Aerosol generating product, preparation method and application thereof

Through the design of cage porous rod structure, the hollow structure of fiber material and the continuous structure of the wrapping material are used to solve the shortcomings of existing filter rods in cooling effect and suction resistance, and the effect of low suction resistance and effective cooling is achieved. , simplifies the process and reduces costs.

CN119054948APending Publication Date: 2024-12-03NANTONG CELLULOSE FIBERS CO LTD +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410770822.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The filter rods of existing new tobacco products have limited cooling effects, and the structural complexity makes it difficult to control the preparation process and cost, which affects the smoking experience.

Method used

The cage-type porous rod structure is adopted to form a hollow structure through the weaving and dissolution process of fiber material, providing a porous channel to reduce the flue gas temperature, and forming a continuous structure through the encapsulation material to improve the heat conduction effect.

Benefits of technology

It achieves low flue gas interception, low suction resistance and effective cooling, simplifies the cigarette coiling process, reduces costs and material demands, and improves the production speed and structural stability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119054948A_ABST
    Figure CN119054948A_ABST
Patent Text Reader

Abstract

An aerosol generating product comprises a fuming element, a cooling element and an outer layer packaging material wrapping and connecting the fuming element and the cooling element, the cooling element is located on the downstream of the flowing direction of smoke generated by the fuming element and comprises a cage type porous bar, and the cage type porous bar comprises a wall material. And the wall material has a hollow structure formed by interpenetrating and interweaving fiber materials. The cage type porous bar further comprises a hollow channel which is consistent with or parallel to the central axis of the wall material. The fiber material extends in a three-dimensional space, and a plurality of pore channels are formed among different fibers. The fiber materials are in a wave-like shape, and at least one fiber material extends spirally along the axis. The invention also discloses a preparation method and application of the aerosol generating product. According to the aerosol generating product, a smoke circulation path is increased, so that the aerosol generating product not only can effectively reduce the smoke temperature, but also can keep low smoke interception and low suction resistance of the smoke concentration as much as possible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of tobacco product production, and relates to an aerosol generating product, in particular to an aerosol generating product with cooling, low inhalation resistance and low filtering functions, a preparation method and application thereof. Background Art

[0002] In recent years, with the upgrading of consumption and the enhancement of people's health awareness, new tobacco products (heat-not-burn cigarettes) have attracted widespread attention in the domestic and foreign markets. They mainly meet the needs of smokers by volatilizing and releasing nicotine and flavor substances through heating (about 400°C). The smoke volume is small and the smoke temperature is high (the highest temperature in the first three puffs exceeds 60°C). Therefore, the corresponding filter rods are required to have low smoke retention, low suction resistance and improved cooling. The traditional acetate fiber tow filter rods have a complex network structure formed by thousands of fibers arranged axially, which will lead to large suction resistance and obvious smoke interception and filtration effects, affecting the smoker's experience. Chinese patent CN104203015 discloses an aerosol-generating article with an aerosol cooling element. The cooling element of the product is composed of a pleated polylactic acid film layer. When the cigarette is smoked, the continuous polylactic acid will undergo significant thermal shrinkage deformation, and its safety needs to be verified. At the same time, its high surface area also improves smoke adsorption and reduces the consumer's smoking experience.

[0003] Some new filter rods have been developed at home and abroad to meet the needs of new tobacco use, mainly by designing new filter rods, making structural innovations on filter rods, or adjusting the pore distribution of filter rods through punching technology to achieve low suction resistance, or embedding a section of empty tube structure in the filter rod. CN115297740A and CN115297739A disclose a cooling element for cooling external air entering the first tubular element through the ventilation area. The cooling effect of this structure on the smoke is very limited, lacking a complex pore structure that effectively cools the smoke, and the ventilation area affects the release of smoke from mouth to mouth. Or use more complex porous special-shaped firmware to disturb the airflow and reduce the temperature. The complexity of the product structure of this type of filter rod poses a great challenge to the preparation process, continuous production application and cost control.

[0004] Therefore, it is urgent to develop a new type of cigarette filter rod suitable for new tobacco products (heat-not-burn cigarettes) with a rich pore structure. Cigarettes using the new filter rod can effectively reduce the smoke temperature and maintain low smoke retention and low inhalation resistance at the smoke concentration as much as possible. Summary of the invention

[0005] To solve the above problems, the object of the present invention is to provide an aerosol generating product with low smoke retention, low draw resistance and the ability to quickly reduce the temperature of cigarette smoke, a preparation method and its application.

[0006] The technical solution of the present invention to solve the technical problem is:

[0007] An aerosol generating product comprises: a smoking element, a cooling element, and an outer packaging material wrapping and connecting the smoking element and the cooling element, wherein the cooling element is located downstream of the flow direction of smoke generated by the smoking element, and the cooling element comprises a rod with a shaped hole, and the cooling element may comprise a shaped hole structure and a wrapping material, wherein the wrapping material wraps the shaped hole structure to form a rod with a porous structure.

[0008] Furthermore, the cooling element comprises a cage-type porous bar, and the cage-type porous bar comprises a wall material, and the wall material has a hollow structure formed by interlacing and interweaving fiber materials.

[0009] Optionally, the cage-type porous rod further comprises a hollow channel which is consistent with or parallel to the central axis of the wall material.

[0010] Optionally, the fiber material extends in three-dimensional space, and a plurality of pore channels are formed between different fibers.

[0011] Optionally, the fiber material is wavy in shape, and at least one fiber material extends spirally along the axis.

[0012] Optionally, the wall material contains pore channels, including uniform and / or non-uniform channels; optionally, the pore channels are three-dimensional, non-linear network gaps.

[0013] Optionally, the cage-type porous rod is cylindrical; and / or, its outer diameter is 4-9 mm; and / or, the hollow channel is a single diameter or variable diameter channel, and the diameter of the hollow channel is 0.1 mm-8.5 mm, preferably 0.5-4.5 mm.

[0014] Optionally, the outer diameter length of the cage-type porous rod varies periodically along the axial direction, and the outer diameter varies in the range of 0.5-9 mm, preferably 2-8 mm.

[0015] Optionally, the wall material has a thickness of 0.2-4 mm and a porosity of 10-90%.

[0016] Optionally, the hardness of the cage-type porous rod is above 30%, preferably 60%-98%, more preferably 80%-95%.

[0017] Optionally, the fiber material is yarn, which is a long linear material comprising: at least one basic fiber, which may be fiber filament, staple yarn, fancy yarn, polymer wire, or metal wire; and / or at least one bonding material, which may be used as a shaping material and distributed between and on the surface of the basic fiber material.

[0018] Optionally, the content of the bonding material (shaping material) is 0.1-95%, preferably 5-75%, preferably 15-45%; and the base fiber is the remainder of 100%.

[0019] Optionally, the base fiber includes but is not limited to cellulose, regenerated cellulose, cellulose ester, cellulose ether, any derivatives thereof, starch-based thermoplastic resin, cellulose acetate, polylactic acid, chitosan, alginate, polyhydroxybutyrate, poly-ε-caprolactone, polyglycolic acid, polyhydroxyalkanoate, polypropylene, polyethylene, polyvinyl alcohol, polyester fiber, polyamide fiber, polyurethane, polyacrylonitrile, and any derivatives thereof, any copolymers thereof, and any one or more combinations of metals.

[0020] Optionally, the adhesive material comprises a film-forming material having an adhesive effect, including but not limited to one or more of cellulose acetate, polylactic acid, chitosan and its derivatives, cellulose derivatives, alginate, polyvinyl alcohol, polysaccharides, polyester, polyolefin, polyethylene glycol, and any derivatives thereof.

[0021] Preferably, the bonding material is a soluble fiber that dissolves in a certain dissolving medium, including but not limited to any one of acetate fiber, polylactic acid fiber, polyvinyl alcohol fiber, chitosan fiber, seaweed fiber, cellulose derivatives, and composite fibers of two or more of these materials.

