusoidal continuous wave voltage (NSCWV) signal. In this article, "non-sinusoidal continuous wave voltage" generally refers to a continuous electrical pulse that has a periodicity, but the amplitude is characterized by a non-monotonic increase or decrease shape.

[0034] In at least one embodiment, the NSCWV signal has a frequency range, for example, between 100 kHz and 400 KHz. In at least one embodiment, a low frequency signal (e.g., less than 400 KHz) ensures that it is not blocked by the capacitance of an insulator layer present between the wafer and an electrostatic chuck electrode (e.g., an electrostatic chuck). In at least one embodiment, the amplitude of the NSCWV signal can also be adjusted to provide an effective voltage that overcomes the increase in ion current on the wafer during operation. In at least one embodiment, the NSCWV signal is different from a common RF waveform. In at least one embodiment, the RF waveform has a defined oscillation frequency and oscillation peak amplitude. In at least one embodiment, the NSCWV signal can include a plurality of voltage ramps, as will be discussed below.

[0035] Reducing the spread of ion energy without reducing the absolute voltage level in the NCSWV waveform may not be beneficial. As ions continue to bombard the wafer surface, the mask used to pattern the grooves may be eroded even with the ion energy distribution. Simply reducing the absolute voltage level can slow the etch rate, but this may also potentially reduce the etch anisotropy, such as becoming more isotropic.

[0036] In at least one embodiment, the NCSWV waveform has been superimposed with a high frequency RF bias to provide a combined voltage pulse to the electrostatic chuck. In at least one embodiment, the high frequency RF bias has a frequency greater than, for example, 1 MHz. In at least one embodiment, above 1 MHz, ions passing through the sheath may experience many cycles of voltage oscillations so that the ions respond to the time-averaged sheath voltage. In at least one embodiment, the amplitude of the time-averaged sheath voltage depends on the amplitude of the applied voltage bias. In at least one embodiment, the time-averaged sheath voltage corresponding to the high frequency RF bias may not have the same effect as the NCSWV waveform. In at least one embodiment, the high frequency RF bias modulates the ion energy distribution in the sheath to have a larger ion energy distribution. But the ions in the NCSW sheath may have a very narrow energy spread. In at least one embodiment, the NCSWV waveform applied alone can be advantageously used for etching.

[0037] In at least one embodiment, using the NSCWV signal, the ion distribution can be tightened, and thus the etching anisotropy can be controlled. But in order to also reduce mask damage, according to at least one embodiment, a dual voltage pulse sequence can be implemented. In at least one embodiment, the dual voltage pulse sequence includes changing the voltage level between two voltage levels. In at least one embodiment, a higher voltage level can be used to reduce the ion energy distribution, increase anisotropy, and maintain the etching rate. In at least one embodiment, by reducing continuous high energy ion bombardment, a lower voltage can be used to give the mask relaxation time. In at least one embodiment, the higher voltage level can be part of a first voltage envelope that lasts for a first finite duration. In at least one embodiment, the higher voltage level can be measured relative to a first reference voltage.

[0038] In at least one embodiment, a higher voltage level is obtained during a first portion of the first pulse train within a first voltage envelope. In at least one embodiment, additional features of the first pulse train include a second portion (which includes a gradually gradient voltage phase) and a third portion (which is at a first reference voltage). In at least one embodiment, the first and second portions of the first pulse train can have a greater duty cycle than the third portion. In at least one embodiment, the first portion of the first pulse train is designed to reduce the ion angular spread. In at least one embodiment, the gradient voltage phase can be designed to offset the increase in ion current at the wafer substrate. In this document, "duty cycle" generally refers to the ratio of the time that the NSCWV signal is at a first defined voltage level to the time that the NSCWV signal is at a second defined voltage level. In at least one embodiment, the first voltage can be finite, both positive or negative, and the second voltage can be finite, both positive, negative, or zero.

[0039] In at least one embodiment, the lower voltage level can be part of a second voltage envelope that lasts for a second finite duration. In at least one embodiment, the lower voltage level can be measured relative to a second reference voltage. In at least one embodiment, within the second voltage envelope, the lower voltage level can be obtained during a first portion of the second pulse train. In at least one embodiment, additional features of the second pulse train include a second portion (which includes a gradually tapering voltage phase) and a third portion (which is at a second reference voltage). In at least one embodiment, the first and second portions of the second pulse train can have a greater duty cycle than the third portion. In at least one embodiment, the first portion of the second pulse train can be designed to reduce ion bombardment to provide some respite for the mask. In at least one embodiment, the tapering voltage phase can be designed to offset an increase in ion current at the wafer substrate.

[0040] In at least one embodiment, the dual voltage pulse train can have a duty cycle that favors the first voltage envelope relative to the second voltage envelope. In at least one embodiment, the first reference level and the second reference level can be at the same level or at different levels. In at least one embodiment, the difference between the higher voltage level and the first reference voltage can be greater than the difference between the lower voltage level and the second reference voltage.

[0041] Although the NCSWV waveform has been described with respect to implementation in an inductively coupled plasma, it may generally be implemented in other plasma processing tools as well, according to at least one embodiment.

[0042] Figure 1A schematic diagram of a plasma processing tool 100 is shown according to at least one embodiment. In at least one embodiment, the plasma processing tool 100 is an example of an inductively coupled etch tool that includes an electrostatic chuck 102 within a process chamber 104 and an RF generator 106 coupled to a coil above the process chamber 104. In at least one embodiment, the plasma processing tool 100 may also include a non-sinusoidal continuous wave voltage (NSCWV) generator 108 coupled in series with the electrostatic chuck 102.

[0043] In at least one embodiment, the electrostatic chuck 102 includes an electrode plate 102A coupled to the NSCWV generator 108, and an insulator 102B on the electrode plate 102A. In at least one embodiment, the insulator 102B may include a dielectric material, including alloys and ceramics, such as aluminum oxide (Al2O3), silicon dioxide (SiO2), silicon nitride (Si3N4), and sapphire.

[0044] In at least one embodiment, the NSCWV generator 108 can be configured to generate a pulsed voltage waveform 110 at the electrostatic chuck 102. In at least one embodiment, the NSCWV generator 108 can generate a peak voltage of up to 100 kV. In at least one embodiment, the NSCWV generator 108 can be configured to generate a voltage in the range of 2 kV to 10 kV. In at least one embodiment, the NSCWV generator 108 can generate voltage pulses in the range of 50 kHz to 500 kHz.

[0045] In at least one embodiment, during operation, a plasma 112 can be generated within the processing chamber 104. In at least one embodiment, ions are ejected from a plasma sheath, which is the outermost portion of the plasma 112, which can be near the insulator 102B. In at least one embodiment, the plasma sheath can be a non-neutral region formed at the plasma boundary to balance electron and ion losses to maintain quasi-neutrality. In at least one embodiment, the ions impact a substrate 114 placed on the electrostatic chuck 102 and perform various etches (e.g., chemical, mechanical, etc.) on one or more materials within the substrate 114.

[0046] In at least one embodiment, the characteristics (e.g., velocity and angular distribution) of ions within the sheath region of the plasma 112 can depend on (a) the plasma potential and (b) the potential at the surface of the substrate 114, which can be controlled by the voltage applied to the electrostatic chuck 102. In at least one embodiment, the velocity of the ions can be directly affected by both (a) and (b) because an increase in both (a) and (b) increases the electric field, which drives the ions toward the electrostatic chuck 102. In at least one embodiment, the electric field in the bulk of the plasma can be very small (e.g., 10 V / cm or less), but the field in the sheath region (e.g., adjacent to the substrate 114) can be between 1 KV / cm.

