Glass fiber based aluminophosphate molecular sieve moisture absorbent as well as preparation method and application thereof
By using glass fiber-based aluminum phosphate molecular sieve as a moisture absorber, combined with the treatment of aqueous composite glue and dispersant, the problems of insufficient adsorption performance and high desorption energy consumption in low humidity are solved, and low-temperature desorption and high efficiency are achieved Dehumidification reduces the energy consumption of lithium-ion battery production.
Patent Information
- Application Number
- CN202411068589.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-12-03
AI Technical Summary
The absorbents of traditional dehumidification wheels lack adsorption performance under low humidity and have high energy consumption for desorption, resulting in a high proportion of energy consumption in lithium-ion battery production, increasing production costs.
Using glass fiber-based aluminum phosphate molecular sieve as moisture absorbent, by adding aqueous composite glue and dispersant to the dispersed slurry of aluminum phosphate molecular sieve, the glass fiber paper is impregnated and sintered to form a honeycomb corrugated rotor block, reducing adsorbed water molecules The mass transfer resistance of the mass transfer rate of the adsorption and desorption process can be improved, and the cycle stability can be improved through the procedure of heating and sintering.
The effects of low-temperature desorption, low energy consumption, and deep dehumidification are achieved, which significantly improves moisture absorption and cycle stability, and reduces the energy consumption of lithium-ion battery production.
Smart Images

Figure CN119056426A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rotary dehumidification, and in particular to a glass fiber-based aluminum phosphate molecular sieve moisture absorbent and a preparation method and application thereof. Background Art
[0002] In order to achieve the development strategy of "carbon peak and carbon neutrality", actively developing new technologies for energy conservation and emission reduction and developing new products have become the focus of current scientific researchers. Adsorption dehumidification wheels are widely used in batteries, medicine, papermaking, chemical fiber, textile, pharmaceutical, food and other fields that require a low humidity environment. In particular, the production of lithium-ion batteries for new energy vehicles requires a deep dehumidification working environment. The desiccant used in traditional dehumidification wheels includes silica gel, molecular sieves, etc., which can be used for deep dehumidification. However, silica gel has problems such as small adsorption capacity at low humidity and high desorption temperature of 150°C; and although molecular sieves have good adsorption performance at low humidity, the desorption temperature is as high as 250°C. According to preliminary analysis of the lithium-ion battery industry, the energy consumption for dehumidification accounts for 40% of the energy consumption required for its entire production line, which greatly increases the production cost of lithium-ion batteries. Therefore, under the background of energy conservation, consumption reduction and emission reduction, it is of theoretical guiding significance and practical application value to develop a desiccant with high hygroscopicity, low desorption energy consumption and low desorption temperature at low humidity, and combine it with the wheel process to make a low-temperature desorption dehumidification wheel.
[0003] Aluminophosphate molecular sieves (AIPOs) have a regular pore structure, a unique S-type water vapor adsorption isotherm, a low desorption temperature of 50 to 90 ° C, and high hydrothermal stability. As commercial products, they have been used in adsorption heat pumps, such as Mitsubishi's AQSOA-Z01, Z02, and Z05. However, its adsorption capacity at low humidity, such as 15% RH, is low, only 20%. With the emergence and use of synthesis processes and new templates (structure directing agents), various topological AIPOs such as LTA structure AlPO-42 and SFO structure EMM-8 have been prepared, and their notable feature is high hygroscopicity at low humidity. The Chinese invention patent with application number 202010346128.9 also discloses a method for preparing an organic hybrid -CLO structure aluminum phosphate molecular sieve, which has a -CLO type topological structure confirmed by the International Zeolite Association, and has better water resistance, higher specific surface area and micropore volume than unhybridized isomorphs. But so far, there are few reports on the application of AIPOs molecular sieves in dehumidification wheels.