[0022] Preferably, the bonding material is water-soluble fiber, preferably including polyvinyl alcohol fiber, seaweed fiber, carboxymethyl cellulose fiber.

[0023] The preparation method of the cage filter rod includes selecting basic fibers and fiber-line-shaped adhesive materials (also called adhesive fibers), wherein the basic fibers and the adhesive fibers have different solubility properties. The cage rod is prepared by weaving, dissolving and drying the basic fibers and the adhesive fibers; wherein the dissolving means placing the intermediate product obtained by weaving into a dissolving medium, and removing part of the adhesive fibers by dissolving to obtain the cage rod.

[0024] The following steps are involved:

[0025] (1) selecting a certain ratio of base fiber and binder fiber to prepare at least two yarns, wherein the yarns are single-component fibers or multi-component fibers;

[0026] Optionally, the multi-component fiber yarn is obtained as a linear material by doubling or sizing base fibers and / or bonding fibers.

[0027] Optionally, the multi-component fiber yarn is obtained by composite spinning of a base fiber material and / or a bonding fiber material to obtain a linear material.

[0028] Preferably, cellulose acetate is selected as the basic fiber and the cage rod skeleton, and water-soluble polyvinyl alcohol is selected as the bonding and shaping material and the pore-forming material.

[0029] Preferably, the base fiber is acetate fiber filament or staple fiber yarn, with a fineness of 100-5000D and a weight percentage of 10-95%; the preferred bonding fiber is polyvinyl alcohol fiber filament or staple fiber yarn, with a fineness of 100-5000D and a weight percentage of 90-5%.

[0030] (2) Winding different yarns on a braiding machine spindle for braiding to obtain a round belt-shaped intermediate product;

[0031] The number of spindles of the knitting machine is 16-128, and the ratio of the number of spindles of different yarns is 1:15-15:1. Preferably, the ratio of the number of spindles of acetate fiber yarn to polyvinyl alcohol fiber yarn is 1:5-5:1.

[0032] The pore channels of the cage-type rods of the present invention are related to the arrangement direction of the fiber yarns and can be adjusted by selecting different weaving process parameters.

[0033] Optionally, when the ratio of the number of spindles of acetate fiber to that of polyvinyl alcohol fiber is 1:1 and they are evenly arranged alternately, the wall material of the cage-type rod obtained in step 3 below has evenly distributed channels. When the ratio of the number of spindles of acetate fiber to that of polyvinyl alcohol fiber is not 1:1, or they are unevenly arranged alternately, or the fineness of the fiber yarns is different, the pore channels of the wall material obtained in step (3) are unevenly distributed pore channels.

[0034] (3) Soaking the round-shaped intermediate product obtained in step (2) in a certain dissolving medium and drying it to dissolve part of the bonding fiber to obtain a hollow tube wall structure and a cage-like rod with stiffness meeting the requirements, wherein the main body of the tube wall is the basic fiber and the remaining bonding fiber material as the shaping material.

[0035] Compared with the round belt intermediate product (step 2) that has not been washed in step (3), the ends of the intermediate product are loose and cannot be cut into short lengths for use; it cannot maintain a stable circumference and is easily squeezed and stretched to form a flat structure similar to shoelaces, which is not in the shape of a strip, and the structure is unstable in all directions, which cannot meet the requirements of the cigarette rolling process.

[0036] Optionally, when polyvinyl alcohol fiber is selected as the bonding material, the dissolving medium is water, and the round-shaped intermediate product is placed in water by one or more methods such as standing, flushing with running water, heating, and ultrasound to achieve partial dissolution of the bonding fiber (polyvinyl alcohol fiber) and separation from the base fiber (acetate fiber).

[0037] Optionally, the round-belt-shaped intermediate product is placed in room temperature water, the water temperature is uniformly increased to 40-100° C. within 0.5-30 min, the heating is stopped and the product is kept warm and soaked for 1-60 min, and then taken out and dried. This allows the round-belt-shaped intermediate product to shrink uniformly and move inwards close to the core material diameter, making the tube wall more three-dimensional.

[0038] Optionally, the round-ribbon intermediate product is soaked in room temperature water for 0.5-30 min, then transferred to 40-100° C. water for ultrasonic treatment for 1-15 min, with an ultrasonic power of 20-60 KHz and a power of 200 W-1000 W, and then taken out and dried.

[0039] Optionally, the round-shaped intermediate product is soaked in room temperature water for 0.5-30 minutes, transferred to 40-100°C water for fixation, and then washed with running water at a water flow rate of 1-10 m / s, a water temperature of 20-100°C, and a time of 1-30 minutes, and then taken out and dried. When washing with running water, mechanical vibration can be used to improve the dissolution performance.

[0040] The cage rod needs to be dried or naturally dried after the dissolving process to make the cage rod dry and harden, the drying temperature is 40-120° C., the drying time is 2-60 minutes, or it can be naturally dried until it is completely hardened, and then the core rod is taken out.

[0041] About the use and principle of the mandrel:

[0042] Optionally, a braiding mandrel A and a soaking mandrel B are used in step (2) and step (3).

[0043] The diameter of the round belt intermediate product obtained by the braiding machine is directly related to the fineness of the yarn on the braiding machine spindle and the number of spindles. The finer the yarn and the more spindles, the higher the cage rod diameter.

[0044] In the weaving process of step (2), the role of the weaving mandrel A is to expand the round belt intermediate product to the required diameter by filling the mandrel A when the yarn fineness and the number of weaving spindles make it difficult to directly prepare the round belt intermediate product with the required diameter. The diameter of the round belt intermediate product can be flexibly adjusted by adjusting the diameter of the mandrel A, which is more convenient than adjusting the number of weaving spindles and the yarn fineness.

[0045] Optionally, the diameter of the braided mandrel A is 0.1-8.5 mm, and the material is a material with a smooth surface and a certain compressive resistance, including but not limited to polytetrafluoroethylene, silicone, wood, metal, etc.

[0046] Furthermore, in order to obtain a cylindrical rod with the required diameter and stability, a core rod B is added during the washing process in step (3), that is, the core material B is added to the central cavity of the round belt-shaped intermediate product. The use of the soaking core rod B has the following functions: first, to prevent the round belt intermediate product from over-shrinking during soaking and reducing the diameter to a value lower than the required value; second, to prevent uneven shrinkage and undesirable deformation of the round belt intermediate product, and the core rod B can be shaped; third, to prevent the round belt intermediate product from being deformed under water scouring, ultrasonic and other operations; fourth, when transferring from the soaking environment to the drying environment, the round belt intermediate product is very easy to deform due to its own softening. Adding the core rod B can prevent deformation during transfer and maintain the shape of the round belt intermediate product unchanged and uniform during drying.

[0047] The diameter of the soaked core rod B is 10%-100% of the diameter of the cavity of the round intermediate product obtained in step (2). The core material is a smooth, water-resistant, and high-temperature resistant material, including but not limited to polytetrafluoroethylene, silicone, wood, metal, etc.

[0048] Optionally, after step (3), an independent sizing process is performed to infiltrate the fibers and the surface with a bonding material so that the obtained cage-type rod maintains a certain cylindrical shape and structural stiffness. The bonding material includes, but is not limited to, one or more of cellulose acetate, polylactic acid, chitosan and its derivatives, cellulose derivatives, alginate, polyvinyl alcohol, polysaccharides, polyesters, polyolefins, polyethylene glycol, flavors and fragrances, humectants, dyes, and any derivatives thereof.

[0049] Optionally, a certain amount of hot-melt fiber can be added in step (1), wherein the hot-melt fiber is one or a mixture of polyolefin, polyester, polyamide, polyimide, polyacetal, cellulose ester, cellulose ether, polysaccharide-based thermoplastic material, any derivative thereof, or any copolymer thereof; the softening point of the hot-melt fiber is lower than that of other base fibers and bonding fibers.