[0047] In at least one embodiment, when the pulsed voltage waveform 110 can be applied to the electrostatic chuck by the NSCWV generator 108, the plasma sheath oscillates in response to the pulsed voltage waveform 110. In at least one embodiment, the application of the pulsed voltage waveform 110 changes the width (and potential) of the sheath. In at least one embodiment, the change in sheath width or sheath-presheath boundary relative to the substrate 114 can be defined by the rapid oscillation of the sheath width at the boundary in response to the frequency of the pulsed voltage waveform 110. In at least one embodiment, because the mobility of ions is significantly lower than that of electrons, the ions respond slowly and respond in a time averaged over the frequency of the pulsed voltage waveform 110. In at least one embodiment, the slower response may result in a spread of ion energies, or alternatively may result in a distribution of ion energies. In at least one embodiment, the oscillations in the sheath may be caused by the induced electric field in the bulk plasma driving the plasma oscillations, as well as the pulsed voltage waveform 110 applied to the electrostatic chuck 102. In at least one embodiment, to affect the ion distribution in an inductively coupled plasma system, the pulsed voltage waveform 110 plays a substantially dominant role in the effects due to the voltage oscillations. In at least one embodiment, the form of the pulsed voltage waveform 110 and the effect on the etched features and mask within the substrate 114 are described in detail below.

[0048] According to at least one embodiment, Figure 2 The relationship between the temperature of ions in the plasma 112, the voltage applied to the sheath 202A, and the angular spread is shown in graph 200 in FIG. In at least one embodiment, the plasma 202 includes a sheath 202A and a pre-sheath 202B adjacent to the sheath 202A. In at least one embodiment, the voltage at the boundary 203 between the sheath 202A and the pre-sheath 202B is relative to the voltage V supplied to the surface of the substrate 114. s A net electric field E is generated in the sheath 202A. In at least one embodiment, the voltage V sThe thickness D of the sheath 202A is also determined. In at least one embodiment, the electric field E is a function of the power that is coupled to sustain the plasma 112 and raises the potential of the plasma to a level that is used to sustain the plasma. In at least one embodiment, the electric field E is directed toward the electrostatic chuck 102. In at least one embodiment, the electric field E is caused by T i The transverse component of the ion velocity is generated by the random motion of the ions in the plasma. In at least one embodiment, the lateral component of the ion velocity is generated by the random motion of the ions in the plasma. i The ion velocity and the V s The vector sum of the velocities provides the maximum ion angular spread, σθ.

[0049] In at least one embodiment, Figure 2 The relationship between the ion temperature, the voltage supplied to the ions within the sheath, and the angular spread of the ion velocity is shown by Equation 1.1:

[0050] Sigma θ = Tan -1 [Square root (T i / eV s )], (1.1) where sigma θ is the angular spread, T i is the ion temperature, and V s is the sheath voltage of the plasma sheath of the plasma 112 in the processing chamber 104 ( Figure 1 ).

[0051] In at least one embodiment, the angular spread θ of ions accelerated toward the electrostatic chuck 102 is directly affected by T i 、V s In at least one embodiment, the voltage V s is set by the pulse voltage applied to the electrostatic chuck 102. In at least one embodiment, it is highly desirable to not increase T i In the case of increasing V s In at least one embodiment, the ion energy and ion angular spread are controlled by coupling from the RF generator 106 ( Figure 1 ) determines the plasma potential and hence T i .

[0052] Figure 3 The NSCWV generator 108 ( Figure 1) is a schematic diagram of a pulse voltage waveform 300 generated by a clock signal. In at least one embodiment, generating the pulse voltage waveform 300 includes generating a NSCWV signal 302 within a first duration T1 of a clock cycle. The NSCWV signal 302 includes a first base voltage V1 and a frequency f1. In at least one embodiment, as shown, although T1 includes three pulses, the number of pulses is arbitrary.

[0053] In at least one embodiment, generating the pulsed voltage waveform 300 further includes performing a transition including changing from generating the NSCWV signal 302 to generating the NSCWV signal 304. In at least one embodiment, the NSCWV signal 304 is generated for a duration T2 of the clock cycle. In at least one embodiment, the NSCWV signal 304 includes a second base voltage V2 and a frequency f2. As shown, although T2 includes three pulses, the number of pulses is arbitrary.

[0054] In at least one embodiment, generating the pulse voltage waveform 300 further includes performing a second transition, including changing from the NSCWV signal 304 back to the NSCWV signal 302. In at least one embodiment, the first transition and the second transition are repeated within a clock cycle. In this document, a "clock cycle" can generally refer to the total time period of the duration of the pulse voltage waveform 300. In at least one embodiment, the pulse voltage waveform 300 can be an example of a level-to-level voltage pulse by transitioning between V1 and V2.

[0055] In at least one embodiment, for the purpose of controlling ion energy and distribution, V1 and a first reference voltage V R1 The difference between V2 and the second reference voltage V R2 The difference between |V1-V R1 |Sum and difference|V2-V R2 | is useful. In at least one embodiment, V R1 and V R2 Can be different. In at least one embodiment, V R1 With V R2 In at least one embodiment, the main feature of the pulse voltage waveform 300 is |V1-V R1 |Greater than|V2-V R2 |.

[0056] In at least one embodiment, |V1-V R1 | and |V2-V R2 The difference between | is directly reflected in the difference in ion energy distribution and the subsequent Figure 1 ) in the etching of features.

[0057] In at least one embodiment, the inverse of the sum of the first duration T1 and the second duration T2 defines the duty cycle of the pulse voltage waveform 300. In at least one embodiment, the duty cycle of the NSCWV signal 302 is between at least 50% and 75%. In at least one embodiment, T2 can be less than T1. In at least one embodiment, T2 can be greater than T1. In at least one embodiment, the duty cycle of the NSCWV signal 302 determines how long the plasma discharge will be used to produce the high etch rate phase and the lower etch rate phase.

[0058] In at least one embodiment, the sum of the first duration and the second duration, ie, T1+T2, defines the pulse frequency f of the pulse voltage waveform 300. p In at least one embodiment, f p Between 1 Hz and 100 kHz. In at least one embodiment, f p Cannot be less than f1 and f2.

[0059] Figure 4 A graph 400 is shown of an actual applied first NSCWV signal 302 according to at least one embodiment. In at least one embodiment, in conjunction with Figure 1 The NSCWV generator 108 described above may be used to generate the NSCWV signal 302. In at least one embodiment, referring again to Figure 4 Applying or generating the NSCWV signal 302 includes performing a first operation, the first operation including increasing the voltage from the first reference voltage V within a first time interval T3. R1 to the voltage level of the first base voltage V1. In at least one embodiment, V R1 is a "zero level". In at least one embodiment, V R1 It may be a positive voltage level. In at least one embodiment, the first time interval T3 may be quasi-instantaneous.

[0060] In at least one embodiment, a second operation is performed in which the magnitude of the voltage level increases from the first base voltage V to the second base voltage V within the second time interval T4. l The NSCWV signal 302 is configured to gradually change to a first peak voltage V3. In at least one embodiment, the amplitude of V3 is greater than the amplitude of V1. In at least one embodiment, the amplitude of V3 is between 25% and 50% greater than the amplitude of V1. In at least one embodiment, each harmonic is an integer multiple of a fundamental frequency, such as 400 kHz. In at least one embodiment, the NSCWV signal 302 includes up to (and including) the tenth harmonic (e.g., 4000 kHz). In at least one embodiment, the gradual decrease from V1 to V3 includes low frequency oscillations from 400 kHz to 4000 kHz due to the superposition of different harmonics.

[0061] In at least one embodiment, generating the NSCWV signal 302 further includes performing a third operation including reducing the voltage level from the first peak voltage V3 to the reference voltage V within a third time interval T5. R1 In at least one embodiment, the magnitude of V3 is greater than V R In at least one embodiment, T5 can be quasi-instantaneous.

