Preparation method and application of iron monatomic porous framework adsorbent for deep purification of uranium-containing wastewater

By preparing the iron single-atom porous frame adsorbent Fe-N-C, the high specific surface area and porous structure, the adsorption capacity and selectivity of uranium ions are significantly improved, and the problem of insufficient adsorbent performance in the prior art is solved, achieving high efficiency purification of uranium-containing wastewater.

CN119056418AActive Publication Date: 2024-12-03EAST CHINA UNIV OF TECH

Patent Information

Application Number
CN202411339390.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-03
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

The existing metal organic frame uranium adsorbents have shortcomings in adsorption capacity, selectivity and regeneration properties, and it is difficult to meet the deep purification needs of uranium-containing wastewater.

Method used

A preparation method is adopted to form the iron single-atom porous frame adsorbent Fe-N-C by combining ZIF-8 nanocrystals with tannin acid and iron nitrate, and the adsorption capacity and selection of uranium ions are significantly improved by using its high specific surface area and porous structure. sex.

Benefits of technology

The adsorption capacity under pH 6 reached 491.46 mg/g, and the removal rate reached 98.29%, which significantly improved the selectivity and purification efficiency of the adsorbent, and solved the problems of low adsorption capacity and poor selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056418A_ABST
    Figure CN119056418A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of an iron monatomic porous framework adsorbent for deep purification of uranium-containing wastewater, and relates to a preparation method and application of an adsorbent for deep purification of uranium-containing wastewater. The method aims at solving the technical problem that an existing metal organic framework uranium adsorbent is low in adsorption capacity. The method comprises the steps that ZIF-8 nanocrystals are prepared; 2, adjusting the pH value of a tannic acid solution to 8 by using potassium hydroxide, and then adding the tannic acid solution into the ZIF-8 nanocrystal solution to form a stable ZIF-8 (at) K-TA compound; 3, the ZIF-8 (at) K-TA is soaked in a ferric nitrate nonhydrate, and ZIF-8 (at) Fe-TA is obtained; and 4, calcining under dry argon flow to obtain the iron monatomic porous framework adsorbent. In uranium-containing wastewater with the pH value of 6, the adsorption capacity of the adsorbent to uranium reaches 491.46 mg / g, and the removal rate is 98.29%. The method can be used in the field of deep purification treatment of uranium-containing wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of an adsorbent for deep purification of uranium-containing wastewater. Background Art

[0002] With the development and widespread application of nuclear energy, the treatment and purification of uranium-containing wastewater has become an important environmental protection task. As a radioactive element, the presence of uranium in water bodies will pose a serious threat to the ecological environment and human health. Therefore, it is particularly important to develop efficient adsorbents for uranium-containing wastewater purification. Existing adsorbent materials still have many deficiencies in adsorption capacity, selectivity and regeneration performance, and it is difficult to meet the needs of practical applications. In recent years, metal organic framework materials (MOFs) have become a very potential adsorption material due to their advantages such as high specific surface area, porous structure and adjustable chemical properties. The Chinese patent application number CN202410469977.1 discloses a uranium adsorbent, its preparation method and application. The uranium adsorbent is a metal organic framework with a nanocage structure, and a keggin-type heteropoly acid is in situ encapsulated in the nanocage; the metal organic framework is MIL-101 (Cr), but the uranium adsorption capacity of the uranium adsorbent is only 280.60 mg / g, which is low. Summary of the invention

[0003] The present invention aims to solve the technical problem of low adsorption capacity of existing metal organic framework uranium adsorbents, and provides a preparation method and application of an iron single atom porous framework adsorbent for deep purification of uranium-containing wastewater. The adsorbent is a method for preparing an efficient iron single atom porous framework adsorbent, which is used for deep purification of uranium-containing wastewater.

[0004] The preparation method of the iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater of the present invention is carried out according to the following steps:

[0005] 1. Preparation of ZIF-8 nanocrystals;

[0006] 2. Synthesis of ZIF-8@K-TA:

[0007] Dispersing ZIF-8 nanocrystals in deionized water at a concentration of 20 to 25 g / L and stirring for 1 to 2 hours to obtain a ZIF-8 dispersion;

[0008] The tannic acid (TA) aqueous solution having a concentration of 6 to 24 m mol / L is adjusted to pH 8 with a KOH solution to obtain an alkaline tannic acid solution;

[0009] Then, the alkaline tannic acid solution was added to the ZIF-8 dispersion at a volume ratio of 3:10, stirred for 7 to 10 minutes, and then centrifuged. The solid product was washed three times with deionized water and methanol, respectively, and dried to obtain ZIF-8@K-TA.