[0050] The step (2) is to weave a round-belt-shaped intermediate product containing hot-melt fibers; heat the hot-melt fibers until they are melted and bond them to the surface of the round-belt-shaped intermediate product to fix them; and wash the round-belt-shaped intermediate product to obtain a cage-type rod with a porous structure and high stiffness.

[0051] Optionally, in step 2, the content of the hot-melt fiber in the base fiber is 5%-100%, preferably 15-85%, while the content ratio of the base fiber to the bonding fiber remains unchanged, still 10%-95%:90%-5%; the bonding fiber here can only play a pore-forming role, such as the complete dissolution of polyvinyl alcohol. The hot-melt fiber can play a bonding role or can be completely used as a basic skeleton fiber.

[0052] Optionally, any functional fibers are introduced into the yarn to obtain rods with desired pore characteristics and functional properties.

[0053] Furthermore, the aerosol generating product further comprises an upstream element located upstream of the smoking element, which can adjust the draw resistance of the aerosol generating product and block the granular smoking element. Optionally, a filter rod or a hollow filter rod made of conventional acetate fiber tow is used.

[0054] Furthermore, the aerosol generating product further comprises a mouthpiece element, which is located downstream of the smoke flow direction through which the smoke cooling element passes.

[0055] Optionally, the mouthpiece element is made of ultra-high denier cellulose acetate tow, and the ultra-high denier cellulose acetate tow has a denier greater than or equal to 10 deniers. By combining with the cooling element, low smoke absorption resistance and low smoke retention can be achieved.

[0056] Optionally, a hollow element is further included, which is located upstream of the flue gas flow direction through which the flue gas cooling element passes.

[0057] The preparation method of the aerosol generating product is as follows: the cage-type porous rod is encapsulated in an outer layer of wrapping material to obtain a cigarette filter rod; the cigarette filter rod is cut into a fixed length and then combined with other components to obtain the aerosol generating product; optionally, the wrapping material includes but is not limited to cellulose paper, fabric, non-woven fabric, plastic sheet, ceramic, glass; preferably, the wrapping material is cigarette forming paper or transparent film.

[0058] The aerosol generating product is used in cigarettes and heat-not-burn cigarettes.

[0059] Due to the adoption of the above technical solution, the present invention has the following beneficial effects:

[0060] 1. The nonlinear and porous structure on the wall of the cage structure guides and distributes the circulating flue gas, prolongs the flow path of the flue gas, provides the flue gas heat exchange and cooling potential, and is conducive to flue gas condensation and cooling;

[0061] 2. The pores on the wall of the cage structure of the present invention can form a continuous structure with the wrapping material, which is beneficial to the heat conduction of high-temperature flue gas and further improves the cooling effect;

[0062] 3. Compared with conventional acetate fiber pipes, the cage-type rods have millimeter-level large pores on their walls, multiple levels of pores, and low gram weight. They can replace the existing technology (combination of thin-walled tubes and thick-walled tubes), reduce at least one step of the cigarette rolling process, and reduce cigarette processing costs and material costs;

[0063] 4. The cage structure can be woven into rods and washed to form holes in one step, which has the characteristics of fast production speed, low cost and stable product structure quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1The present invention is a schematic diagram of a three-stage aerosol generating product structure embodiment with a smoke temperature reducing element.

[0065] Figure 2 The figure is a schematic diagram of a structural embodiment of a four-stage aerosol generating product having a smoke temperature reducing element according to the present invention.

[0066] Figure 3 This is a schematic diagram of another structural embodiment of a four-stage aerosol generating product with a smoke temperature reducing element of the present invention.

[0067] Figure 4 Schematic diagram of the structure of a four-stage aerosol generating product in the prior art (a reference sample containing a wrinkled polylactic acid film).

[0068] Figure 5 It is a schematic structural diagram of an embodiment of a cage-type rod intermediate product of the present invention before immersion.

[0069] Figure 6 This is a schematic diagram of the structure of an embodiment of the cage-type bar intermediate product of the present invention after being filled with core material.

[0070] Markings in the figure: 1- round belt-shaped intermediate product, 2- core material.

[0071] Fig. 7A This is a 3D schematic diagram of the braided structure of an embodiment of the cage rod of the present invention.

[0072] Figure 7B This is a physical picture of an intermediate product (before immersion) in one embodiment of the cage rod of the present invention.

[0073] Figure 7C This is a real picture of the intermediate product after soaking and drying in one embodiment of the cage-type rod of the present invention.

[0074] Figure 8 This is a physical picture taken from another angle of view of the intermediate product after soaking and drying in one embodiment of the cage-type rod of the present invention.

[0075] Fig. 9A It is a 3D schematic diagram of a radial cross section of an embodiment of a cage rod of the present invention.

[0076] Fig. 9B This is a physical diagram of a radial cross section of an embodiment of a cage-type rod of the present invention.

[0077] Fig.10 It is a schematic axial cross-sectional view of an embodiment of a cage rod of the present invention. DETAILED DESCRIPTION

[0078] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0079] The present invention relates to an aerosol generating product with low smoke retention and capable of reducing cigarette smoke temperature and a related method.

[0080] An aerosol generating product is assembled into a bar by multiple components in the form of bar composite molding. The multiple components include a smoking component and a component for reducing the temperature of smoke located downstream of the smoking component, and the aerosol passing through the smoke cooling component is cooled.

[0081] An aerosol generating product comprises: a smoking element, a cooling element, and an outer packaging material wrapping and connecting the smoking element and the cooling element, wherein the cooling element is located downstream of the flow direction of smoke generated by the smoking element, and the cooling element comprises a cage-type porous rod, wherein the cage-type porous rod comprises a wall material, and the wall material has a hollow structure formed by interlacing and interweaving fiber materials.

[0082] The aerosol generating product of the present invention can provide a new smoke flow channel, thereby producing different effects on smoke composition, temperature reduction and inhalation resistance.

[0083] The present invention will be further described below in conjunction with the embodiments shown in the accompanying drawings. Obviously, the described embodiments are only some examples, not all examples.

[0084] Example 1

[0085] like Figure 1 As shown, a three-stage aerosol production product 10 with a smoke temperature reducing element of the present invention includes a plurality of elements assembled in the form shown in the figure, and the plurality of elements include a smoking element 20, a cooling element 30 downstream of the smoking element, and a mouthpiece 40 downstream of the cooling element. When the cigarette is inhaled, the direction of smoke flow in the cigarette is recorded as from "upstream" to "downstream". These three elements are coaxially assembled in sequence by tightly wrapping with cigarette paper 50 to form a rod 11. When compositely assembled, the rod 11 has a length of approximately 45 mm, an outer diameter of approximately 7.2 mm, and an inner diameter of approximately 6.9 mm.

[0086] The smoking element 20 comprises filamentous or pleated tobacco material, which is rolled by a cigarette rolling machine and wrapped in a forming paper to form a rod. The tobacco material comprises additives, and the additives include glycerol and propylene glycol, which are additives for forming aerosols.

[0087] The smoke cooling element 30 is immediately downstream of the smoke generating element 20 and is a rod containing a cage-like porous substance. The cage-like porous rod is wrapped by a wrapping material or may not be wrapped by a wrapping material.

[0088] The cage-type porous rod has an outer diameter of about 6.9 mm, a center hole diameter of about 4 mm, a wall thickness of about 1.4 mm, wall holes accounting for about 75%, and a pore spacing of about 2 mm.

[0089] The method for preparing the cage-type porous rod comprises:

[0090] (1) Select acetate fiber with a fineness of 2200D and polyvinyl alcohol fiber with a fineness of 1100D.

[0091] (2) The number of weaving spindles is 32, the ratio of acetate fiber spindles to polyvinyl alcohol fiber spindles is 1:1, and a hollow round belt-shaped intermediate product is woven, in which the ratio of acetate fiber to polyvinyl alcohol fiber is 67%:33%.

[0092] (3) The hollow part of the round-shaped intermediate product is filled with a core material with a diameter of 4 mm. The initial immersion temperature is 20°C and the immersion time is 30 min. It is then transferred and immersed in 80°C water. After being fixed, it is flushed with running water for 20 min at a flushing speed of 2 m / s.