[0004] Powdered aluminum phosphate molecular sieve has a series of problems such as poor heat and mass transfer performance, and is not suitable for use in dehumidification wheels. Loading it is the key to solving these problems. Usually, the carrier of the powder material is a porous substrate, including inorganic porous substrates and organic porous substrates; inorganic substrates such as porous ceramics, porous glass, sepiolite, cordierite, etc.; organic porous substrates such as polyurethane sponges, melamine sponges, etc. The former mainly has deficiencies such as low porosity and high density. When aluminum phosphate molecular sieve is compounded with it, the adsorbent loading rate is low, only 15%; and the latter is a polymer with poor heat resistance. When used for a long time under the cycle of room temperature adsorption and high temperature desorption, the polymer is easy to age and fall off, resulting in problems such as adsorbent powder loss and poor cycle stability. Summary of the invention
[0005] In order to overcome the defects of the prior art mentioned above, the technical problem to be solved by the present invention is to provide a glass fiber-based aluminum phosphate molecular sieve desiccant with low desorption energy consumption and high water adsorption capacity, and a preparation method and application thereof.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a glass fiber-based aluminum phosphate molecular sieve moisture absorbent, comprising the following steps:
[0007] S1: under stirring, adding aluminum phosphate molecular sieve and aqueous composite glue into deionized water to obtain a mixed solution, and then adding a dispersant into the mixed solution to form an aluminum phosphate molecular sieve dispersed slurry;
[0008] S2: Dipping glass fiber paper in the aluminum phosphate molecular sieve dispersion slurry, taking it out and drying it after it is completely soaked, and then sintering it to obtain the glass fiber-based aluminum phosphate molecular sieve.
[0009] Another technical solution adopted by the present invention is: a glass fiber-based aluminum phosphate molecular sieve desiccant is prepared by the above-mentioned preparation method of the glass fiber-based aluminum phosphate molecular sieve desiccant.
[0010] Another technical solution adopted by the present invention is: use of the above-mentioned glass fiber-based aluminum phosphate molecular sieve desiccant in the preparation of a low-temperature desorption dehumidification wheel.
[0011] The beneficial effects of the present invention are as follows: the preparation method of the glass fiber-based aluminum phosphate molecular sieve desiccant of the present invention selects aluminum phosphate molecular sieve as the adsorbent, and has the advantages of high dehumidification efficiency, low operating energy consumption and good cycle stability. Glass fiber paper is selected as the substrate, and together with the aluminum phosphate molecular sieve, it can be processed into a honeycomb corrugated wheel block, which can reduce the mass transfer resistance of the adsorbate water molecules in the honeycomb channel and increase the mass transfer rate of the adsorbent in the adsorption and desorption process. At the same time, an aqueous composite glue is added to the aluminum phosphate molecular sieve dispersion slurry, and its adhesion properties are utilized to make the aluminum phosphate molecular sieve highly loaded on the surface of the substrate, and it is not easy to fall off during the processing. The preparation process is simple and green and environmentally friendly. The prepared glass fiber-based aluminum phosphate molecular sieve desiccant has the characteristics of large moisture absorption, low-temperature desorption and stable performance, and can realize the deep dehumidification of the low-temperature desorption dehumidification wheel. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 The water vapor adsorption and desorption isotherms of the glass fiber-based aluminum phosphate molecular sieve in Example 1 of the present invention and the EMM-8 activated powder in the comparative example are shown;
[0013] Figure 2 Shown are X-ray diffraction (XRD) spectra of the glass fiber-based aluminum phosphate molecular sieve in Example 1 of the present invention and the EMM-8 activated powder in the comparative example;
[0014] Figure 3 Shown are N2 adsorption-desorption curves and pore size and distribution curves of the glass fiber-based aluminum phosphate molecular sieve in Example 1 of the present invention and the EMM-8 activated powder in the comparative example;
[0015] Figure 4 The differential thermal gravimetric loss (DTG) curves of the glass fiber-based aluminum phosphate molecular sieve in Example 1 of the present invention and the EMM-8 activated powder in the comparative example are shown;
[0016] Figure 5 The graph shows the stability test results of 15 water vapor adsorption-desorption cycles of the glass fiber-based aluminum phosphate molecular sieve in Example 1 of the present invention and the EMM-8 activated powder in the comparative example. DETAILED DESCRIPTION
[0017] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in combination with the implementation modes and the accompanying drawings.
[0018] A method for preparing a glass fiber-based aluminum phosphate molecular sieve moisture absorbent comprises the following steps:
[0019] S1: under stirring, adding aluminum phosphate molecular sieve and aqueous composite glue into deionized water to obtain a mixed solution, and then adding a dispersant into the mixed solution to form an aluminum phosphate molecular sieve dispersed slurry;
[0020] S2: Dipping glass fiber paper in the aluminum phosphate molecular sieve dispersion slurry, taking it out and drying it after it is completely soaked, and then sintering it to obtain the glass fiber-based aluminum phosphate molecular sieve.
[0021] From the above description, it can be seen that the beneficial effects of the present invention are: glass fiber paper has a thickness of 19 to 30 g / m 2 With low weight and excellent processability, it can form a honeycomb corrugated structure. It also has excellent heat resistance and durability, and can withstand high temperatures above 600°C and solvent corrosion. It has become an ideal choice for the substrate of dehumidification wheels. Due to the low density and high porosity of glass fiber paper, the loading rate of aluminum phosphate molecular sieve is as high as 60% or more when glass fiber paper is used as the substrate.