[0010] 3. Synthesis of ZIF-8@Fe-TA: ZIF-8@K-TA was immersed in a methanol solution of ferric nitrate, stirred for 2-3 hours, centrifuged, and the solid product was washed three times with methanol and dried in vacuum to obtain ZIF-8@Fe-TA;

[0011] 4. Synthesis of Fe-NC: ZIF-8@Fe-TA was transferred into a ceramic crucible, placed in a furnace under a flow of dry argon, heated from room temperature to 900-950 °C at a heating rate of 5 °C / min and maintained for 2-3 h for annealing, and then cooled to room temperature to obtain an iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater, denoted as Fe-NC.

[0012] Furthermore, the preparation method of ZIF-8 nanocrystals is carried out according to the following steps:

[0013] (1) Weigh 2-methylimidazole (MeIM) and zinc nitrate hexahydrate at a molar ratio of 4.71:1;

[0014] (2) preparing a mixed solution of N,N-dimethylformamide (DMF), methanol (MeOH) and ethanol (EtOH) in a volume ratio of 3:1:1; dissolving the 2-methylimidazole weighed in step (1) in the mixed solution to obtain a solution A; wherein the concentration of the 2-methylimidazole in the solution A is 1.5 to 1.6 mol / L;

[0015] (3) N,N-dimethylformamide (DMF) and methanol (MeOH) are prepared into a mixed solvent in a volume ratio of 3:2; the zinc nitrate hexahydrate (Zn(NO3)2·6H2O) weighed in step (1) is dissolved in the mixed solvent to obtain a solution B; the concentration of the zinc nitrate hexahydrate in the solution B is 0.20-0.25 mol / L;

[0016] (4) adding the solution A prepared in step (2) dropwise to the solution B prepared in step (3), stirring at room temperature for 20 to 24 hours, centrifuging, washing the solid phase with methanol three times, and vacuum drying to obtain ZIF-8 nanocrystals;

[0017] Furthermore, the concentration of the KOH solution in step 2 is 6 mol / L.

[0018] Furthermore, the drying in step 2 is carried out in an oven at a temperature of 35 to 40° C. for 8 to 10 hours.

[0019] Furthermore, the vacuum drying in step three is carried out in a vacuum drying oven at a temperature of 45 to 50° C. for 10 to 12 hours.

[0020] The application of the single-atom porous framework adsorbent for deep purification of iron from uranium-containing wastewater prepared by the above method is to use the single-atom porous framework adsorbent to treat uranium-containing wastewater. The specific method is: adding the single-atom porous framework adsorbent to the uranium-containing wastewater, adjusting the pH value to 6-9; after adsorbing for 10-20 hours at a temperature of 15-55°C, separating the single-atom porous framework adsorbent to complete the treatment of the uranium-containing wastewater.

[0021] The method of the present invention first uses ZIF-8 powder to prepare ZIF-8@K-TA powder. ZIF-8, as a typical metal organic framework material, has a high specific surface area and excellent chemical stability. By combining it with tannic acid (TA), its adsorption performance can be further enhanced. Subsequently, ZIF-8@K-TA powder is soaked in a methanol solution containing ferric nitrate to prepare ZIF-8@Fe-TA powder. Ferric nitrate provides iron ions in this process, and TA coordinates with iron ions through its abundant phenolic hydroxyl groups to form a stable iron single atom dispersion system. Finally, ZIF-8@Fe-TA is converted into Fe-NC adsorbent by high-temperature heat treatment. The adsorbent not only retains the porous structure of ZIF-8, but also significantly improves its selectivity and adsorption capacity for uranium ions by introducing single iron atoms.