[0062] In at least one embodiment, generating the NSCWV signal 302 further includes performing a fourth operation, including maintaining the voltage level at the reference voltage V during a fourth time interval T6. R1 In at least one embodiment, the voltage overshoots to a positive voltage.

[0063] In at least one embodiment, the first operation, the second operation, the third operation, and the fourth operation constitute a single cycle of the NSCWV signal 302 and are repeated for a first duration T1.

[0064] In at least one embodiment, the NSCWV signal 302 has a frequency f1 that is equal to 1 divided by the sum of the first time interval T3, the second time interval T4, the third time interval T5, and the fourth time interval T6. In at least one embodiment, the frequency f1 may be less than 100 KHz. In at least one embodiment, the ratio between the second time interval T4 and the fourth time interval T6 is greater than or equal to 2:1. In at least one embodiment, the ratio between the second time interval T4 and the fourth time interval T6 is equal to 3:1. In at least one embodiment, the NSCWV signal 302 has a duty cycle in which the non-zero negative voltage portion (below V R1 ) is greater than 50 and less than 100. In at least one embodiment, the NSCWV signal 302 has a duty cycle of 75%. In at least one embodiment, the second time interval T4 is at least 100 times greater than the first time interval T3 or the third time interval T5.

[0065] Figure 5 Graph 500 shows an actual applied NSCWV signal 304 according to at least one embodiment. In at least one embodiment, in conjunction with Figure 1 The NSCWV generator 108 described above may be used to generate the NSCWV signal 304. Referring again to Figure 5 In at least one embodiment, applying or generating the NSCWV signal 304 includes performing a fifth operation, including increasing the amplitude of the voltage level from the second reference voltage V to the second reference voltage V within the first time interval T7. R2 Increase to the first base voltage V2. In at least one embodiment, V R2 is a "zero level". In at least one embodiment, V R2 Can be a positive voltage level. V R2 Can be used with VR1 Same or Different ( Figure 4 ). In at least one embodiment, the first time interval T7 can be quasi-instantaneous.

[0066] In at least one embodiment, a second operation is performed in which the amplitude of the voltage level is gradually changed from the first base voltage V2 to the first peak voltage V4 within a second time interval T8. In at least one embodiment, the amplitude of V4 is greater than the amplitude of V2, as shown. In at least one embodiment, the amplitude of V4 is between 25% and 50% greater than the amplitude of V2. In at least one embodiment, each harmonic is an integer multiple of a fundamental frequency such as 400kHz. In at least one embodiment, the NSCWV signal 304 includes up to and including the tenth harmonic (e.g., 4000kHz). In at least one embodiment, the gradual decrease from V2 to V4 includes low frequency oscillations from 400kHz to 4000kHz due to the superposition between different harmonics.

[0067] In at least one embodiment, generating the NSCWV signal 304 further includes performing a third operation including reducing the voltage level from the first peak voltage V4 to the second reference voltage V within a third time interval T9. R2 In at least one embodiment, the magnitude of V4 is greater than V R2 In at least one embodiment, the third time interval T9 may be quasi-instantaneous. In at least one embodiment, the second time interval T8 is at least 100 times greater than the first time interval T7 or the third time interval T9.

[0068] In at least one embodiment, generating the NSCWV signal 304 further includes performing a fourth operation including performing, during a fourth time interval T 10 The voltage level is maintained at the reference voltage V R2 In at least one embodiment, the voltage overshoots to a positive voltage.

[0069] In at least one embodiment, the first operation, the second operation, the third operation, and the fourth operation constitute a single cycle of the NSCWV signal 304 and are repeated within a first duration T1.

[0070] In at least one embodiment, the NSCWV signal 304 has a frequency f1 that is equal to 1 divided by the first time interval T7, the second time interval T8, the third time interval T9, and the fourth time interval T 10 In at least one embodiment, the frequency is less than 100 KHz. In at least one embodiment, the second time interval T8 and the fourth time interval T 10 The ratio between the second time interval T8 and the fourth time interval T is greater than or equal to 2:1. 10=The ratio between is equal to 3:1. In at least one embodiment, the NSCWV signal 304 has a duty cycle in which the non-zero negative voltage portion (below V R2 ) is greater than 50 and less than 100. In at least one embodiment, the NSCWV signal 304 has a duty cycle of 75%. In at least one embodiment, the second time interval T8 is at least 100 times greater than the first time interval T7 or the third time interval T9. In at least one embodiment, T7 is comparable to T3 ( Figure 4 ), and T9 is equivalent to T5 ( Figure 4 ).

[0071] In at least one embodiment, frequency f2 may not be equal to frequency f1. In at least one embodiment, f2 may be greater than, equal to, or less than f1, depending on the embodiment. In at least one embodiment, T8 may be comparable to T4, or may not be comparable to T4 ( Figure 4 ), and T 10 May or may not be equivalent to T6 ( Figure 4 ). In at least one embodiment, the ratio between T4:T8 can be at least 1:1. In at least one embodiment, the ratio between T4:T8 is 3:1.

[0072] In at least one embodiment, the voltage peaks V2 and V3 may be equal or unequal. In at least one embodiment, V3 may have a greater amplitude than V4, or vice versa. In at least one embodiment, the gradual change from V1 to V3 may correspond to a voltage slope selected to compensate for the linear voltage increase across the blocking capacitance due to the positive ion bombardment. Figure 1 In at least one embodiment, the blocking capacitor is Figure 1 The blocking capacitor 102A is not shown, but may be located between the NSCWV generator 108 and the electrostatic chuck 102. In at least one embodiment, the blocking capacitor may be the insulator 102B between the electrode plate 102A and the substrate 114.

[0073] Figure 6 A substrate (eg Figure 3 600 of an induced voltage waveform 602 on the surface of a substrate 114 in the sheath. In at least one embodiment, the induced voltage waveform 602 is a combination of the NSCWV signal 302 and the ions leaving the sheath 202A that impact the surface of the substrate 114. Figure 2) induced voltage waveform 602 has a substantially constant average voltage and oscillations 604 during time interval T4. In at least one embodiment, oscillations 604 are caused by a 400kHz to 4000kHz signal generated by the NSCWV generator and by the superposition of the above-mentioned different harmonics. In at least one embodiment, the NSCWV signal 302 generated by the NSCWV generator is superimposed for comparison. In at least one embodiment, the gradual change from V1 to V3 corresponds to a voltage slope that is selected to compensate for the linear voltage increase due to the positive ions bombarding the electrostatic chuck 102 ( Figure 1 ) accumulated charge.

[0074] Figure 7 A method 700 for changing ion energy and ion angular spread directed toward a substrate surface during an etching operation according to at least one embodiment is shown. In at least one embodiment, some or all of the operations of method 700 may be performed or controlled by hardware, software, or a combination thereof. In at least one embodiment, method 700 begins at operation 710 by placing a substrate on an electrostatic chuck within a plasma chamber. In at least one embodiment, the electrostatic chuck is electrically coupled to a NSCWV generator. In at least one embodiment, method 700 continues to operation 720 by forming a plasma within the plasma chamber, wherein the plasma generates a sheath having a first sheath voltage. In at least one embodiment, method 700 continues to operation 730 by changing the first sheath voltage to a second sheath voltage by applying a first NSCWV signal at the electrostatic chuck. In at least one embodiment, the first NSCWV signal includes a first periodic function and generates a first voltage response on a wafer substrate. In at least one embodiment, the first voltage response achieves a first change in the spread of ion energy at the wafer due to the change from the first sheath voltage to the second sheath voltage. In at least one embodiment, as the sheath voltage increases from a first sheath voltage to a second sheath voltage, the ion energy increases. In at least one embodiment, the ion energy distribution decreases and a high etch rate plasma is generated.