[0022] The present invention uses aluminum phosphate molecular sieve as a desiccant. The aluminum phosphate molecular sieve has a relatively high moisture absorption rate at low humidity and a low desorption temperature. When used as a rotary dehumidifier, the aluminum phosphate molecular sieve has low operating energy consumption, and the aluminum phosphate molecular sieve is resistant to a high temperature of 700°C and has good stability. Secondly, the aluminum phosphate molecular sieve dispersion slurry is selected as the impregnation liquid, and the glass fiber paper is immersed in the aluminum phosphate molecular sieve dispersion slurry. This step utilizes the characteristics of low density, high porosity and high wettability of the glass fiber paper to achieve uniform dispersion of the aluminum phosphate molecular sieve on the substrate, and the aluminum phosphate molecular sieve powder is highly loaded on it.
[0023] The preparation method of the present invention reduces the gaps between aluminum phosphate molecular sieve particles and between the molecular sieve and the substrate, resulting in close contact, thereby reducing the heat transfer resistance of the desiccant adsorption and desorption process as much as possible. Secondly, glass fiber paper is used as the substrate, which can be processed into a honeycomb corrugated runner block together with the aluminum phosphate molecular sieve, which can greatly reduce the mass transfer resistance of the adsorbent water molecules in the honeycomb channel, and the pressure drop is small, thereby increasing the mass transfer rate of the adsorbent in the adsorption and desorption process.
[0024] In order to solve the problem of low interface effect between substrate and aluminum phosphate molecular sieve, the present invention adopts water-based composite glue, and utilizes its adhesion performance to make the hygroscopic agent highly loaded on the substrate surface and not easy to fall off. At the same time, a dispersant is added, which is conducive to the uniform dispersion of aluminum phosphate molecular sieve in the dispersion slurry, without precipitation, and is convenient for the dip coating of the dispersion slurry to the substrate. Finally, sintering is carried out to remove the organic components in the substrate and the dispersion slurry, and the cyclic stability of the aluminum phosphate molecular sieve is improved. The glass fiber-based aluminum phosphate molecular sieve hygroscopic agent obtained based on the above design concept has the advantages of low desorption energy consumption, high water adsorption capacity, low temperature desorption, and high cyclic stability.
[0025] Furthermore, the aluminum phosphate molecular sieve is an aluminum phosphate series with a topological structure.
[0026] Furthermore, the aluminum phosphate molecular sieve includes any one of SAPO-34 with a CHA structure, AlPO4-5 with an AFI structure, AlPO-42 with a LTA structure, EMM-8 with a SFO structure, and derivatives thereof.
[0027] Furthermore, the derivative is an aluminum phosphate molecular sieve in which Si, Fe, Co and Ni partially replace the above structure.
[0028] Preferably, the aluminum phosphate molecular sieve is EMM-8 with an SFO structure.
[0029] From the above description, it can be seen that considering the adsorption capacity of the aluminum phosphate molecular sieve itself at low humidity, the desorption temperature and the price of raw materials, EMM-8 with SFO structure is selected as the aluminum phosphate molecular sieve.
[0030] Furthermore, the water-based composite adhesive includes inorganic adhesive and organic adhesive.
[0031] From the above description, it can be seen that the inorganic glue can provide the aluminum phosphate molecular sieve and the substrate with structural strength and heat resistance of the product after high-temperature sintering, making them integrated; while the organic glue provides the initial adhesion between the aluminum phosphate molecular sieve and the substrate.
[0032] Furthermore, the inorganic adhesive accounts for 50 to 90 wt % of the weight of the water-based composite adhesive.
[0033] Preferably, the inorganic adhesive accounts for 65-85 wt % of the weight of the water-based composite adhesive.
[0034] From the above description, it can be seen that in the water-based composite adhesive, if the content of inorganic adhesive is too little, the slurry viscosity is low, and the debt ratio of aluminum phosphate molecular sieve to the substrate is low; if the content of inorganic adhesive is too much, the moisture absorption rate of the hygroscopic agent is reduced because it does not have hygroscopic properties. Therefore, the inorganic adhesive is controlled to account for 50-90wt% of the weight of the water-based composite adhesive.
[0035] Furthermore, the inorganic colloid includes at least one of aluminum sol, silica sol, silica-alumina sol, titanium sol and zirconium sol.