[0093] (4) The round strip intermediate product after soaking is dried at 60°C for 30 minutes. The flue gas cooling element containing the porous rod has a length of about 25 mm.

[0094] The mouthpiece 40 is made of an ultra-high denier cellulose acetate tow bar of 20D, with a length of 8mm, an outer diameter of about 7.1mm, an inner diameter of about 6.9mm, and a pressure drop of 8.3Pa / mm.

[0095] like Figure 1 In the aerosol generating product shown in the figure, a heating element is inserted upstream of the smoking element 20 to heat the tobacco material in the smoking element 20 so that volatile compounds are released from the tobacco material. The consumer draws on the end face of the mouthpiece 40 of the aerosol generating product 10, and these volatile compounds are condensed and atomized to form an aerosol, which is delivered to the mouth of the consumer through the rod 10.

[0096] The aerosol is sucked through the smoke cooling element 30 to exchange heat, the temperature of the aerosol is reduced, and the moisture in the aerosol is intercepted.

[0097] Control group - aerosol generating product A:

[0098] According to the cigarette smoking model specified in the national standard GB / T19609-2004, the smoking was simulated, and the Canadian deep smoking mode (HCI) was used to investigate the effect of the smoke cooling element on the mainstream aerosol temperature and the mainstream aerosol nicotine content of each puff. The reference aerosol generating product A containing a hollow tube with a length of 15 mm and an inner diameter of about 5.2 mm and a cellulose acetate hollow tube with a length of 10 mm upstream and an inner diameter of 3.3 mm as a cooling element was studied and compared. The thermocouple temperature probe was located at the center of the filter tip 40 0 ​​mm from the mouth end. The test results are shown in Tables 1 and 2.

[0099] It can be found that compared with the cooling element of the acetate fiber hollow tube structure, the aerosol production product containing the cage-type cylindrical rod of the present invention has basically the same draw resistance, that is, low draw resistance; the inlet smoke temperature is reduced by about 4-11°C, and at the same time the nicotine release in the smoke is increased by 0.2 mg, that is, the interception efficiency of the mouthpiece is reduced, showing a significant cooling and low filtration effect.

[0100] Table 1 - Mainstream aerosol temperature test results

[0101] Suction port sequence 1 2 3 4 5 6 Smoke temperature of product A (℃) 65 66 58 55 55 54 Example 1 Smoke Temperature of the Product (°C) 60 61 52 48 46 43

[0102] Table 2-Aerosol generating products and main smoke data

[0103]

[0104] Example 2

[0105] like Figure 2 As shown, a four-stage aerosol production product 10 with a smoke temperature reducing element of the present invention comprises a plurality of elements assembled in the form shown in the figure, the plurality of elements comprising a smoking element 20, a cellulose acetate filter rod 60 upstream of the smoking element, a cooling element 30 downstream of the smoking element, and a mouthpiece 40 downstream of the cooling element. These four elements are coaxially wrapped and assembled into a rod 11 with cigarette paper 50 in sequence. When compositely assembled, the rod 11 has a length of approximately 45 mm, an outer diameter of approximately 7.2 mm, an inner diameter of approximately 6.9 mm, and can be perforated for ventilation at a position 18 mm from the mouthpiece end, with a ventilation degree of approximately 50%.

[0106] The smoking element 20 includes filamentous or pleated tobacco material, which is rolled by a cigarette rolling device, and can be any other form of tobacco material such as granular.

[0107] The smoke cooling element 30 is immediately downstream of the smoke-generating material and is a rod having a cage-type porous structure, which is wrapped by a wrapping material 31. In this embodiment, the preparation method of the smoke cooling element 30 is the same as that of Example 1, with an outer diameter of about 6.9 mm, a center hole diameter of about 4 mm, a wall thickness of about 1.4 mm, and wall holes accounting for about 75%.

[0108] The flue gas cooling element including the porous rod has a length of approximately 16 mm.

[0109] The mouthpiece 40 is made of an ultra-high denier cellulose acetate tow bar of 20D, with a length of 12mm, an outer diameter of about 7.1mm, an inner diameter of about 6.9mm, and a pressure drop of about 8.3Pa / mm.

[0110] The acetate filter rod 60 is located upstream of the smoke generating element 20 and is made of a conventional acetate tow filter rod. It is 5 mm in length, has an outer diameter of about 7.1 mm, and an inner diameter of about 6.9 mm. It can be used to block the granular smoke generating element 20 and reduce cleaning requirements during use.

[0111] like Figure 2 The aerosol generating product shown in the figure has a heating element wrapped around the outer periphery of the smoking element 20, which can be electromagnetic induction heating or resistance heating, to heat the tobacco material in the smoking element 20, so that volatile compounds are released from the tobacco material. According to the national standard GB / T19609-2004, the smoke temperature and release amount of the trial-produced cigarettes were tested using the Canadian deep smoking mode, and the results are shown in Table 3.

[0112] Control group - aerosol generating product B:

[0113] The prior art reference sample, containing a hollow tube with a length of 8mm and an inner diameter of 5.3mm and an upstream acetate hollow tube with a length of 8mm and an inner diameter of 3.3mm, with a hole punched 2mm away from the upstream tube and a ventilation rate of about 50%, was used as a cooling element. A study and comparison was conducted, and the results are shown in 3.

[0114] Table 3 Data of aerosol generating products using 16 mm cooling elements

[0115]

[0116] It can be found that compared with the acetate hollow filter rod cooling element of the prior art, the temperature of the product using the cage-type hollow rod of the present invention is reduced by about 5°C. This is mainly because the pore structure distributed on the wall of the cage structure is conducive to the external transfer of heat; the nicotine release amount remains basically the same.

[0117] Example 3

[0118] like Figure 3 As shown, a four-stage aerosol production product 10 with a smoke temperature reducing element of the present invention includes a plurality of elements assembled in the form shown in the figure, the plurality of elements including a smoking element 20, a hollow acetate fiber tube 70 downstream of the smoking element, a cooling element 30 located downstream of the hollow fiber tube 70, and a mouthpiece 40 downstream of the cooling element. When the cigarette is inhaled, the direction of smoke flow in the cigarette is recorded as from "upstream" to "downstream". These four elements are coaxially assembled in sequence by tightly wrapping with cigarette paper 50 to form a rod 11. When compositely assembled, the rod 11 has a length of approximately 45 mm, an outer diameter of approximately 7.2 mm, and an inner diameter of approximately 6.9 mm.

[0119] The smoking element 20 comprises filamentous or pleated tobacco material, which is rolled by a cigarette rolling machine and wrapped in a forming paper to form a rod. The tobacco material comprises additives, and the additives include glycerol and propylene glycol, which are additives for forming aerosols.

[0120] The smoke cooling element 30 is located downstream of the hollow tube 70. In this embodiment, the smoke cooling element comprises a cage-type porous rod, and the smoke cooling element 30 has a length of approximately 15 mm.

[0121] The hollow tube 70 is made of cellulose acetate, has a length of 10 mm, an outer diameter of 7.1 mm, and an inner diameter of 3.3 mm.

[0122] The mouthpiece 40 is made of an ultra-high denier cellulose acetate tow bar of 22D denier, 8 mm in length, with an outer diameter of about 7.1 mm, an inner diameter of about 6.9 mm, and a pressure drop of 8.2 Pa / mm.

[0123] like Figure 4 In the conventional aerosol generating product shown in FIG, a heating element is inserted upstream of the smoking element 20 to heat the tobacco material in the smoking element 20 so that volatile compounds are released from the tobacco material. The consumer draws on the end face of the mouthpiece 40 of the aerosol generating product 10, and these volatile compounds are condensed and atomized to form an aerosol, which is delivered to the consumer's mouth through the rod 10.

[0124] The aerosol is sucked through the smoke cooling element 30 to exchange heat, and the temperature of the aerosol is reduced.