[0075] In at least one embodiment, the method 700 ends at operation 740 by changing the second sheath voltage to a third sheath voltage by applying a second NSCWV signal at the electrostatic chuck. In at least one embodiment, the second non-sinusoidal voltage waveform includes a second periodic function and produces a second voltage response on the wafer substrate. In at least one embodiment, the second voltage response causes a second change in the spread of ion energy at the wafer due to the change from the second sheath voltage to the third sheath voltage. In at least one embodiment, as the sheath voltage decreases, the ion energy decreases. In at least one embodiment, the ion energy distribution decreases and a low etch rate plasma is generated.

[0076] In at least one embodiment, again referring to Figure 4 , the pulse voltage waveform 300 is applied to the electrostatic chuck 102 ( Figure 1 ). In at least one embodiment, a first sheath voltage is generated at the plasma boundary at the wafer surface immediately upon plasma generation. In at least one embodiment, a first non-sinusoidal voltage waveform, such as NSCWV signal 302, is applied at the electrostatic chuck. In at least one embodiment, this generates a voltage response on the wafer substrate that results in a first change in the spread of ion energy at the wafer. In at least one embodiment, the second sheath voltage is averaged over time period T3+T4.

[0077] Reference Figure 5 In at least one embodiment, a pulse voltage waveform 300 is applied to the electrostatic chuck 102 ( Figure 1 ). In at least one embodiment, the non-sinusoidal voltage waveform changes from the first periodic function to a second periodic non-sinusoidal voltage waveform, such as NSCWV signal 304. In at least one embodiment, the lower amplitude base voltage V2 in NSCWV signal 304 produces a voltage response on the wafer that results in a second change in the spread of ion energy at the wafer. In at least one embodiment, compared to V1 ( Figure 4 ), the lower amplitude V2 reduces the ion energy distribution and reduces the etching rate, but does not stop the etching process. In at least one embodiment, the third sheath voltage is averaged over the time period T7+T8.

[0078] In at least one embodiment, in combination Figure 3 The pulsed voltage waveform 300 is described as being applied to an electrostatic chuck to etch features having a high aspect ratio that is selective to a mask formed on a wafer that is placed in the electrostatic chuck.

[0079] Fig. 8A is a cross-sectional view of a patterned wafer 800 according to at least one embodiment. In at least one embodiment, patterned wafer 800 includes a substrate 802 and a mask 804 formed on substrate 802. In at least one embodiment, substrate 802 may include a single layer or multiple layers. In at least one embodiment, substrate 802 includes silicon, germanium, III-V group, sapphire, or quartz. In at least one embodiment, substrate 802 includes a dielectric formed on a silicon-containing material. In at least one embodiment, mask 804 includes a photoresist material patterned by a photolithography process. In at least one embodiment, mask 804 includes a dielectric material that has been patterned by a previous photolithography process and a subsequent etching process. In at least one embodiment, mask 804 has a thickness T M1In at least one embodiment, the integrity of the mask 804 is maintained during etching. In at least one embodiment, erosion near the mask edge 805, in particular, and the extent of isotropic erosion may result in flares in the sidewalls of the mask 804. In at least one embodiment, depending on the erosion rate of the mask 804 compared to the target etch depth, the upper portion of the substrate 802 may be adversely eroded. In at least one embodiment, it is desirable to balance the control of ion energy, ion energy distribution, and directionality to pattern features with high fidelity.

[0080] Figure 8B According to at least one embodiment Fig. 8A , after a process of plasma etching and forming a groove in substrate 802. In at least one embodiment, different waveforms can be generated by the NSCWV generator when etching substrate 802. In at least one embodiment, the waveform has the same Figure 3 As shown (by NSCWV generator 108 ( Figure 1 ) generates the NSCWV signals 302 and 304 in the pulse voltage waveform 300 having the same or substantially the same characteristics to etch the substrate 802.

[0081] In at least one embodiment, the groove 806 has substantially vertical sidewalls 802A. In at least one embodiment, the substantially vertical sidewalls can enable a device to be manufactured with substantially uniform electrical properties. In at least one embodiment, the mask 804 is eroded substantially uniformly to a new thickness T M2 , where T M2 Less than T M1 In at least one embodiment, a balance between high energy etching and low energy mask preservation operations can be achieved to form recess 806 .

[0082] Figures 9A to 9D A simulation of the ion angular spread and ion energy distribution at the wafer surface during processing in an ICP plasma with different voltages applied on the electrostatic chuck according to at least one embodiment is shown. The vertical axis corresponds to the energy of the ions and the horizontal axis corresponds to the ion angular spread (θ), measured in degrees.

[0083] Fig.9A Graph 900 shows the angular spread of ions resulting from an applied voltage of 330 V generated by an RF generator. In at least one embodiment, the RF generator generates a sinusoidal voltage. In at least one embodiment, the sinusoidal voltage has a peak voltage V B In at least one embodiment, the sinusoidal voltage may be offset relative to a reference voltage. In at least one embodiment, the peak voltage of one voltage polarity will have an amplitude of |V B |+|Vshift |, and the magnitude of the peak voltage of opposite polarity will be |V B |-|V shift In at least one embodiment, for a peak ion energy of 550 eV, the ion angular spread E A1 is about 3.32 degrees. In at least one embodiment, the sinusoidal bias voltage V b Produces peak energy of 1.6 to 1.8 Vb eV.

[0084] Fig. 9B A non-sinusoidal continuous wave voltage generator (e.g. Figure 1 910 is a graph of the ion angular spread resulting from an applied voltage of 330 V generated by the NCSWV generator 108 in FIG. 910. In at least one embodiment, for a peak applied voltage of 330 V, the ion angular spread E A2 is about 8.1 degrees. In at least one embodiment, the non-sinusoidal bias voltage V b-ns Produces about 1V b-ns In at least one embodiment, the peak ion energy is about 370 eV.

[0085] Fig. 9C According to at least one embodiment, a non-sinusoidal continuous wave voltage generator (e.g. Figure 1 920 shows the angular spread of ions caused by the low-level to high-level pulse voltage waveform generated by the NSCWV generator 108 in FIG. 1 . In at least one embodiment, the low-level voltage is about 120V and the high-level voltage is about 360V. In at least one embodiment, Figure 3 In the pulse voltage waveform 300 shown, the low level voltage of 120V corresponds to V2 (NSCWV signal 304), and the high level voltage of 360V corresponds to V1 (NSCWV signal 302). In at least one embodiment, the angular spread of each ion in the time interval of the NCSWV signal 304 is greater than the angular spread of each ion in the time interval of the NCSWV signal 302. In at least one embodiment, again referring to Fig. 9C , the average ion angular spread E at high and low voltage levels A3 In at least one embodiment, the ion angular spread is less than Fig. 9B Angular spread of ions is shown for an applied voltage of 330 V. In at least one embodiment, as expected, the peak energy increases and the average angular spread decreases.

[0086] Fig.9D According to at least one embodiment, a non-sinusoidal continuous wave voltage generator (e.g. Figure 1930 shows the ion angular spread caused by the low-level to high-level pulse voltage waveform generated by the non-sinusoidal continuous wave voltage generator 108 in FIG. In at least one embodiment, the low-level voltage is about 210V and the high-level voltage is about 630V. In at least one embodiment, Figure 3 In the pulse voltage waveform 300 shown, the low level voltage of 210V corresponds to V2 (NSCWV signal 304), and the high level voltage of 630V corresponds to V1 (NSCWV signal 302). In at least one embodiment, the angular spread of each ion in the time interval of the NCSWV signal 304 is greater than the angular spread of each ion in the time interval of the NCSWV signal 302. In at least one embodiment, referring again to Fig.9D , the average ion angular spread E at high and low voltage levels A4 In at least one embodiment, the ion angular spread is less than Fig. 9B The angular spread of the ions for an applied voltage of 330 V is shown, or Fig. 9C In at least one embodiment, as expected, the peak energy increases and the average angular spread decreases.