[0022] The iron single atom porous framework adsorbent of the present invention exhibits excellent performance in adsorbing uranium ions, especially under the condition of pH = 6, the adsorption capacity reaches 491.46 mg / g and the removal rate is 98.29%. The adsorbent prepared by the method of the present invention can effectively solve the problems of low adsorption capacity, poor selectivity and poor regeneration performance in the prior art, and can be used in the field of deep purification treatment of uranium-containing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is the microscopic morphology of ZIF-8 in Example 1;

[0024] Figure 2 This is the microscopic morphology of ZIF-8@K-TA in Example 1;

[0025] Figure 3 This is the microscopic morphology of ZIF-8@Fe-TA in Example 1;

[0026] Figure 4This is the microscopic morphology of Fe-NC-6 in Example 1;

[0027] Figure 5 This is the microscopic morphology of Fe-NC-12 in Example 2;

[0028] Figure 6 The microscopic morphology of Fe-NC-24 in Example 3;

[0029] Figure 7 This is a high-resolution transmission electron microscopy image of Fe-NC-6 in Example 1;

[0030] Figure 8 is the element distribution diagram of Fe-NC-6 in Example 1;

[0031] Fig. 9 is a graph of the specific surface area of ​​Fe-NC-6 in Example 1;

[0032] Fig.10 is a graph of the specific surface area of ​​Fe-NC-12 in Example 2;

[0033] Fig.11 is a graph of the specific surface area of ​​Fe-NC-24 in Example 3;

[0034] Fig.12 This is the effect of pH on the adsorption capacity of Fe-NC-6 in Application Example 1;

[0035] Fig.13 This is the effect of pH on Fe-NC-6 removal rate in Application Example 1;

[0036] Fig.14 This is the effect of temperature on the adsorption capacity of Fe-NC-6 in Application Example 2;

[0037] Fig.15 This is the effect of time on Fe-NC-6 removal rate in Application Example 3;

[0038] Fig.16 This is the effect of initial concentration on the adsorption capacity of Fe-NC-6 in Application Example 4;

[0039] Fig.17 This is a graph showing the effect of competing ions on the adsorption capacity of Fe-NC-6 in Application Example 5;

[0040] Fig.18 The microstructure and energy spectrum of Fe-NC-6 adsorbent after purifying uranium-containing wastewater in Application Example 1. DETAILED DESCRIPTION

[0041] Use the following examples to verify the beneficial effects of the present invention:

[0042] Example 1: The preparation method of the iron single atom porous framework adsorbent for deep purification of uranium-containing wastewater in Example 1 is carried out according to the following steps:

[0043] 1. Preparation of ZIF-8 nanocrystals:

[0044] (1) Weigh 2.626 g of 2-methylimidazole (MeIM) and 2.238 g of zinc nitrate hexahydrate (Zn(NO3)2·6H2O);

[0045] (2) 12 mL of N,N-dimethylformamide (DMF), 4 mL of methanol (MeOH) and 4 mL of ethanol (EtOH) were mixed evenly to prepare a mixed solution; and the 2-methylimidazole weighed in step (1) was dissolved in the mixed solution to obtain solution A;

[0046] (3) 18 mL of N,N-dimethylformamide (DMF) and 12 mL of methanol (MeOH) were mixed evenly to prepare a mixed solvent; then the zinc nitrate hexahydrate (Zn(NO3)2·6H2O) weighed in step (1) was dissolved in the mixed solvent to obtain a solution B;

[0047] (4) adding the solution A prepared in step (2) dropwise to the solution B prepared in step (3), stirring at room temperature for 24 hours, centrifuging, washing the solid phase with methanol three times, and drying in a vacuum oven at 40° C. for 8 hours to obtain ZIF-8 nanocrystals;

[0048] 2. Synthesis of ZIF-8@K-TA:

[0049] 200 mg of ZIF-8 nanocrystals were dispersed in 10 mL of deionized water and stirred for 2 h to obtain a ZIF-8 dispersion;

[0050] The tannic acid (TA) aqueous solution with a concentration of 6 mmol / L is adjusted to a pH value of 8 with a 6 mol / L KOH solution to obtain an alkaline tannic acid solution;

[0051] Then, 3 ml of alkaline tannic acid solution was added to 10 mL of ZIF-8 dispersion, stirred for 7 minutes, and then centrifuged. The solid product was washed three times with deionized water and methanol, respectively, and dried in an oven at 40 °C for 8 hours to obtain ZIF-8@K-TA.