[0036] Furthermore, the organic glue includes at least one of polyvinyl alcohol glue, polyacrylate emulsion, epoxy resin emulsion, water-based polyurethane dispersion and water-based silicone dispersion.
[0037] Preferably, the inorganic glue is silica sol or alumina sol, and the organic glue is polyvinyl alcohol or water-based silicone resin.
[0038] From the above description, it can be seen that when the inorganic glue is silica sol or aluminum sol, and the organic glue is polyvinyl alcohol or water-based silicone resin, the inorganic glue and the organic glue have good compatibility, the compounded water-based composite glue is tightly bonded to the glass fiber substrate, and has good high-temperature sintering performance, so that the molecular sieve is tightly bonded to the substrate.
[0039] Furthermore, the dispersant includes at least one of sodium polyacrylate, polyvinyl pyrrolidone, sodium gluconate and sodium hexametaphosphate.
[0040] Preferably, the dispersant is sodium polyacrylate.
[0041] From the above description, it can be seen that the amount of sodium polyacrylate added to the dispersion is small and the price is low.
[0042] Furthermore, the dispersant is 0.5 to 5 wt % of the mixed solution.
[0043] Preferably, the dispersant is 1 to 3 wt % of the mixed solution.
[0044] From the above description, it can be seen that if the dispersant content is too little, the slurry dispersion effect is poor; if the dispersant content is too much, the slurry viscosity is high, making the aluminum phosphate molecular sieve unevenly dispersed in the substrate. Therefore, the dispersion is controlled to account for 0.5-5wt% of the weight of the aluminum phosphate molecular sieve dispersion slurry.
[0045] Furthermore, in terms of solid content, the mixed solution includes: 50-80 wt % of aluminum phosphate molecular sieve and 20-50 wt % of water-based composite adhesive.
[0046] Preferably, in terms of solid content, the mixed solution includes: 60-75wt% aluminum phosphate molecular sieve, 25-40wt% water-based composite glue. The aluminum phosphate molecular sieve can be 62, 64, 68, 70, 73wt%, and the water-based composite glue can be 28, 30, 34, 36, 38wt%.
[0047] From the above description, it can be seen that in the aluminum phosphate molecular sieve dispersed slurry, the aluminum phosphate molecular sieve content is too little, the loading rate in the substrate is low, and the product moisture absorption rate is low; the aluminum phosphate molecular sieve content is too much, the interaction between the substrate and the molecular sieve is weak, and it is easy to fall off; the composite glue content is too little, and it is easy to fall off; the composite glue content is too much, and the loading rate of the aluminum phosphate molecular sieve is low; therefore, the aluminum phosphate molecular sieve dispersed slurry is controlled to include 60-75wt% of aluminum phosphate molecular sieve and 25-40wt% of aqueous composite glue.
[0048] Furthermore, programmed temperature is adopted during sintering, the temperature of the first stage of programmed temperature increase is 120-300°C, and the temperature of the second stage is 450-600°C.
[0049] Preferably, the temperature of the first stage of the programmed temperature rise is 150-280° C., and the temperature of the second stage is 450-550° C. The temperature of the first stage can be 160, 180, 200, 220, 240° C., and the temperature of the second stage can be 470, 490, 510, 530° C.
[0050] From the above description, it can be seen that the purpose of the programmed temperature sintering of the present invention is to remove organic impurities in the substrate and slurry, and increase the bonding strength between the inorganic glue and the substrate and the adsorbent. Therefore, the programmed temperature is divided into two stages. The first stage is to carbonize the organic components. If the carbonization temperature of the first stage is too high, it is easy to form a flame that damages the substrate and the pore structure of the adsorbent. If the carbonization temperature is low, the organic matter is not completely carbonized. Therefore, the temperature of the first stage is controlled to be 120-300°C; the second stage is to dehydrate the inorganic glue to form an oxide coating that combines with the substrate and the adsorbent, thereby improving the structural strength and heat resistance. If the sintering temperature in the second stage is too high, it is also easy to damage the substrate and cause the adsorbent structure to collapse. The programmed temperature can also minimize the deformation of the block adsorbent formed by the combination of the substrate and the adsorbent during the heating process, and prevent the adsorbent from cracking during dehydration and decomposition of organic matter.
[0051] Another technical solution adopted by the present invention is: a glass fiber-based aluminum phosphate molecular sieve desiccant is prepared by the above-mentioned preparation method of the glass fiber-based aluminum phosphate molecular sieve desiccant.