[0125] The smoking simulation was carried out according to the cigarette smoking model specified in the national standard GB / T19609-2004, using the Canadian deep smoking mode (HCI). The effects of the smoke cooling element on the mainstream aerosol temperature and the total mainstream aerosol nicotine content of each puff were investigated.

[0126] Control group - aerosol generating product C:

[0127] Prior art reference samples: Figure 4 As shown, a reference aerosol generating product C comprises a PLA film folded cooling element with a length of 15 mm, a porosity of 72%, and a thickness of about 35 microns, and a acetate hollow tube with a length of 10 mm and an inner diameter of 3.3 mm. The test results are shown in Tables 4 and 5.

[0128] Table 4 Mainstream aerosol temperature test results of four-stage aerosol production products

[0129]

[0130] Table 5 - Mainstream smoke and product draw resistance data

[0131]

[0132] It can be found from Tables 4 and 5 that, compared with the 15 mm corrugated polylactic acid cooling element (product C), the aerosol production product containing the cage-type porous cylindrical cooling element of the present invention has a significantly increased nicotine release in the smoke of about 0.8 mg / cig, an increase of 43%. At the same time, the maximum temperature of the smoke is basically the same at 60°C. After inhalation, it is observed that the cage-type porous structure close to the smoking end does not undergo the heat melting deformation phenomenon of the PLA corrugated membrane, showing the effects of low suction resistance, low filtration and cooling.

[0133] Reference Sample C

[0134] like Figure 4 As shown, the four-stage aerosol generating product 10 (reference sample D) in the prior art includes four components: a smoking element 20, a hollow cellulose acetate tube 70, a pleated polylactic acid film cooling element 80, an outer layer wrapping material 81 of the cooling element, and a filter 40. When the cigarette is inhaled, the direction of smoke flow in the cigarette is recorded as from "upstream" to "downstream". The aerosol smoking element 20 is located upstream of the rod; the hollow cellulose acetate tube 70 is located downstream of the smoking element; the pleated polylactic acid film cooling element 80 is located downstream of the hollow cellulose acetate tube 70; and the filter 40 is located downstream of the pleated polylactic acid film cooling element 80. These four components are coaxially wrapped and tightly wrapped with cigarette paper 50 in sequence to form a rod 11.

[0135] Figures 5 to 10 The following are pictures of the cage-type rods used in the aerosol production product of the present invention, specifically:

[0136] Figure 5 The figure shows a schematic diagram of the structure of the intermediate product before soaking in one embodiment of the cage-type rod. The round belt-shaped intermediate product is a hollow cylindrical structure before soaking, and the tube wall is interwoven acetate fiber and polyvinyl alcohol fiber, and the center is a cavity. At this time, the tube wall is tightly interwoven, with only tiny gaps caused by the interweaving of fibers, the surface is relatively flat, the texture is soft and easy to deform, lacks stiffness, and the cross section is easy to fall apart after shearing.

[0137] Figure 6 The figure shows a schematic diagram of the structure of an intermediate product of an embodiment of a cage-type rod before immersion and after filling with core material. The core material is smaller than the diameter of the cavity, so that after the polyvinyl alcohol fiber is dissolved, the acetate fiber shrinks to produce a thickened hollow tube wall, thereby increasing the three-dimensional degree of the smoke channel and the contact area with the smoke. After drying, the hollow cavity of the hollow cage-type round belt-shaped intermediate product has the same diameter as the core material.

[0138] Fig. 7A The figure shows a 3D schematic diagram of the braided structure of one embodiment of the cage-type rod of the present invention, from which the wavy fiber material and the spiral arrangement along the axial direction can be clearly seen; Figure 7BThe figure shows a real picture of an intermediate product (before immersion) in one embodiment of the cage-type rod of the present invention; Figure 7C The figure shows a real picture of the intermediate product of one embodiment of the cage-type bar of the present invention after soaking and drying. It can be seen from the figure that the polyvinyl alcohol fiber is dissolved in the water (playing a pore-forming role), and a hollow structure appears between the remaining acetate fibers. The residual polyvinyl alcohol adheres to the acetate fibers and the surface after drying (playing a bonding role), maintaining the stability of the hollow cage-type bar, providing stiffness, and facilitating processing and transportation. The hollow tube wall structure and the reduced central cavity increase the contact area between the smoke and the cooling structure, improve the cooling effect, and make the suction resistance stable and appropriate, reduce smoke adsorption, and ensure the smoke flavor.

[0139] Figure 8 The figure shows a real picture of the intermediate product of one embodiment of the cage-type bar rod of the present invention after soaking and drying. It can be seen from the figure that the acetate fibers are interwoven in a woven form (wave-like) to form the main body of the cage-type round belt intermediate product. The polyvinyl alcohol fibers are partially dissolved to form evenly distributed holes. The remaining polyvinyl alcohol fibers adhere to the surface and inside of the acetate fibers, providing stiffness for the hollow cage-type round belt intermediate product and preventing it from falling apart. The tortuous and complex smoke channel increases the contact area with the smoke, and the loose holes reduce adsorption and reduce the suction resistance, effectively improving the smoking experience.

[0140] Fig. 9A , Fig. 9B The figures show a radial cross-section 3D schematic diagram and a real-object picture of an embodiment of a cage-type bar. It can be seen from the figure that acetate fibers are interwoven on the cross section to form a tube wall of a certain thickness, the tube wall has evenly distributed holes, and there is a cavity in the center of the hollow cylindrical cage-type bar. Residual polyvinyl alcohol fibers can be seen attached to the surface and inside of the acetate fibers, making the cage structure stable and not deformed, and not falling apart after shearing.

[0141] Fig.10 The figure shows an axial cross-sectional view of an embodiment of the cage rod of the present invention. Figure 3 The cage-type rods are extruded through dies with different diameters to obtain rods with periodically changing outer diameters required by the design.

[0142] The porosity of the wall pores of the cage rods is calculated by using the water exclusion method to measure the volume v1 of the fiber material of the porous wall material, and by using the diameters of the inner core rod and the rods to calculate the overall volume V0 of the cage wall, and by using the pore formula (V0-V1) / V0*100%.

[0143] The filter rod hardness performance is determined according to GB / T 22838.6-2009.

[0144] The following is a further description of a specific embodiment of the cage rod used in the present invention.

[0145] Example A1

[0146] (1) Select acetate fiber (base fiber) with a fineness of 1100D and polyvinyl alcohol fiber (binder fiber) with a fineness of 1100D.

[0147] (2) A braiding machine with 32 spindles (such as a 90 series round rope single-head single-machine 32-spindle high-speed braiding machine) is used, with 16 spindles of acetate fiber and 16 spindles of polyvinyl alcohol fiber to weave into a hollow round belt-shaped intermediate product, in which the ratio of acetate fiber to polyethylene fiber is 50%:50%, and the corresponding spindle ratio is 1:1.

[0148] (3) The hollow part of the round-shaped intermediate product is filled with a core material with a diameter of 4 mm. The initial immersion temperature is 15°C, and the temperature is raised to 80°C at a uniform speed or intermittently for 40 minutes.

[0149] (4) The round-shaped intermediate product after soaking is dried at a temperature of 60° C. for 40 minutes.

[0150] (5) Through the washing process, the water-soluble polyethylene fiber is porous while retaining a certain bonding effect. According to the measurement, the diameter of the obtained hollow cage rod is 6.8 mm, the wall thickness is 1.4 mm, the wall porosity is 76%, the content ratio of acetate fiber (fiber yarn) and polyvinyl alcohol (setting material) is 70%:30%, and the hardness is 82%, which meets the requirements of the filter rod forming process.

[0151] Example A2

[0152] (1) Select acetate fiber with a fineness of 1100D and polyvinyl alcohol fiber with a fineness of 1100D, and compound the acetate fiber and polyvinyl alcohol fiber in parallel, with a total fineness of 2200D; polyvinyl alcohol fiber is paralleled, with a total fineness of 2200D.