[0087] In at least one embodiment, the etch profile, relative etch time and maximum groove width W T exist Figures 10A to 10D In at least one embodiment, simulation results of etching grooves in a substrate are shown corresponding to different pulse voltage waveforms applied to the chuck electrode when etching the grooves. Figures 10A to 10D The grooves shown are for use Figure 8B An embodiment of a recess 806 formed in a substrate 802 by a mask 804 is shown.

[0088] Fig. 10A is a cross-sectional view 1000 of an etch profile of a recess 1002 formed in a silicon substrate 1004 using a mask 804 according to at least one embodiment. In at least one embodiment, the plasma etching process used to form the recess 1002 corresponds to a process combining Fig.9A 1002 has an initial mask opening of 10 nm. In at least one embodiment, groove 1002 has a maximum width of 18.3 nm, which is caused by a peak ion angular spread of 3.32 degrees and an average ion angular spread of 7.7 degrees. In at least one embodiment, the etching time for etching a groove depth of about 200 nm is normalized to time t0.

[0089] Fig. 10B is a cross-sectional view 1010 of an etch profile of a recess 1012 formed in silicon recess 1004 using mask 804, as shown in at least one embodiment. Fig. 9B The ion angular spread described results in. In at least one embodiment, the groove 1012 has an initial mask opening of 10 nm. In at least one embodiment, the groove 1012 has a maximum width W of 18.8 nm. T , which is caused by a peak / average ion energy distribution of 8.1 degrees. In at least one embodiment, an etching time of 1.05t0 for etching a groove 1012 of about 200 nm is greater than that used to pattern the groove 1002 ( Fig. 10A )’s etching time is about 5% longer.

[0090] Fig. 10C is a cross-sectional view 1020 of an etch profile of a recess 1022 formed in a silicon substrate 1004 using a mask 804, according to at least one embodiment. Fig. 9C In at least one embodiment, the groove 1022 has an initial mask opening of 10 nm. In at least one embodiment, the groove 1022 has a maximum width of 16.9 nm, which is caused by the peak ion energy distribution of 7.3 degrees and the average ion angular spread of 7.1 degrees. In at least one embodiment, an etching time ratio of 1.05t0 is used to pattern the groove 1002 ( Fig. 10A )’s etching time is 5% longer.

[0091] In at least one embodiment, as the average angular spread decreases to 7.1 degrees, the maximum width W T In at least one embodiment, compared to etching groove 1002 ( Fig. 10A ) is reduced, which results in a longer etching time because of the addition of low voltage level pulses. In at least one embodiment, despite having a higher level of voltage, the etching rate is substantially the same as that of the etching groove 1012 ( Fig. 10B ) have the same etching rate.

[0092] Fig. 10D is a cross-sectional view 1030 of an etch profile of a recess 1032 formed in a silicon substrate 1004 using a mask 804 according to at least one embodiment, which is formed by combining Fig.9D The ion angular spread described above results in: In at least one embodiment, groove 1032 has an initial mask opening of 10 nm. In at least one embodiment, groove 1042 has a maximum width W of 17 nm. T , which is caused by a peak ion angular spread of 6.02 degrees and an average ion angular spread of 6.6 degrees. In at least one embodiment, an etching time ratio of 0.95t0 is used for patterning the groove 1002 ( Fig. 10A ) is about 7% shorter than the etching time for patterning recesses 1012 and 1022 (respectively at Fig. 10B and Fig. 10C )’s etching time is about 11% shorter.

[0093] In at least one embodiment, due to the addition of a higher level voltage and an additional “higher” low voltage level pulse, relative to the etched groove 1022 ( Fig. 10C ) of the etching rate, the etching rate is improved. In at least one embodiment, W T Maintained at approximately 17nm.

[0094] In at least one embodiment, the etch profile and mask erosion are Figures 10A to 10D In at least one embodiment, the different graphs correspond to pulsed voltage waveforms applied to a chuck electrode while etching a recessed feature in a substrate. Figures 10A to 10D The grooves shown are for use Figure 8B An embodiment of a recess 806 formed in a substrate 802 by a mask 804 is shown.

[0095] Figures 11A to 11D According to at least one embodiment Figures 10A to 10D FIG. 1 is an enhanced cross-sectional view of a mask in FIG. The recesses formed under each mask are not shown in the figure. According to at least one embodiment, each figure corresponds to a corresponding pulse voltage waveform applied to the chuck electrode when etching a recess feature in the substrate.

[0096] Fig.11A According to at least one embodiment, in etching and forming Fig. 10A 1100 of a cross-sectional view of mask 804 after a process of forming recess 1002 in the substrate. In at least one embodiment, the plasma etching process used to form recess 1002 corresponds to a process of combining Fig.9A Describe the voltage bias conditions on the chuck electrodes.

[0097] In at least one embodiment, again referring to Fig.11A , dotted line 1101 represents a reference line of the top of mask 804 before etching recess 1002. In at least one embodiment, mask 804 is eroded during etching of the recess. In at least one embodiment, mask 804 is eroded by an amount E1. In at least one embodiment, as shown, E1 is normalized to 100% erosion.

[0098] Fig. 11B According to at least one embodiment, in etching and forming Fig. 10B 1110 of a cross-sectional view of mask 804 after a process of forming recess 1012 in the mask. In at least one embodiment, the plasma etching process used to form recess 1012 corresponds to a process of combining Fig. 9B Describe the voltage bias conditions on the chuck electrodes.

[0099] Reference again Fig.11A , dotted line 1101 represents a reference line of the top of mask 804 before etching recess 1012. In at least one embodiment, mask 804 is eroded during etching of the recess. In at least one embodiment, mask 804 is eroded by an amount E2. As shown, E2 is about 1.04E1. In at least one embodiment, the greater mask erosion is a result of the narrow energy band, but is not related to the increase in the energy due to the combination of Fig.9A The voltage bias conditions on the chuck electrodes described result in a wider ion angular spread than that of ions .

[0100] Fig. 11C According to at least one embodiment, in etching and forming Fig. 10C The plasma etching process used to form the recess 1022 corresponds to the plasma etching process combined with the Fig. 9C Describe the voltage bias conditions on the chuck electrodes.

[0101] Reference again Fig.11A , dotted line 1101 represents a reference line of the top of mask 804 before etching recess 1022. In at least one embodiment, mask 804 is eroded by an amount E3. As shown, E3 is about 0.88E1. In at least one embodiment, the reduction in erosion of mask 804 is a level-by-level pulse voltage waveform (e.g. Figure 3 804). In at least one embodiment, high energy etching is prevalent during the higher voltage pulse stage. In at least one embodiment, reducing the voltage level from a high voltage level to a lower voltage level reduces the peak ion energy at the mask 804. In at least one embodiment, the ions are slowed down sufficiently to reduce the ion bombardment rate. In at least one embodiment, the duration of the higher ion energy bombardment and the lower ion energy bombardment depends on the duty cycle of the level-by-level pulse voltage waveform. In at least one embodiment, the duty cycle can determine the degree of mitigation of the different ion energy bombardment of the mask 804. In at least one embodiment, reducing the voltage level from a high voltage level to a lower voltage level can increase the preservation of the mask 804.

[0102] In at least one embodiment, the peak voltage is about 360 V and the ratio between the high voltage level and the low voltage level is 3: 1. In at least one embodiment, the angular spread of ions corresponding to the higher voltage level is less than 70% of the angular spread of ions corresponding to the lower voltage level.

[0103] Fig.11D According to at least one embodiment, in etching and forming Fig. 10D 1130 of a cross-sectional view of mask 804 after a process of forming recess 1032 in the mask. In at least one embodiment, the plasma etching process used to form recess 1032 corresponds to a process of combining Fig.9D Describe the voltage bias conditions on the chuck electrodes.