[0052] 3. Synthesis of ZIF-8@Fe-TA:

[0053] 300 mg of ZIF-8@K-TA was immersed in 120 mL of 0.5 g / L methanol solution of iron (III) nitrate nonahydrate (Fe(NO3)3·9H2O), stirred for 2 hours, and centrifuged. The solid product was washed three times with methanol and dried in a vacuum oven at 50 °C for 12 hours to obtain ZIF-8@Fe-TA.

[0054] 4. Synthesis of Fe-NC: ZIF-8@Fe-TA was transferred into a ceramic crucible, placed in a furnace under a flow of dry argon, heated from room temperature to 900 °C at a heating rate of 5 °C / min and maintained for 2 h for annealing, and then cooled to room temperature to obtain an iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater, recorded as Fe-NC-6.

[0055] Example 2: This example is different from Example 1 in that the concentration of the tannic acid aqueous solution in step 2 is 12 mmol / L, and the other steps and parameters are the same as those in Example 1, and an iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater is obtained, which is recorded as Fe-NC-12.

[0056] Example 3: This example is different from Example 1 in that the concentration of the tannic acid aqueous solution in step 2 is 24 mmol / L, and the other steps and parameters are the same as those in Example 1, and an iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater is obtained, which is recorded as Fe-NC-24.

[0057] The scanning electron microscope photo of ZIF-8 prepared in step 1 in Example 1 is as follows Figure 1 As shown, from Figure 1 It can be seen that ZIF-8 is a framework cubic nanoparticle.

[0058] The scanning electron microscope photo of ZIF-8@K-TA prepared in step 2 in Example 1 is as follows: Figure 2 As shown, from Figure 2 It can be seen that TA is a pore-forming agent, and the dispersion of Fe in ZIF-8 can be controlled by adjusting the amount of TA.

[0059] The scanning electron microscope photo of ZIF-8@Fe-TA prepared in step 3 in Example 1 is as follows: Figure 3 As shown, from Figure 3 It can be seen that after the coordination of iron ions, it still remains as a framework cubic nanoparticle.

[0060] The scanning electron microscope photo of Fe-NC-6 prepared in step 4 in Example 1 is as follows: Figure 4 As shown, from Figure 4It can be seen that after high-temperature pyrolysis, the regular dodecahedral shape is maintained, and the whole is concave toward the center with protruding edges and corners, indicating that a hollow structure is formed. The hollow structure is beneficial to the transmission of Fe charges, thereby increasing the adsorption of uranium.

[0061] Example 2 The scanning electron microscope photo of Fe-NC-12 prepared in step 4 is as follows Figure 5 As shown, from Figure 5 It can be seen that after high-temperature pyrolysis, a hollow structure is formed, but tannic acid aggregates to form nanowires.

[0062] Example 3 The scanning electron microscope photo of Fe-NC-24 prepared in step 4 is as follows Figure 6 As shown, from Figure 6 It can be seen that after high-temperature pyrolysis, a hollow structure is formed, but the nanowires are aggregated in large quantities.

[0063] The Fe-NC-6 prepared in step 4 of Example 1 was subjected to high-resolution transmission electron microscopy scanning test, and the obtained crystal structure micromorphology was as follows Figure 7 The element distribution is shown in Figure 8 As shown, from Figure 7 From the microscopic scanning electron microscope image, it can be seen that Fe-NC-6 is a framework cubic nanoparticle, and the Fe element is evenly distributed in the porous framework.

[0064] The specific surface area was tested by a specific surface and porosity analyzer (BET). The specific surface area of ​​Fe-NC-6 prepared in step 4 of Example 1 is shown in the figure below: Fig. 9 As shown, from Fig. 9 It can be seen that the specific surface area of ​​Fe-NC-6 is 512.606m 2 g -1 Example 2 The specific surface area of ​​Fe-NC-12 prepared in step 4 is shown in FIG. Fig.10 As shown, from Fig.10 It can be seen that the specific surface area of ​​Fe-NC-12 is 512.672m 2 g -1 Example 3 The specific surface area of ​​Fe-NC-24 prepared in step 4 is shown in FIG. Fig.11 As shown, from Fig.11 It can be seen that the specific surface area of ​​Fe-NC-24 is 435.808m 2 g -1 .