[0052] Another technical solution adopted by the present invention is: use of the above-mentioned glass fiber-based aluminum phosphate molecular sieve desiccant in the preparation of a low-temperature desorption dehumidification wheel.
[0053] The raw materials used in the following examples include: aluminum sol: CAS1344-28-1; silica sol: CAS 112926-00-8; polyvinyl alcohol glue: model PVA-10-1L; water-based silicone dispersion: Dow Corning DC51; sodium polyacrylate: CAS9003-04-7.
[0054] Since a template agent is added to the aluminum phosphate molecular sieve during the synthesis process, and the presence of the template agent will seriously affect the hygroscopicity and stability of the adsorbent, it is necessary to remove the template agent by activation. The preparation method of the activated aluminum phosphate molecular sieve powder in the following embodiment is: the aluminum phosphate molecular sieve powder is placed in a crucible, transferred to a programmed temperature muffle furnace, heated to 500°C at a rate of 10°C / min, and kept at a constant temperature for 12 hours to remove the template agent and other impurities, and then naturally cooled to room temperature to obtain the activated aluminum phosphate molecular sieve powder.
[0055] Embodiment 1 of the present invention is: a method for preparing a glass fiber-based aluminum phosphate molecular sieve moisture absorbent, the steps are as follows:
[0056] S1: Under stirring, according to the solid content mass percentage of EMM-8 / organic glue / inorganic glue = 70 / 7.5 / 22.5, 7g EMM-8 activated powder, 7.5g 10wt% PVA (polyvinyl alcohol) glue, and 11.25g 20wt% aluminum sol were weighed in sequence and added into 80mL deionized water, and then 6.67g 30wt% sodium polyacrylate dispersant was added, and stirring was continued until a uniformly dispersed aluminum phosphate molecular sieve dispersion slurry was formed.
[0057] S2: Take a glass fiber paper with a size of 10×10 cm (weight 25g / m 2 ), immersed in the aluminum phosphate molecular sieve dispersion slurry, after being completely wetted, taken out and dried, and then transferred to a muffle furnace for programmed temperature sintering. The sintering process is: in the first stage, the temperature is increased to 250°C at a heating rate of 10°C / min and kept at a constant temperature for 2h; in the second stage, the temperature is increased to 500°C at a heating rate of 10°C / mi, kept at a constant temperature for 4h, and then naturally cooled to room temperature to obtain a glass fiber-based aluminum phosphate molecular sieve.
[0058] Embodiment 2 of the present invention is:
[0059] The only difference between Example 2 and Example 1 is that the solid content mass ratio of EMM-8 / organic glue / inorganic glue is 60 / 10 / 30.
[0060] Embodiment 3 of the present invention is:
[0061] The only difference between Example 3 and Example 1 is that the solid content mass ratio of EMM-8 / organic glue / inorganic glue is 75 / 6.25 / 18.75.
[0062] Embodiment 4 of the present invention is:
[0063] The only difference between Example 4 and Example 1 is that the solid content mass ratio of EMM-8 / organic glue / inorganic glue is 70 / 10.5 / 19.5.
[0064] Embodiment 5 of the present invention is:
[0065] The only difference between Example 5 and Example 1 is that the solid content mass ratio of EMM-8 / organic glue / inorganic glue is 70 / 4.5 / 25.5.
[0066] Embodiment 6 of the present invention is:
[0067] The only difference between Example 6 and Example 1 is that 3.34 g of 30 wt % sodium polyacrylate dispersant is added to S1.
[0068] Embodiment 7 of the present invention is:
[0069] The only difference between Example 7 and Example 1 is that 10 g of 30 wt % sodium polyacrylate dispersant is added to S1.
[0070] Embodiment 8 of the present invention is:
[0071] The only difference between Example 8 and Example 1 is that the sintering process is: in the first stage, the temperature is increased to 150°C at a heating rate of 10°C / min and kept at a constant temperature for 2 hours; in the second stage, the temperature is increased to 500°C at a heating rate of 10°C / min and kept at a constant temperature for 4 hours.
[0072] Embodiment 9 of the present invention is:
[0073] The only difference between Example 9 and Example 1 is that the sintering process is: in the first stage, the temperature is increased to 280°C at a heating rate of 10°C / min and kept at a constant temperature for 2 hours; in the second stage, the temperature is increased to 500°C at a heating rate of 10°C / min and kept at a constant temperature for 4 hours.
[0074] Embodiment 10 of the present invention is:
[0075] The only difference between Example 10 and Example 1 is that the sintering process is: in the first stage, the temperature is increased to 250°C at a heating rate of 10°C / min and kept at a constant temperature for 2 hours; in the second stage, the temperature is increased to 450°C at a heating rate of 10°C / min and kept at a constant temperature for 4 hours.