[0104] Reference again Fig.11D , dotted line 1101 represents a reference line of the top of mask 804 before etching recess 1032. In at least one embodiment, mask 804 is eroded by an amount E4. As shown, E4 is about 0.87E1.

[0105] In at least one embodiment, the reduced erosion of the mask 804 is the result of a level-to-level pulse voltage waveform, wherein ion bombardment of the mask 804 is mitigated during the lower voltage phase. In at least one embodiment, the peak voltage may be about 630 V. In at least one embodiment, the voltage level is higher than that of the etched recess 1022 ( Fig. 10A ) is implemented. In at least one embodiment, the ratio between the high voltage level and the low voltage level is maintained at 3:1. In at least one embodiment, the etching rate for forming the groove 1032 is significantly different from that for forming the groove 1022 ( Fig. 10C ). In at least one embodiment, the mask erosion rate is substantially similar to Fig. 11C The mask erosion rate observed in , for example, E4 to E3.

[0106] Reference again Fig.11D In one embodiment, the angular spread of ions corresponding to the higher voltage level is less than 70% of the angular spread of ions corresponding to the lower voltage level.

[0107] According to at least one embodiment, when used to form the groove 1032 ( Fig. 10D ) is further extended to produce a recess 1032 having a depth greater than the depth of recess 1032, a reduction in mask erosion may be beneficial.

[0108] Fig.12 A processor system 1200 having a machine-readable storage medium having instructions that, when executed, cause the processor to enhance ion energy and reduce ion energy distribution in an inductively coupled plasma according to at least one embodiment is shown. In at least one embodiment, the process can be stored as computer-executable instructions in a machine-readable storage medium (e.g., 1203). In at least one embodiment, the processor system 1200 includes a memory 1201, a processor 1202, a machine-readable storage medium 1203 (also referred to as a tangible machine-readable medium), a communication interface 1204 (e.g., a wireless or wired interface), and a network bus 1205 coupled together as shown.

[0109] In at least one embodiment, processor 1202 is a digital signal processor (DSP), an application specific integrated circuit (ASIC), a general purpose central processing unit (CPU), or low power logic that implements a simple finite state machine to perform the various processes described herein.

[0110] In at least one embodiment, the various logic blocks of the processor system 1200 are coupled together via a network bus 1205. In at least one embodiment, any suitable protocol can be used to implement the network bus 1205. In at least one embodiment, the machine-readable storage medium 1203 includes instructions (also referred to as program software code / instructions) for enhancing ion energy and reducing ion angular spread in an inductively coupled plasma as described above.

[0111] In at least one embodiment, the machine-readable storage medium 1203 is a machine-readable storage medium having instructions for enhancing ion energy and reducing ion angular spread in an inductively coupled plasma. In at least one embodiment, the machine-readable storage medium 1203 has machine-readable instructions that, when executed, cause the processor 1202 to perform the methods of measuring and / or reporting as discussed with reference to various embodiments.

[0112] In at least one embodiment, the program software codes / instructions associated with the various embodiments may be implemented as a portion of an operating system or a special purpose program, a component, a program, an object, a module, a routine, or other sequence of instructions or an organization of instruction sequences referred to as "program software codes / instructions", "operating system program software codes / instructions", "application software codes / instructions" or simply "software" or firmware embedded in a processor. In at least one embodiment, the program software codes / instructions associated with the processes of the various embodiments are executed by the processor system 1200.

[0113] In at least one embodiment, program software codes / instructions associated with various embodiments are stored in a computer executable machine readable storage medium 1203 and executed by a processor 1202. In this article, a computer executable machine readable storage medium 1203 is a tangible machine readable medium that can be used to store program software codes / instructions and data, which when executed by a computer device causes one or more processors (e.g., processor 1202) to perform a process. In at least one embodiment, the process can include controlling a pulsed voltage waveform. In at least one embodiment, the process can include controlling a pulsed voltage waveform to generate low voltage pulses and high voltage pulses with a predetermined duty cycle. In at least one embodiment, the process can include modulating the expansion of ion energy in a sheath region of a plasma by a pulsed voltage waveform. In at least one embodiment, the sheath region is adjacent to a substrate placed on an electrostatic chuck during processing. In at least one embodiment, the pulsed voltage waveform is a combination of two pulsed voltage signals, wherein the first voltage pulse has a higher base voltage amplitude level, and wherein the second voltage pulse has a lower base voltage amplitude level. In at least one embodiment, the first voltage pulse includes a first periodic voltage, and the second voltage pulse includes a second periodic voltage. In at least one embodiment, the first voltage pulse may be applied for a first duration that is greater than, equal to, or less than a second duration of the second voltage pulse. In at least one embodiment, the first voltage pulse is an example of a first NCSWV signal, and the second voltage pulse is an example of a second NCSWV signal that is combined with Figure 3 to Figure 5 The NCSWV signals 302 and 304 described are identical.

[0114] Reference again Fig.12 In at least one embodiment, the tangible machine-readable storage medium 1203 may include storage devices for executable software program codes / instructions and data in various tangible locations, including, for example, ROM, volatile RAM, non-volatile memory and / or cache memory (cache) and / or other tangible memory. In at least one embodiment, portions of program software codes / instructions and / or data may be stored in any of these storage devices and memory devices. In at least one embodiment, program software codes / instructions may be obtained from other storage devices, including, for example, through a centralized server or a peer-to-peer network (peer to peer network), including the Internet. In at least one embodiment, different portions of software program codes / instructions and data may be obtained at different times and in different communication sessions (communication session) or in the same communication session.

[0115] In at least one embodiment, the software program code / instructions can be obtained in full before executing the corresponding software program or application. In at least one embodiment, portions of the software program code / instructions and data can be obtained dynamically, such as in a timely manner, when execution is required. In at least one embodiment, some combination of these ways of obtaining software program code / instructions and data can occur, such as for different applications, components, programs, purposes, modules, routines, or other instruction sequences or organizations of instruction sequences. In at least one embodiment, it may not be necessary for the data and instructions to be all located on a tangible machine-readable medium at a particular point in time.

[0116] In at least one embodiment, the tangible machine-readable storage medium 1203 includes, but is not limited to, recordable and non-recordable media such as volatile and non-volatile memory devices, read-only memory (ROM), random access memory (RAM), flash memory devices, floppy disks and other removable disks, magnetic storage media, optical storage media (such as compact disk read-only memory (CDROM), digital versatile disk (DVD), etc.), etc. In at least one embodiment, the software program code / instructions may be temporarily stored on such digital tangible communication link while the transmission of electrical, optical or acoustic or other forms of signals such as carrier waves, infrared signals, digital signals, etc. is achieved through the tangible communication link.

[0117] Example 1: A method of generating a voltage pulse, comprising: generating a first non-sinusoidal continuous wave voltage (NSCWV) signal for a first duration of a clock cycle, the first NSCWV signal comprising a first base voltage and a first frequency; and performing a first transition, the first transition comprising changing from the first NSCWV signal to a second NSCWV signal, the second NSCWV signal being generated for a second duration of the clock cycle, the second NSCWV signal comprising a second base voltage and a second frequency.

[0118] Example 2: The method of Example 1, further comprising performing a second transition, the second transition comprising changing from the second NSCWV signal back to the first NSCWV signal.

[0119] Example 3: The method of Example 2, further comprising repeating the first transition and the second transition within the clock cycle range.

[0120] Example 4: The method of Example 1, wherein the magnitude of the first base voltage is greater than the magnitude of the second base voltage.

[0121] Example 5: The method according to Example 1, wherein the inverse of the sum of the first duration and the second duration defines a duty cycle of the voltage pulse, wherein the duty cycle of the first NSCWV signal is between 50% and 75%.