[0065] Application Example 1: Add 0.005 g of Fe-NC adsorbent to each of a series of conical flasks, and then add 50 mL of uranium-containing solution; the UO2 in the uranium-containing solution 2+The concentration was 50 ppm, and the pH values ​​of the solutions were adjusted to 2, 3, 4, 5, 6, 7, 8, and 9, respectively. The conical flask was placed in a constant temperature shaker, the shaking speed was set to 180 rpm, and the adsorption experiment was carried out at room temperature. After 24 hours of adsorption, samples were taken to determine the uranium ion concentration in the supernatant, and the adsorption capacity and removal rate were calculated.

[0066] The adsorption capacity of Fe-NC-6, Fe-NC-12 and Fe-NC-24 varies with pH value. Fig.12 As shown in the figure, Fe-NC-6, Fe-NC-12 and Fe-NC-24 have a significant influence on the UO2 2+ The removal rate changes with pH value as shown in Fig.13 As shown, from Fig.12 and Fig.13 It can be seen that under the strong acidic condition of pH = 2, the adsorption capacity and removal rate of Fe-NC are very low, but with the increase of pH value, the adsorption performance gradually increases and reaches the best performance at pH = 6. The adsorption capacity of Fe-NC-6 is 491.46 mg g -1 , the removal rate was 98.29%; the adsorption capacity of Fe-NC-12 was 480.16 mg g -1 , the removal rate was 96.03%; the adsorption capacity of Fe-NC-24 was 462.41 mg g -1 The removal rate was 92.48%, and then it showed a downward trend with the increase of pH. Fig.12 and 13 It can be seen that the optimal pH value is 6-9.

[0067] Application Example 2: Add 0.005 g of Fe-NC adsorbent to a series of conical flasks, and then add 50 mL of uranium-containing solution, where UO2 2+ The concentration was 60ppm, and the pH value of the solution was adjusted to 6; the conical flask was placed in a constant temperature shaker, the shaking speed was set to 180rpm, and the adsorption experiments were carried out at temperatures of 15℃, 25℃, 35℃, 45℃ and 55℃, respectively. After 24h of adsorption, the uranium ion concentration in the supernatant was measured by sampling, and the adsorption capacity and removal rate were calculated.

[0068] The adsorption capacity of Fe-NC-6, Fe-NC-12 and Fe-NC-24 varies with temperature. Fig.14 As shown, from Fig.14 It can be seen that in the temperature range of 15 to 55 ° C, Fe-NC-6, Fe-NC-12 and Fe-NC-24 adsorb UO2 2+ The adsorption amount of Fe-NC-6 increased with the increase of temperature, from 483.55 mg g-1 Increased to 592.68 mg g -1 ; Fe-NC-12 is 449.55 mg g -1 Increased to 590.28 mg g -1 ; Fe-NC-24 is 420.15 mg g -1 Increased to 583.88 mg g -1 , proving that increasing temperature is beneficial to the adsorption of uranyl ions.

[0069] Application Example 3: Add 0.005 g of Fe-NC adsorbent to each of a series of conical flasks, and then add 50 mL of uranium-containing solution; the UO2 in the uranium-containing solution 2+ The concentration was 50ppm, and the pH value of the solution was adjusted to 6; the conical flask was placed in a constant temperature shaker, the shaking speed was set to 180rpm, and the adsorption experiments were carried out at a temperature of 25°C. The adsorption time was 0 to 22h, and samples were taken every hour to determine the uranium ion concentration in the supernatant, and the adsorption capacity and removal rate were calculated.

[0070] Fe-NC-6, Fe-NC-12 and Fe-NC-24 for UO2 2+ Uranium-containing solution UO2 2+ The removal rate changes with time as shown in Fig.15 As shown, from Fig.15 It can be seen that the Fe-NC adsorbent was able to remove 60% of UO2 within the first 6 hours. 2+ As the adsorption time increased, the removal performance gradually increased and reached adsorption equilibrium after 20 hours. The removal rate of Fe-NC-6 was 98.29%; the removal rate of Fe-NC-12 was 96.03%; and the removal rate of Fe-NC-24 was 92.48%.