[0076] Embodiment 11 of the present invention is:
[0077] The only difference between Example 11 and Example 1 is that the sintering process is: in the first stage, the temperature is increased to 250°C at a heating rate of 10°C / min and kept at a constant temperature for 2 hours; in the second stage, the temperature is increased to 550°C at a heating rate of 10°C / min and kept at a constant temperature for 4 hours.
[0078] Embodiment 12 of the present invention is:
[0079] The only difference between Example 12 and Example 1 is that the inorganic glue in S1 is replaced by silica sol.
[0080] Embodiment 13 of the present invention is:
[0081] The only difference between Example 13 and Example 1 is that the organic glue in S1 is replaced by a water-based silicone dispersion.
[0082] The comparative example of the present invention is: the EMM-8 activated powder in Example 1.
[0083] The water vapor adsorption and desorption isotherms of the glass fiber-based aluminum phosphate molecular sieve in Example 1 and the EMM-8 activated powder in the comparative example are shown in FIG. Figure 1 .like Figure 1As shown, the EMM-8 activated powder has a high saturation adsorption rate of 35.97%. Especially at low relative humidity such as 15% RH, its water vapor absorption rate increases rapidly, steeply adsorbs, and the adsorption rate is as high as 30.79%, indicating that the aluminum phosphate molecular sieve activated powder has high hygroscopic performance at low humidity, which is much higher than silica gel (about 8%) and molecular sieve (about 20%) at the same humidity. Correspondingly, the glass fiber-based aluminum phosphate molecular sieve of Example 1 has the same excellent performance: it has a saturation adsorption rate of 27.01%, and at 15% RH, the water vapor absorption rate rises steeply, up to 22.79%, indicating that the dehumidification wheel made of glass fiber-based aluminum phosphate molecular sieve can achieve deep dehumidification in the field of lithium-ion batteries.
[0084] The X-ray diffraction (XRD) spectra of the glass fiber-based aluminum phosphate molecular sieve in Test Example 1 and the EMM-8 activated powder in Comparative Example are shown in FIG. Figure 2 .Depend on Figure 2 It can be seen that the diffraction peaks presented by the glass fiber-based aluminum phosphate molecular sieve of Example 1 are completely matched with the diffraction peaks of the comparative example having the characteristics of the SFO structure aluminum phosphate molecular sieve (EMM-8), indicating that the surface loading process of the aluminum phosphate molecular sieve powder in the glass fiber dipping and programmed sintering process does not destroy the inherent topological structure of EMM-8.
[0085] The N2 adsorption and desorption curves and pore size and distribution curves of the glass fiber-based aluminum phosphate molecular sieve in Example 1 and the EMM-8 activated powder in the comparative example are shown in FIG. Figure 3 .Depend on Figure 3 It can be seen that the N2 adsorption-desorption isotherms of the comparative example completely overlap, and the comparative example exhibits a high adsorption capacity at a low relative pressure of about 0.05, indicating that the comparative example is completely microporous, and its specific surface area is as high as 773.32 m 2 / g. Example 1 has the same N2 adsorption-desorption isotherm curve as the comparative example. Due to the introduction of the glass fiber substrate, its specific surface area is reduced, but it still shows 462.34m 2 The pore size and distribution curves show that they are all in the micropore range, which is consistent with their N2 adsorption-desorption isotherms.
[0086] The differential thermal gravimetric (DTG) curves of the glass fiber-based aluminum phosphate molecular sieve in Example 1 and the EMM-8 activated powder in the comparative example are shown in FIG. Figure 4 .Depend on Figure 4It can be seen that the desorption peak temperature of Example 1 and the comparative example at different heating rates is relatively low, which is 60-90°C, indicating that the aluminum phosphate molecular sieve and the glass fiber-based aluminum phosphate molecular sieve have a relatively low desorption temperature, which is much lower than the traditional silica gel (150°C) and molecular sieve (250°C). In comparison, since the glass fiber substrate is uniformly dispersed on the aluminum phosphate molecular sieve, it can effectively reduce its heat and mass transfer resistance in the water vapor adsorption and desorption process. Through the desorption peak temperature at different heating rates and the Kissinger equation, further linear fitting can be performed to obtain its desorption activation energy (Ed). The results show that the Ed of the comparative example and Example 1 are 58.99kJ / mol and 41.61kJ / mol, respectively. It shows that the aluminum phosphate molecular sieve is loaded on the glass fiber substrate, and its desorption energy consumption is further reduced. If a dehumidification wheel is made, its desorption energy consumption is significantly reduced.