[0122] Example 6: The method of Example 1, wherein a sum of the first duration and the second duration defines a pulse frequency of the voltage pulses, wherein the pulse frequency is between 1 Hz and 100 kHz.

[0123] Example 7: A method according to Example 1, wherein generating the first NSCWV signal also includes: performing a first operation, which includes increasing a voltage level of a first amplitude from a reference voltage to the first base voltage within a first time interval; performing a second operation, which includes gradually changing the voltage level from the first base voltage to a first peak voltage within a second time interval; performing a third operation, which includes reducing the voltage level from the first peak voltage to the reference voltage within a third time interval; performing a fourth operation, which includes maintaining the voltage level at the reference voltage within a fourth time interval; and repeating the first operation, the second operation, the third operation, and the fourth operation within the first duration.

[0124] Example 8: The method of Example 7, wherein the first frequency is equal to 1 divided by the sum of the first time interval, the second time interval, the third time interval, and the fourth time interval.

[0125] Example 9: The method of Example 8, wherein the first frequency is between 2 Hz and 400 kHz.

[0126] Example 10: The method of Example 7, wherein the second time interval is at least 100 times larger than the first time interval or the third time interval, and wherein the fourth time interval is at least 100 times larger than the first time interval or the third time interval.

[0127] Example 11: The method of Example 10, wherein a ratio between the second time interval and the fourth time interval is greater than or equal to 2:1.

[0128] Example 12: The method of Example 10, wherein a ratio between the second time interval and the fourth time interval is 3:1.

[0129] Example 13: A method according to Example 7, wherein the reference voltage is a first reference voltage, the voltage level is a first voltage level, and wherein generating the second NSCWV signal further comprises: performing a fifth operation, comprising increasing the second voltage level from the second reference voltage to the second base voltage within a fifth time interval; performing a sixth operation, comprising gradually changing the second voltage level from the second base voltage to a second peak voltage within a sixth time interval; performing a seventh operation, comprising reducing the second voltage level from the second peak voltage to the second reference voltage within a seventh time interval; performing an eighth operation, comprising maintaining the second voltage level at the second reference voltage within an eighth time interval; and repeating the fifth operation, the sixth operation, the seventh operation, and the eighth operation within the second duration.

[0130] Example 14: The method of Example 13, wherein the second frequency is equal to 1 divided by the sum of the fifth time interval, the sixth time interval, the seventh time interval, and the eighth time interval.

[0131] Example 15: The method of Example 14, wherein the second frequency is between 2 Hz and 400 kHz.

[0132] Example 16: The method of Example 13, wherein the sixth time interval is at least 100 times larger than the fifth time interval or the seventh time interval, and wherein the eighth time interval is at least 100 times larger than the fifth time interval or the seventh time interval.

[0133] Example 17: The method of Example 16, wherein a ratio between the sixth time interval and the eighth time interval is greater than or equal to 2:1.

[0134] Example 18: The method of Example 16, wherein a ratio between the sixth time interval and the eighth time interval is 3:1.

[0135] Example 19: The method of Example 13, wherein a first magnitude of a first difference between the first base voltage and the first reference voltage is greater than a second magnitude of a second difference between the second base voltage and the second reference voltage.

[0136] Example 20: The method of Example 13, wherein the third amplitude of the first peak voltage is greater than or less than the fourth amplitude of the second peak voltage.

[0137] Example 21: A method of operating a plasma chamber to increase ion energy and reduce ion angular spread at a surface of a substrate during an etching operation, the method comprising: placing the substrate on an electrostatic chuck within the plasma chamber, wherein the electrostatic chuck is electrically coupled to a non-sinusoidal continuous wave voltage (NSCWV) generator; forming a plasma in the plasma chamber, wherein the plasma generates a sheath including a sheath voltage; and changing the sheath voltage by applying a voltage pulse at the electrostatic chuck using a continuous wave voltage source, wherein applying the voltage pulse comprises: generating a first non-sinusoidal continuous wave voltage (NSCWV) signal for a first duration of a clock cycle, the first NSCWV signal comprising a first base voltage and a first frequency; and performing a first transition, the first transition comprising changing from the first NSCWV signal to a second NSCWV signal, the second NSCWV signal being generated for a second duration of the clock cycle, the second NSCWV signal comprising a second base voltage and a second frequency.

[0138] Example 22: The method of Example 21, further comprising performing a second transition, the second transition comprising changing the second NSCWV signal back to the first NSCWV signal.

[0139] Example 23: The method of Example 22, further comprising repeating the first transition and the second transition within the clock cycle, wherein applying the voltage pulse effects a change in the spread of ion energy on the surface of the substrate.

[0140] Example 24: The method of Example 21, wherein the first NSCWV signal includes a first plurality of harmonics, and wherein applying the second NSCWV signal includes a second plurality of harmonics.

[0141] Example 25: The method of Example 24, wherein the first plurality of harmonics and the second plurality of harmonics include a fundamental frequency harmonic of 400 kHz, and up to and including the 10th harmonic.

[0142] Example 26: The method according to Example 21, wherein the voltage pulse further comprises: a positive cycle, a negative cycle, and a duty cycle between 0 and 100.

[0143] Example 27: The method of Example 21, wherein applying the first NSCWV signal further comprises: a first negative voltage and a gradual transition toward a second negative voltage, and wherein the second negative voltage is between 25% and 50% higher than the first negative voltage.

[0144] Example 28. A method of operating a plasma chamber to change the ion energy and ion angular spread at the surface of a substrate during an etching operation, the method comprising: placing the substrate on an electrostatic chuck within the plasma chamber, wherein the electrostatic chuck is electrically coupled to a non-sinusoidal voltage waveform generator; forming a plasma in the plasma chamber, wherein the plasma generates a sheath having a first sheath voltage; changing the first sheath voltage to a second sheath voltage by applying a first non-sinusoidal voltage waveform comprising a first periodic function at the electrostatic chuck to generate a first voltage response on the electrostatic chuck, the first voltage response achieving a first change in the spread of the ion energy at the substrate; and changing the second sheath voltage to a third sheath voltage by applying a second non-sinusoidal voltage waveform comprising a second periodic function at the electrostatic chuck to generate a second voltage response on the electrostatic chuck, the second voltage response achieving a second change in the spread of the ion energy at the substrate.

[0145] Example 29: The method of Example 28, wherein the first non-sinusoidal voltage waveform includes a first base voltage value, and wherein the first non-sinusoidal voltage waveform produces a first ion angular spread at the substrate.

[0146] Example 30: The method of Example 29, wherein the second non-sinusoidal voltage waveform includes a second base voltage value, and wherein the second non-sinusoidal voltage waveform produces a second ion angular spread at the substrate.

[0147] Example 31: The method of Example 30, wherein the first ion angular spread is less than 70% of the second ion angular spread.

[0148] Example 32: The method of Example 29, wherein the first ion angular spread produces an etch rate that is twice the etch rate produced by the second non-sinusoidal voltage waveform.

[0149] Example 33: A machine-readable storage medium having machine-executable instructions, which, when executed, cause one or more machines to perform a method comprising: controlling a pulse voltage waveform; controlling a periodic voltage; and controlling the expansion of ion energy in a sheath region of a plasma by controlling the pulse voltage waveform to produce low voltage pulses and high voltage pulses having a predetermined duty cycle.

[0150] Example 34: The machine-readable storage medium of Example 33, wherein the pulse voltage waveform has a duty cycle of at least 50% of the high voltage pulses.

[0151] In addition to what is described herein, various modifications may be made to at least one embodiment thereof without departing from its scope. Therefore, the description of at least one embodiment herein should be interpreted as an example rather than limiting the scope of at least one embodiment.