[0071] Application Example 4: Add 0.005 g of Fe-NC adsorbent to each of a series of conical flasks, and then add 50 mL of uranium-containing solution; the UO2 in the uranium-containing solution 2+ The initial concentration was 30-90 ppm, and the pH value of the solution was adjusted to 6; the conical flask was placed in a constant temperature shaker, the shaking speed was set to 180 rpm, and the adsorption experiments were carried out at a temperature of 25°C. After 24 hours of adsorption, the uranium ion concentration in the supernatant was measured by sampling, and the adsorption capacity and removal rate were calculated.

[0072] The effect of initial concentration on the adsorption capacity of Fe-NC-6, Fe-NC-12 and Fe-NC-24 is shown in the figure Fig.16 shown; from Fig.16It can be seen that at the initial concentrations of 30ppm, 40ppm, and 50ppm, Fe-NC-6, Fe-NC-12, and Fe-NC-24 can remove most of the UO2 2+ With the increase of initial concentration, the adsorption capacity also increased and reached the maximum adsorption capacity at a concentration of 90 ppm. The adsorption capacity of Fe-NC-6 was 590.42 mg g -1 ; The adsorption capacity of Fe-NC-12 is 549.02 mg g -1 ; The adsorption capacity of Fe-NC-24 is 516.92 mg g -1 .

[0073] Application Example 5: Add 0.005 g of Fe-NC-6 adsorbent to a series of conical flasks, and then add 50 mL of uranium-containing solution; the UO2 in the uranium-containing solution 2+ The concentration was 50ppm, and the pH value of the solution was adjusted to 6, and then 0.1mol / L of competitive ions were added; the competitive ions were Mg 2+ , K + 、Na + , Ca 2+ , Cl - 、NO3 - 、SO4 2- 、CO3 2- , place the conical flask in a constant temperature shaker, set the shaking speed to 180rpm, and conduct the adsorption experiment at room temperature. After 24 hours of adsorption, take samples to measure the uranium ion concentration in the supernatant, and calculate the adsorption capacity and removal rate. The effect of competing ions on the adsorption capacity of Fe-NC-6 is shown in the figure Fig.17 As shown, from Fig.17 It can be seen that in uranium-containing wastewater with competing ions, Fe-NC-6 has a significant effect on UO2 2+ It still has high removal ability and strong anti-interference ability.

[0074] The Fe-NC-6 prepared in Example 1 was subjected to a microscopic electron microscope scanning test after being subjected to purification of uranium-containing wastewater in Application Example 1. The morphology of the Fe-NC-6 and uranyl morphology after adsorption and the corresponding energy spectrum analysis diagram were obtained, as shown in FIG. Fig.18 As shown, from Fig.18 From the microscopic scanning electron microscope image, it can be seen that the Fe-NC-6 framework cubic nanoparticles remain intact after purifying the uranium-containing wastewater, and its original structure is not destroyed during the adsorption process. In addition, new sheet-like crystal morphology grows vertically on the surface of Fe-NC-6. The elemental spectrum image shows that it is composed of O and U elements gathered together to form a sheet, which is a hydrate of uranyl. The element content of the energy spectrum analysis is shown in Table 1.

[0075] Table 1 Element content of Fe-NC-6 after adsorption

[0076]

[0077] The Fe-NC adsorbents prepared in Examples 1, 2, and 3 have a high specific surface area and a porous structure, which significantly improves the adsorption capacity for uranium ions and has a fast adsorption rate. The uniform distribution of single iron atoms in the framework enhances the selectivity and stability of the adsorbent, significantly improving the efficiency and service life of uranium-containing wastewater purification.