[0153] (2) The number of weaving spindles is 32, the ratio of the number of acetate / polyvinyl alcohol composite fiber spindles to the number of polyvinyl alcohol fiber spindles after paralleling is 1:1, and a hollow round belt-shaped intermediate product is woven, in which the ratio of acetate fiber to polyvinyl alcohol fiber is 25%:75%.

[0154] (3) The hollow part of the round-shaped intermediate product is filled with a core material with a diameter of 3 mm. The initial immersion temperature is 15°C, and the temperature is raised to 80°C at a uniform speed or intermittently for 40 minutes.

[0155] (4) The round-shaped intermediate product after soaking is dried at a temperature of 60° C. for 30 min.

[0156] (5) The hollow cage-type rod obtained by measurement has a diameter of 6.8 mm, a wall thickness of 1.9 mm, a wall porosity of 75%, a content ratio of acetate fiber to polyvinyl alcohol of 65%:35%, and a hardness of 92%.

[0157] Comparative Example A: Compared with Example 2, the round belt intermediate product obtained through steps 1 and 2) is not subjected to the washing, pore-forming, bonding and shaping treatment in step 3), and its two ends are loose and cannot maintain a stable circumference. Moreover, it forms a flat structure similar to shoelaces due to compression and stretching, and is not strip-shaped and its structure is unstable in all directions. According to the hardness test method of filter rods for cigarettes, its hardness is only about 30%, and it cannot be directly used for cigarette rolling.

[0158] Example A3

[0159] (1) Select acetate staple yarn with a fineness of 1100D and polyvinyl alcohol staple yarn with a fineness of 1100D, and compound the acetate staple yarn and the polyvinyl alcohol staple yarn in parallel, with a total fineness of 2200D.

[0160] (2) The number of weaving spindles is 32, and the ratio of the number of spindles of acetate / polyvinyl alcohol composite staple yarn to the number of spindles of polyvinyl alcohol staple yarn is 1:1. The intermediate product is woven into a hollow round belt shape, wherein the ratio of acetate fiber to polyvinyl alcohol fiber is 33%:67%.

[0161] (3) The hollow part of the round band-shaped intermediate product is filled with a core material with a diameter of 3 mm. Different from Example 1, the initial immersion temperature is 20°C and the immersion time is 30 min. It is then transferred to 60°C water and ultrasonicated for 10 min. The ultrasonic frequency is 40 KHz and the power is 550 W.

[0162] (4) The round-shaped intermediate product after soaking is dried at a temperature of 60° C. for 30 min.

[0163] The obtained hollow cage-type rod has a diameter of 6.8 mm, a wall thickness of 1.9 mm, a tube wall porosity of 72%, a content ratio of acetate fiber to polyvinyl alcohol of 62%:38%, and a hardness of 93%.

[0164] Example A4

[0165] (1) Select acetate fiber with a fineness of 2200D and polyvinyl alcohol fiber with a fineness of 1100D.

[0166] (2) The number of weaving spindles is 32, the ratio of acetate fiber spindles to polyvinyl alcohol fiber spindles is 1:1, and a hollow round belt-shaped intermediate product is woven, in which the ratio of acetate fiber to polyvinyl alcohol fiber is 67%:33%.

[0167] (3) The hollow part of the round-shaped intermediate product is filled with a core material with a diameter of 4 mm. The initial immersion temperature is 20°C and the immersion time is 30 min. It is then transferred and immersed in 80°C water. After being fixed, it is flushed with running water for 20 min at a flushing speed of 2 m / s.

[0168] (4) The round-shaped intermediate product after soaking is dried at a temperature of 60° C. for 30 min.

[0169] (5) The obtained hollow cage rod has a diameter of 6.8 mm, a wall thickness of 1.4 mm, a wall porosity of 78%, a content ratio of acetate fiber to polyvinyl alcohol of 75%:25%, and a hardness of 83%.

[0170] Example A5

[0171] (1) Select acetate fiber with a fineness of 450D and polyvinyl alcohol fiber with a fineness of 450D.

[0172] (2) The number of weaving spindles is 32, the ratio of acetate fiber spindles to polyvinyl alcohol fiber spindles is 1:1, and a hollow round belt-shaped intermediate product is woven, in which the ratio of acetate fiber to polyethylene fiber is 50%:50%.

[0173] (3) The hollow part of the round-shaped middle product is filled with a core material with a diameter of 5 mm. The initial immersion temperature is 20°C and the immersion time is 10 min. It is then transferred and immersed in 60°C water. After being fixed, it is flushed with running water at a water flow rate of 1 m / s. At the same time, ultrasound is turned on with an ultrasonic frequency of 40 KHz and a power of 200 W for 15 min.

[0174] (4) The round-shaped intermediate product after soaking is dried at a temperature of 60° C. for 30 min.

[0175] (5) The obtained hollow cage rod has a diameter of 6.8 mm, a wall thickness of 0.9 mm, a wall porosity of 80%, a content ratio of acetate fiber to polyvinyl alcohol of 68%:32%, and a hardness of 79%.

[0176] Example A6

[0177] (1) Select acetate fiber with a fineness of 2200D and polyvinyl alcohol fiber with a fineness of 1100D.

[0178] (2) The number of weaving spindles is 32, the ratio of acetate fiber to polyvinyl alcohol spindles is 12:20, and the hollow round belt intermediate product is woven, wherein the ratio of acetate fiber to polyethylene fiber is 55%:45%.

[0179] (3) The hollow part of the round intermediate product is filled with a core material with a diameter of 3 mm. The initial immersion temperature is 15°C and it takes 40 minutes to heat the temperature to 80°C.

[0180] (4) The round-shaped intermediate product after soaking is dried at a temperature of 60° C. for 30 min.

[0181] (5) According to the measurement, the hollow cage rod has a diameter of 6.8 mm, a wall thickness of 1.4 mm, a wall porosity of 84%, a content ratio of acetate fiber to polyvinyl alcohol of 82%:18%, and a hardness of 58%.

[0182] Example A7

[0183] Refer to Example A2, except that: the number of spindles of acetate / polyvinyl alcohol composite fiber and polyvinyl alcohol fiber is changed to 24:8, the weight ratio of acetate fiber to polyethylene fiber of the round belt intermediate obtained by weaving is 37%:63%, and the cage rod obtained by washing and drying has a diameter of 6.8 mm, a wall thickness of 1.4 mm, a tube wall porosity of 75%, a content ratio of acetate fiber to polyvinyl alcohol of 70%:30%, and a hardness of 75%.

[0184] Example A8

[0185] Refer to Example A2, except that: the number of acetate / polyvinyl alcohol composite fiber spindles and the number of polyvinyl alcohol fiber spindles are changed to 30:2, the weight ratio of acetate fiber to polyethylene fiber of the round belt intermediate obtained by weaving is 47%:53%, and the cage rod obtained by washing and drying has a diameter of 6.8 mm, a wall thickness of 1.4 mm, a tube wall porosity of 64%, a content ratio of acetate fiber to polyvinyl alcohol of 75%:25%, and a hardness of 82%.

[0186] Embodiment A9

[0187] (1) Select acetate fiber with a fineness of 1100D and polyester hot-melt fiber with a fineness of 1100D, and compound the acetate fiber and polyester fiber in parallel, with a total fineness of 2200D as the basic fiber; the fineness of the polyvinyl alcohol fiber is 1100D.

[0188] (2) The number of weaving spindles is 32, the ratio of the number of acetate / polyester composite fiber spindles to the number of polyvinyl alcohol fiber spindles is 1:1, and a hollow round belt-shaped intermediate product is woven, wherein the content ratio of acetate fiber to polyvinyl alcohol fiber is 50%:50%, and the content ratio of acetate fiber to polyester fiber is 50%:50%.