[0087] The stability test results of the glass fiber-based aluminum phosphate molecular sieve in Test Example 1 and the EMM-8 activated powder in Comparative Example for 15 cycles of water vapor adsorption-desorption are shown in Figure 1. Figure 5 The test conditions are: adsorption at 25℃, 60%RH, and desorption at 80℃. Figure 5 It can be seen that after 15 consecutive cycles of water vapor adsorption and desorption, the adsorption amount of water vapor by Example 1 and the comparative example did not change significantly, and was stabilized in the range of 0.225g / g and 0.325g / g, respectively, indicating that both have excellent cycle stability and adsorption performance. In addition, after desorption at 80°C, the corresponding residual water amounts were 0.025g / g and 0.028g / g, respectively, indicating that they have a lower desorption temperature and they can easily desorb the adsorbed water vapor. In comparison, loading the aluminum phosphate molecular sieve on the substrate improves the desorption of the molecular sieve more completely, indicating that its heat and mass transfer resistance is reduced, which is conducive to desorption.
[0088] Embodiment 14 of the present invention is: a method for preparing a glass fiber-based aluminum phosphate molecular sieve moisture absorbent, the steps are as follows:
[0089] S1: Under stirring, according to the solid content mass percentage of Si partially substituted AlPO4-5 / organic glue / inorganic glue = 50 / 25 / 25, 5g Si partially substituted AlPO4-5 activated powder, 25g 10wt% polyacrylate emulsion, 12.5g 20wt% silica-alumina sol were weighed in sequence and added into 80mL deionized water, and then 2.04g 30wt% polyvinyl pyrrolidone dispersant (0.5wt% slurry) was added, and stirring was continued until a uniformly dispersed aluminum phosphate molecular sieve dispersion slurry was formed.
[0090] S2: Take a glass fiber paper with a size of 10×10 cm (weight 25g / m 2), immersed in the aluminum phosphate molecular sieve dispersion slurry, after being completely wetted, taken out and dried, and then transferred to a muffle furnace for programmed temperature sintering. The sintering process is: in the first stage, the temperature is increased to 120°C at a heating rate of 10°C / min, and the temperature is kept constant for 2h; in the second stage, the temperature is increased to 450°C at a heating rate of 10°C / min, and the temperature is kept constant for 4h, and then naturally cooled to room temperature to obtain a glass fiber-based aluminum phosphate molecular sieve.
[0091] Embodiment 15 of the present invention is: a method for preparing a glass fiber-based aluminum phosphate molecular sieve moisture absorbent, the steps are as follows:
[0092] S1: Under stirring, according to the solid content mass percentage of SAPO-34 / organic glue / inorganic glue = 80 / 2 / 18, 8g SAPO-34 activated powder, 2g 10wt% epoxy resin emulsion, and 9g 20wt% titanium sol were weighed in sequence and added into 80mL deionized water, and then 16.5g 30wt% sodium gluconate dispersant (5wt% slurry) was added, and stirring was continued until a uniformly dispersed aluminum phosphate molecular sieve dispersion slurry was formed.
[0093] S2: Take a glass fiber paper with a size of 10×10 cm (weight 25g / m 2 ), immersed in the aluminum phosphate molecular sieve dispersion slurry, after being completely wetted, taken out and dried, and then transferred to a muffle furnace for programmed temperature sintering. The sintering process is: in the first stage, the temperature is increased to 300°C at a heating rate of 10°C / min, and the temperature is kept constant for 2h; in the second stage, the temperature is increased to 600°C at a heating rate of 10°C / min, and the temperature is kept constant for 4h, and then naturally cooled to room temperature to obtain a glass fiber-based aluminum phosphate molecular sieve.
[0094] Example 16 of the present invention is: a glass fiber-based aluminum phosphate molecular sieve desiccant prepared by the preparation method of Example 1.
[0095] Embodiment 17 of the present invention is: the use of the glass fiber-based aluminum phosphate molecular sieve desiccant of Embodiment 16 as a desiccant for a low-temperature desorption dehumidification wheel.
[0096] In summary, the present invention provides a glass fiber-based aluminum phosphate molecular sieve moisture absorbent and its preparation method and application, which has the following advantages compared with the existing traditional glass fiber-based adsorbent silica gel and molecular sieve technology:
[0097] (1) Aluminum phosphate molecular sieve is selected as the adsorbent. Aluminum phosphate molecular sieve has the characteristics of high moisture absorption rate at low humidity, low desorption temperature and high temperature resistance. The dehumidification wheel made of it has the advantages of high dehumidification efficiency, low operating energy consumption and good cycle stability.