Claims

1. A method for preparing an iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater, characterized in that The method proceeds as follows:

1. Preparation of ZIF-8 nanocrystals; 2. Synthesis of ZIF-8@K-TA: Disperse ZIF-8 nanocrystals in deionized water at a concentration of 20-25 g / L and stir for 1-2 h to obtain a ZIF-8 dispersion; adjust a tannic acid aqueous solution at a concentration of 6-24 m mol / L to pH 8 with a KOH solution to obtain an alkaline tannic acid solution; then add the alkaline tannic acid solution to the ZIF-8 dispersion at a volume ratio of 3:10, stir for 7-10 minutes, and then centrifuge, wash the solid product three times with deionized water and methanol, respectively, and dry to obtain ZIF-8@K-TA; 3. Synthesis of ZIF-8@Fe-TA: ZIF-8@K-TA was immersed in a methanol solution of ferric nitrate, stirred for 2-3 hours, centrifuged, and the solid product was washed three times with methanol and dried in vacuum to obtain ZIF-8@Fe-TA; 4. Synthesis of Fe-NC: ZIF-8@Fe-TA was transferred into a ceramic crucible, placed in a furnace under a flow of dry argon, heated from room temperature to 900-950 °C at a heating rate of 5 °C / min and maintained for 2-3 h for annealing, and then cooled to room temperature to obtain an iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater, denoted as Fe-NC.

2. The method for preparing an iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater according to claim 1, characterized in that: The preparation method of ZIF-8 nanocrystals in step 1 is carried out according to the following steps: (1) Weigh 2-methylimidazole and zinc nitrate hexahydrate at a molar ratio of 2-methylimidazole to zinc nitrate hexahydrate of 4.71:1; (2) preparing a mixed solution of N,N-dimethylformamide, methanol and ethanol in a volume ratio of 3:1:1; dissolving the 2-methylimidazole weighed in step (1) in the mixed solution to obtain a solution A; wherein the concentration of the 2-methylimidazole in the solution A is 1.5 to 1.6 mol / L; (3) preparing a mixed solvent of N,N-dimethylformamide and methanol in a volume ratio of 3:2; dissolving the zinc nitrate hexahydrate weighed in step (1) in the mixed solvent to obtain a solution B; the concentration of the zinc nitrate hexahydrate in the solution B is 0.20 to 0.25 mol / L; (4) adding the solution A prepared in step (2) dropwise to the solution B prepared in step (3), stirring at room temperature for 20 to 24 hours, centrifuging, washing the solid phase with methanol three times, and vacuum drying to obtain ZIF-8 nanocrystals; 3. A method for preparing an iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater according to claim 1 or 2, characterized in that: The concentration of the KOH solution described in step 2 is 6 mol / L.

4. A method for preparing an iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater according to claim 1 or 2, characterized in that: The drying described in step 2 is carried out in an oven at a temperature of 35 to 40° C. for 8 to 10 hours.

5. The method for preparing an iron single-atom porous framework adsorbent for deep purification of uranium-containing wastewater according to claim 1 or 2, characterized in that: The vacuum drying described in step 3 is to dry in a vacuum drying oven at a temperature of 45 to 50° C. for 10 to 12 hours.

6. Application of a single-atom porous framework adsorbent for deep purification of iron from uranium-containing wastewater prepared by the method of claim 1, characterized in that This application is to use single-atom porous framework adsorbents to treat uranium-containing wastewater.

7. The use of a single-atom porous framework adsorbent for deep purification of iron from uranium-containing wastewater according to claim 6, characterized in that The method for treating uranium-containing wastewater using a single-atom porous framework adsorbent is as follows: adding the single-atom porous framework adsorbent to the uranium-containing wastewater and adjusting the pH value to 6 to 9; after adsorbing for 10 to 20 hours at a temperature of 15 to 55°C, the single-atom porous framework adsorbent is separated to complete the treatment of the uranium-containing wastewater.

Citation Information

Patent Citations

  • Preparation method of nano-enzyme hydrogel sheet and application of nano-enzyme hydrogel sheet in band-aid

    CN113975459A

  • Preparation and application of metal organic framework composite material for radionuclide treatment

    CN114917877A

  • Preparation and application of monatomic Ga catalyst for high-selectivity removal of UO2 < 2 + >

    CN116139905A

  • Preparation method and application of carbon defect type iron monatomic catalyst for efficiently degrading organic dye

    CN117943089A

  • Atomically dispersed metal catalysts and applications thereof

    US20210316289A1

Cited By

  • ZIF-8 composite iron monatomic doped porous carbon nitride material, preparation method thereof and application of ZIF-8 composite iron monatomic doped porous carbon nitride material in extraction of uranium from seawater

    CN121402046A