[0189] (3) The hollow part of the round-shaped intermediate product is filled with a core material with a diameter of 3 mm and heated in an oven at a temperature of 140°C for 20 minutes. It is then washed in a water bath with an initial soaking temperature of 15°C, and the temperature is raised to 80°C at a uniform or intermittent rate for 40 minutes. It is then soaked at 80°C and flushed with running water at a fixed speed of 1 m / s for 60 minutes to ensure that all polyvinyl alcohol is dissolved and separated from the round-shaped intermediate product.

[0190] (4) Drying the soaked round-ribbon intermediate product at a temperature of 60° C. for 30 min.

[0191] (5) The hollow cage-type rod obtained by measurement has a diameter of 6.5 mm, a wall thickness of 1.5 mm, a wall porosity of 42%, a content ratio of acetate fiber to polyester fiber of 50%:50%, a polyvinyl alcohol content of 0, and a hardness of 73%.

[0192] In this embodiment, the polyester fiber is one of the basic fiber components, which plays a bonding and shaping role after melting, and serves as the basic skeleton in the cage rod; the polyvinyl alcohol fiber is completely dissolved and only plays a pore-forming role.

[0193] Embodiment A10

[0194] Referring to Example A9, the difference is that:

[0195] In step 1, 122D polyester fiber is added to 1100D acetate fiber. In step 2, the content ratio of acetate fiber to polyvinyl alcohol fiber in the hollow round ribbon intermediate product obtained is 50%:50%, and the content ratio of acetate fiber to polyester fiber is 90%:10%.

[0196] In step 3, after the same heating treatment, the initial immersion temperature in the water bath is 15°C, and the temperature is raised to 80°C at a uniform speed or intermittently for 40 minutes for washing.

[0197] The obtained cage-type rod has a diameter of 6.8 mm, a wall thickness of 1.9 mm, a wall porosity of 70%, a content ratio of acetate fiber to polyester fiber of 90%:10%, a content ratio of acetate fiber to polyvinyl alcohol of 70%:30%, and a hardness of 87%.

[0198] Embodiment A11

[0199] Referring to Example A9, the difference is that:

[0200] 1) Select polyester fiber with a fineness of 1100D and parallel it with polyvinyl alcohol fiber with a fineness of 1100D, with a total fineness of 2200D; the total fineness of the polyvinyl alcohol fiber is 1100D.

[0201] 2) The content ratio of polyester fiber to polyvinyl alcohol fiber in the round belt-shaped intermediate product obtained by weaving is 33%:67%.

[0202] 3) The hollow part of the round belt-shaped intermediate product is filled with a core material with a diameter of 3.5 mm, heated to 140°C for 30 minutes.

[0203] 4) When the initial soaking temperature in the water bath is 15°C, the temperature is raised to 80°C at a uniform speed or intermittently for 40 minutes for washing, and the temperature is kept at 80°C for 30 minutes.

[0204] 5) The round-shaped intermediate product after soaking is dried at a temperature of 90° C. for 30 minutes.

[0205] The hollow cage-type rod obtained by measurement has a diameter of 6.2 mm, a wall thickness of 1.3 mm, a wall porosity of 56%, a content ratio of polyester fiber to polyvinyl alcohol of 90%:10%, and a hardness of 95%.

[0206] In this embodiment, the polyester fiber is used as the base fiber, which plays a bonding and shaping role after heating; the polyvinyl alcohol fiber is used as the dissolving pore-forming material, and the residual polyvinyl alcohol is used as the bonding material to increase the hardness.

[0207] The 17 mm hollow cage rods of Examples A1-5 were used to replace the polylactic acid film cooling section and the filter section of the traditional cigarette in the heated cigarette cartridge, respectively. The heated cigarette test instrument built by ourselves was used to test and record the data, and compared with the performance of the polylactic acid sheet cooling section and the acetate fiber filter section. The results are shown in Table A1 and Table A2. The cage rod of the present invention has a small draw resistance and can effectively reduce the smoke temperature of the cigarette as a cooling section. The average smoke concentration is similar to that of the polylactic acid folded film cooling section, which is better than the acetate tow filter.

[0208] Table A1 Cage filter rod performance test results of Example A1-5 and performance comparison of polylactic acid membrane filter rod

[0209]

[0210]

[0211] Table A2 Cage filter rod performance test results of Examples A1-5 and comparison of performance of acetate fiber tow filter rod

[0212]

[0213] At present, the new heated cigarettes on the market mainly use the longitudinal channel structure formed by the PLA corrugated film (for related content, see the published Chinese patent CN104203015B) as the cooling section of the heated cigarette. 15mm Example A2 was added to the heated cigarette as a cooling mouthpiece. According to the national standard GB / T19609-2004, the smoke temperature and release amount of the trial cigarettes were tested using the Canadian deep smoking mode (HCI). The results are shown in Table A3.

[0214] Control group B: The cooling section of Example 2 was replaced by a PLA film with a length of 15 mm, a porosity of 72%, and a thickness of about 35 mm (the relevant content is the same as that of the published Chinese patent CN104203015B).

[0215] It can be found that, compared with the cooling section of the polylactic acid film, the nicotine release in the mainstream smoke of the heated cigarette using the cage-type filter rod of the present invention increased by about 20%, and the maximum smoke temperature remained basically the same, without significantly increasing due to the increase in smoke volume. This is mainly due to the pore structure characteristics on the wall of the cage structure, which is conducive to heat transfer and reduces the interception of smoke.

[0216] Table A3 Smoke data of cigarettes heated using cage rods and polylactic acid film cooling sections

[0217]

[0218] The above-mentioned related explanations and descriptions of the embodiments are for the convenience of those skilled in the art to understand and apply the present invention. It is obvious that those familiar with the art can easily make various modifications to these contents and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above-mentioned related explanations and descriptions of the embodiments. Improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. An aerosol generating article comprising: A smoking element, a cooling element, and an outer packaging material wrapping and connecting the smoking element and the cooling element, wherein the cooling element is located downstream of the smoke flow direction generated by the smoking element, and is characterized in that: the cooling element includes a cage-type porous rod, and the cage-type porous rod includes a wall material, and the wall material has a hollow structure formed by interlacing and interweaving fiber materials.

2. The aerosol generating article according to claim 1, characterized in that: The cage-type porous rod further comprises a hollow channel which is consistent with or parallel to the central axis of the wall material.

3. The aerosol generating article according to claim 1, characterized in that: The fiber material extends in three-dimensional space, and a plurality of pore channels are formed between different fibers.

4. The aerosol generating article according to claim 1, characterized in that: The fiber material is in a wave-like shape, and at least one fiber material extends in a spiral shape along the axis.

5. The aerosol generating article according to claim 1, characterized in that: The wall material contains pore channels, including uniform and / or non-uniform channels; optionally, the pore channels are three-dimensional, non-linear network gaps.

6. The aerosol generating article of claim 1, wherein: The cage-type porous rod is cylindrical; and / or, its outer diameter is 4-9 mm; and / or, the hollow channel is a single diameter or a variable diameter channel, and the diameter of the hollow channel is 0.1 mm-8.5 mm, preferably 0.5-4.5 mm.

7. The aerosol generating article of claim 1, wherein: The outer diameter length of the cage-type porous rod varies periodically along the axial direction, and the outer diameter varies in the range of 0.5-9 mm, preferably 2-8 mm.