Claims

1. A method for generating a voltage pulse, wherein include: generating a first non-sinusoidal continuous wave voltage (NSCWV) signal at a first duration of a clock cycle, the first NSCWV signal comprising a first base voltage and a first frequency; and A first transition is performed, the first transition comprising changing from the first NSCWV signal to a second NSCWV signal, the second NSCWV signal being generated for a second duration of the clock cycle, the second NSCWV signal comprising a second base voltage and a second frequency. 2 . The method of claim 1 , further comprising performing a second transition, the second transition comprising changing from the second NSCWV signal back to the first NSCWV signal. The method according to claim 2 , further comprising repeating the first transition and the second transition within the clock cycle range. The method of claim 1 , wherein a magnitude of the first base voltage is greater than a magnitude of the second base voltage. 5 . The method of claim 1 , wherein the inverse of the sum of the first duration and the second duration defines a duty cycle of the voltage pulse, wherein the duty cycle of the first NSCWV signal is between 50% and 75%. 6 . The method of claim 1 , wherein a sum of the first duration and the second duration defines a pulse frequency of the voltage pulses, wherein the pulse frequency is between 1 Hz and 100 kHz.

7. The method of claim 1, wherein generating the first NSCWV signal further comprises: include: performing a first operation comprising increasing a voltage level of a first magnitude from a reference voltage to the first base voltage within a first time interval; performing a second operation comprising gradually changing the voltage level from the first base voltage to a first peak voltage within a second time interval; performing a third operation including reducing the voltage level from the first peak voltage to the reference voltage within a third time interval; performing a fourth operation comprising maintaining the voltage level at the reference voltage for a fourth time interval; as well as The first operation, the second operation, the third operation, and the fourth operation are repeated within the first duration.

8. The method of claim 7, wherein the first frequency is equal to 1 divided by the sum of the first time interval, the second time interval, the third time interval, and the fourth time interval.

9. The method of claim 8, wherein the first frequency is between 2 Hz and 400 kHz.

10. The method of claim 7, wherein the second time interval is at least 100 times greater than the first time interval or the third time interval and wherein the fourth time interval is at least 100 times greater than the first time interval or the third time interval. The method according to claim 10 , wherein a ratio between the second time interval and the fourth time interval is greater than or equal to 2:

1. 12 . The method of claim 10 , wherein a ratio between the second time interval and the fourth time interval is 3:

1.

13. The method of claim 7, wherein the reference voltage is a first reference voltage, the voltage level is a first voltage level, and wherein generating the second NSCWV signal further comprises: include: performing a fifth operation including increasing a second voltage level from a second reference voltage to the second base voltage within a fifth time interval; performing a sixth operation, comprising gradually changing the second voltage level from the second base voltage to a second peak voltage within a sixth time interval; performing a seventh operation including decreasing the second voltage level from the second peak voltage to the second reference voltage within a seventh time interval; performing an eighth operation including maintaining the second voltage level at the second reference voltage during an eighth time interval; as well as The fifth operation, the sixth operation, the seventh operation, and the eighth operation are repeated during the second duration.

14. The method of claim 13, wherein the second frequency is equal to 1 divided by the sum of the fifth time interval, the sixth time interval, the seventh time interval, and the eighth time interval. The method of claim 14 , wherein the second frequency is between 2 Hz and 400 kHz.

16. The method of claim 13, wherein the sixth time interval is at least 100 times greater than the fifth time interval or the seventh time interval and wherein the eighth time interval is at least 100 times greater than the fifth time interval or the seventh time interval. 17 . The method of claim 16 , wherein a ratio between the sixth time interval and the eighth time interval is greater than or equal to 2:

1. The method of claim 16 , wherein a ratio between the sixth time interval and the eighth time interval is 3:

1.

19. The method of claim 13, wherein a first magnitude of a first difference between the first base voltage and the first reference voltage is greater than a second magnitude of a second difference between a second base voltage and the second base voltage and the second reference voltage.

20. The method of claim 13, wherein a third magnitude of the first peak voltage is greater than or less than a fourth magnitude of the second peak voltage.

21. A method of operating a plasma chamber to increase ion energy and reduce ion angular spread at the surface of a substrate during an etching operation, the method include: placing the substrate on an electrostatic chuck within the plasma chamber, wherein the electrostatic chuck is electrically coupled to a non-sinusoidal continuous wave voltage (NSCWV) generator; forming a plasma in the plasma chamber, wherein the plasma generates a sheath including a sheath voltage; as well as The sheath voltage is varied by applying a voltage pulse at the electrostatic chuck using a continuous wave voltage source, wherein applying the voltage pulse comprises: generating a first non-sinusoidal continuous wave voltage (NSCWV) signal at a first duration of a clock cycle, the first NSCWV signal comprising a first base voltage and a first frequency; and A first transition is performed, the first transition comprising changing from the first NSCWV signal to a second NSCWV signal, the second NSCWV signal being generated for a second duration of the clock cycle, the second NSCWV signal comprising a second base voltage and a second frequency.

22. The method of claim 21, further comprising performing a second transition, the second transition comprising changing the second NSCWV signal back to the first NSCWV signal.

23. The method of claim 22, further comprising repeating the first transition and the second transition within the clock cycle, wherein applying the voltage pulse effects a change in the spread of ion energy on the surface of the substrate.

24. The method of claim 21, wherein the first NSCWV signal comprises a first plurality of harmonics and wherein applying the second NSCWV signal comprises a second plurality of harmonics.

25. The method of claim 24, wherein the first plurality of harmonics and the second plurality of harmonics include a fundamental harmonic of 400 kHz, and up to and including the 10th harmonic.

26. The method of claim 21, wherein the voltage pulse further include: Positive cycle, negative cycle, and duty cycle between 0 and 100.

27. The method of claim 21, wherein applying the first NSCWV signal further comprises: include: A first negative voltage and a gradual change toward a second negative voltage, wherein the second negative voltage is higher than the first negative voltage by between 25% and 50%.

28. A method of operating a plasma chamber to vary the ion energy and ion angular spread at the surface of a substrate during an etching operation, the method include: placing the substrate on an electrostatic chuck within the plasma chamber, wherein the electrostatic chuck is electrically coupled to a non-sinusoidal voltage waveform generator; forming a plasma in the plasma chamber, wherein the plasma generates a sheath having a first sheath voltage; changing the first sheath voltage to a second sheath voltage by applying a first non-sinusoidal voltage waveform comprising a first periodic function at the electrostatic chuck to produce a first voltage response on the electrostatic chuck, the first voltage response effecting a first change in the spread of ion energy at the substrate; as well as The second sheath voltage is changed to a third sheath voltage by applying a second non-sinusoidal voltage waveform including a second periodic function at the electrostatic chuck to produce a second voltage response on the electrostatic chuck, the second voltage response achieving a second change in the spread of ion energy at the substrate.

29. The method of claim 28, wherein the first non-sinusoidal voltage waveform comprises a first base voltage value and wherein the first non-sinusoidal voltage waveform produces a first ion angular spread at the substrate.

30. The method of claim 29, wherein the second non-sinusoidal voltage waveform comprises a second base voltage value, and wherein the second non-sinusoidal voltage waveform produces a second ion angular spread at the substrate.

31. The method of claim 30, wherein the first ion angular spread is less than 70% of the second ion angular spread.

32. The method of claim 29, wherein the first ion angular spread produces an etch rate that is twice the etch rate produced by the second non-sinusoidal voltage waveform.

33. A machine-readable storage medium having machine-executable instructions, which, when executed, cause one or more machines to perform a method comprising: Control pulse voltage waveform; Controlling periodic voltage; as well as The spread of ion energy in the sheath region of the plasma is controlled by controlling the pulse voltage waveform to generate low voltage pulses and high voltage pulses having a predetermined duty ratio.

34. The machine-readable storage medium of claim 33, wherein the pulse voltage waveform has a duty cycle of at least 50% of the high voltage pulses.