[0098] (2) Aqueous composite glue is added to the aluminum phosphate molecular sieve dispersion slurry, and its adhesion properties are utilized to make the aluminum phosphate molecular sieve highly loaded on the surface of the substrate and not easy to fall off.
[0099] (3) Glass fiber paper is used as the substrate, which can be processed into a honeycomb corrugated wheel block together with aluminum phosphate molecular sieve, which can greatly reduce the mass transfer resistance of the adsorbent water molecules in the honeycomb channel, reduce the pressure drop, and thus increase the mass transfer rate of the adsorbent during the adsorption and desorption process.
[0100] (4) Programmed temperature sintering is used to minimize the deformation of the bulk adsorbent formed by the combination of the substrate and the adsorbent during the heating process and prevent the adsorbent from cracking during water loss and organic matter decomposition; at the same time, the organic components in the substrate and the impregnation solution are removed to improve the cyclic stability of the aluminum phosphate molecular sieve.
[0101] (5) It has the characteristics of simple process, green and environmental protection, large moisture absorption capacity, low-temperature desorption and stable performance, and can achieve deep dehumidification of low-temperature desorption dehumidification wheel.
[0102] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a glass fiber-based aluminum phosphate molecular sieve moisture absorbent, characterized in that: The following steps are involved: S1: under stirring, adding aluminum phosphate molecular sieve and aqueous composite glue into deionized water to obtain a mixed solution, and then adding a dispersant into the mixed solution to form an aluminum phosphate molecular sieve dispersed slurry; S2: Dipping glass fiber paper in the aluminum phosphate molecular sieve dispersion slurry, taking it out and drying it after it is completely soaked, and then sintering it to obtain the glass fiber-based aluminum phosphate molecular sieve.
2. The method for preparing the glass fiber-based aluminum phosphate molecular sieve moisture absorbent according to claim 1, characterized in that: The aluminum phosphate molecular sieve is an aluminum phosphate series with a topological structure.
3. The method for preparing the glass fiber-based aluminum phosphate molecular sieve moisture absorbent according to claim 1, characterized in that: The aluminum phosphate molecular sieve includes any one of SAPO-34 with CHA structure, AlPO4-5 with AFI structure, AlPO-42 with LTA structure, EMM-8 with SFO structure and derivatives thereof.
4. The method for preparing the glass fiber-based aluminum phosphate molecular sieve moisture absorbent according to claim 1, characterized in that: The water-based composite glue includes inorganic glue and organic glue.
5. The method for preparing the glass fiber-based aluminum phosphate molecular sieve moisture absorbent according to claim 4, characterized in that: The inorganic adhesive accounts for 50-90wt% of the weight of the water-based composite adhesive.
6. The method for preparing the glass fiber-based aluminum phosphate molecular sieve moisture absorbent according to claim 1, characterized in that: The dispersant includes at least one of sodium polyacrylate, polyvinyl pyrrolidone, sodium gluconate and sodium hexametaphosphate.
7. The method for preparing the glass fiber-based aluminum phosphate molecular sieve moisture absorbent according to claim 1, characterized in that: In terms of solid content, the mixed solution includes: 50-80wt% of aluminum phosphate molecular sieve and 20-50wt% of water-based composite glue.
8. The method for preparing the glass fiber-based aluminum phosphate molecular sieve moisture absorbent according to claim 1, characterized in that: The sintering is performed by programmed temperature rise, wherein the temperature of the first stage of the programmed temperature rise is 120-300°C, and the temperature of the second stage is 450-600°C.
9. A glass fiber-based aluminum phosphate molecular sieve desiccant prepared by the method for preparing a glass fiber-based aluminum phosphate molecular sieve desiccant according to any one of claims 1 to 8.
10. Use of the glass fiber-based aluminum phosphate molecular sieve desiccant as claimed in claim 9 in the preparation of a low-temperature desorption dehumidification wheel.
Citation Information
Patent Citations
Method for manufacturing ultralow dew point adsorption-type desiccant rotary wheel
CN106196348A
Regular structure adsorbent and application thereof
CN106669636A
Molecular sieve dehumidification rotating wheel and preparation process thereof
CN113457376A
Preparation method and application of regional functionalized sandwich structured adsorbent
CN118122278A
Aluminium modified silica-gel adsorbent material and its preparing process
CN1586711A