8. The aerosol-generating article of claim 1, wherein: The thickness of the wall material is 0.2-4 mm, and the porosity of the wall material is 10-90%; and / or, Optionally, the hardness of the cage-type porous rod is above 30%, preferably 60%-98%, more preferably 80%-95%; and / or, Optionally, the fiber material is a yarn, comprising: at least one basic fiber, including filament, spun yarn, fancy yarn, wire; and / or at least one bonding material, the bonding material is distributed between the basic fibers and on the surface; and / or, Optionally, the content of the bonding material in the fiber material is 0.1-95%, preferably 5-75%, more preferably 15-45%; and / or, Optionally, the base fiber includes but is not limited to cellulose, regenerated cellulose, cellulose ester, cellulose ether, any derivative thereof, starch-based thermoplastic resin, cellulose acetate, polylactic acid, chitosan, alginate, polyhydroxybutyrate, poly-ε-caprolactone, polyglycolic acid, polyhydroxyalkanoate, polypropylene, polyethylene, polyvinyl alcohol, polyester, polyamide, polyurethane, polyacrylonitrile, any derivative thereof, any copolymer thereof, any one or more combinations of metals; and / or, Optionally, the bonding material comprises a material having film-forming property and bonding effect, including but not limited to one or more of cellulose acetate, polylactic acid, chitosan and its derivatives, cellulose derivatives, alginate, polyvinyl alcohol, polysaccharides, polyester, polyolefin, polyethylene glycol, and any derivatives thereof; and / or, Optionally, the bonding material is obtained by washing fibers that are soluble in a dissolving medium, and the fibers that are soluble in a dissolving medium include but are not limited to any one of acetate fibers, polylactic acid fibers, polyvinyl alcohol fibers, chitosan fibers, seaweed fibers, cellulose derivatives, and composite fibers composed of two or more of these materials; and / or, Optionally, the bonding material is obtained by washing water-soluble fibers. Preferably, the water-soluble fibers include polyvinyl alcohol fibers, seaweed fibers, and carboxymethyl cellulose fibers.

9. The aerosol-generating article of claim 1, wherein: The preparation method of the cage-type porous rod is: the filter rod material is obtained by weaving, dissolving and drying basic fibers and bonding fibers, wherein the bonding fibers are fiber-line bonding materials; the basic fibers and bonding fibers have different solubility properties in a dissolving medium, and the dissolving refers to placing the intermediate product obtained by weaving into a dissolving medium, and removing part or all of the bonding fibers by dissolving to obtain a cage-type porous rod.

10. An aerosol-generating article according to claim 9, characterized in that The preparation method of the cage-type porous rod comprises the following steps: (1) preparing at least two kinds of yarns by using a certain ratio of base fiber and binder fiber, wherein the yarns are single-component fibers or multi-component fibers; (2) Winding different yarns on a braiding machine spindle for braiding to obtain a round belt-shaped intermediate product; (3) soaking the round-shaped intermediate product obtained in step (2) in a certain dissolving medium, drying, and dissolving part of the bonding fiber to obtain a cage-type bar having a hollow structure on the tube wall and stiffness meeting the requirements, wherein the tube wall of the cage-type bar comprises basic fibers and residual bonding fiber material as a shaping material; Alternatively, the method for preparing the cage-type porous rod comprises the following steps: (1) At least two yarns are prepared by using a certain proportion of base fiber and bonding fiber, and the yarns are single-component fibers or multi-component fibers; the base fiber contains a certain amount of hot-melt fiber; the hot-melt fiber is one or a mixture of polyolefin, polyester, polyamide, polyimide, polyacetal, cellulose ester, cellulose ether, polysaccharide-based thermoplastic material, any derivative thereof, or any copolymer thereof; the softening point of the hot-melt fiber is lower than that of other fiber materials; optionally, the content of the hot-melt fiber in the base fiber is 5%-100%, preferably 10-85%; (2) Winding different yarns on a braiding machine spindle for braiding to obtain a round-belt-shaped intermediate product containing hot-melt fibers; heating until the hot-melt fibers are melted and bonded to the surface of the round-belt-shaped intermediate product for shaping; (3) washing the round band-shaped intermediate product to obtain a cage-type rod with a hollow structure and high stiffness; For the above two preparation methods: Optionally, in step (1), the multi-component fiber yarn is obtained by doubling or sizing the base fiber and / or the bonding fiber to obtain a linear material; Optionally, in step (1), the multi-component fiber yarn is obtained by composite spinning of base fiber and / or bonding fiber to obtain a linear material; Optionally, in step (1), the preferred base fiber is acetate fiber filament or staple fiber yarn; and / or, the fineness is 100-5000D; and / or, the weight percentage is 10-95%; the preferred bonding fiber is polyvinyl alcohol fiber filament or staple fiber yarn, and / or, the fineness is 100-5000D, and / or, the weight percentage is 90%-5%; Optionally, in step (2), the number of spindles of the braiding machine is 16-128, and / or the ratio of the number of spindles of different yarns is 1:15-15:1; preferably, the ratio of the number of spindles of acetate fiber yarn to that of polyvinyl alcohol fiber yarn is 1:5-5:1; optionally, the braiding machine is braided with a core rod; and / or the diameter of the core rod is 0.1-8.5 mm, and / or the core rod is made of a material with a smooth surface and a certain compressive resistance, including but not limited to polytetrafluoroethylene, silicone, wood, and metal; Optionally, in step (3), a core rod is introduced before dissolving; and / or, the diameter of the core rod is 10%-100% of the diameter of the cavity of the round band-shaped intermediate product; and / or, the core rod is made of a material with a smooth surface, solvent resistance, and high temperature resistance, including but not limited to polytetrafluoroethylene, silicone, wood, and metal; Optionally, the bonding fiber is polyvinyl alcohol fiber; and / or, in step (3), the dissolving medium is water; and / or, the round-shaped intermediate product is placed in water by one or more of the following methods: standing, flushing with running water, heating, and ultrasound to achieve partial dissolution of the bonding fiber and separation from the base fiber; and / or, the standing time in room temperature water is 0.5-30 min; and / or, during flushing with running water, the water flow rate is 1-10 m / s, the water temperature is 20-100° C., and the time is 1-30 min, and mechanical shock treatment can be added at the same time; and / or, the standing water is heated to 40-100° C. and the time is 1-60 min; and / or, the ultrasonic power is 20-60 KHz, the power is 200 W-1000 W, and the time is 1-15 min; Optionally, the drying is drying or natural drying until completely hardened; optionally, the drying temperature is 40-120° C., and the drying time is 2-60 min; Optionally, after step (3), the bonding material is impregnated between the fibers and on the fiber surface through an independent sizing process, so that the obtained cage-type rods maintain a certain cylindrical shape and structural stiffness; optionally, the bonding material includes but is not limited to cellulose acetate, polylactic acid, chitosan and its derivatives, cellulose derivatives, alginate, polyvinyl alcohol, polysaccharides, polyesters, polyolefins, polyethylene glycol, flavors and fragrances, preservatives, dyes, and any derivatives thereof.

11. The aerosol-generating article of claim 1 , wherein: It also includes a mouthpiece element, which is located downstream of the flue gas flow direction through which the flue gas cooling element passes; optionally, the mouthpiece element is made of ultra-high denier cellulose acetate tow; optionally, the ultra-high denier cellulose acetate tow has a denier greater than or equal to 10 denier.

12. The aerosol-generating article of claim 1, wherein: It also includes a hollow element, which is located upstream of the flue gas flow direction through which the cooling element passes.

13. The aerosol-generating article of claim 1, wherein: It also includes an upstream element, which is located upstream of the smoking element and can adjust the suction resistance of the aerosol generating product and block the granular smoking element; optionally, a filter rod or a hollow filter rod made of conventional acetate fiber bundle is used.

14. A method for preparing an aerosol-generating article according to any one of claims 1 to 13, characterized in that: The cage-type porous rod is encapsulated in an outer wrapping material to obtain a cigarette filter rod; the cigarette filter rod is cut into a fixed length and combined with other components to obtain the aerosol generating product; optionally, the wrapping material includes but is not limited to cellulose paper, fabric, non-woven fabric, plastic sheet, ceramic, glass; preferably, the wrapping material is cigarette forming paper or transparent film.

15. Use of an aerosol-generating article according to any one of claims 1 to 13 in cigarettes and heat-not-burn cigarettes.

Citation Information

Patent Citations

  • Material for non-combustible cigarette filter as well as preparation method and application of material

    CN116141796A

  • Hollow-out tubular cooling filter rod

    CN213307410U

  • Cooling element for cigarette

    CN213881747U

  • Particle aggregate and filter tip containing same

    CN214386058U

  • Aerosol-generating system and aerosol-generating article thereof

    CN215381427U