Preparation method and application of catalyst for MMP synthesis

The network structure formed through chemical connection solves the problem of core-shell catalyst shell shedding, extends the service life of the catalyst and improves the efficiency of MMP synthesis.

CN119056431AInactive Publication Date: 2024-12-03SHENZHEN PRECHEM FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411561985.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-05
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the roasting and application of existing core-shell structure catalysts, due to the low degree of bonding between core-shells, the shell layer is prone to fall off, which cannot effectively extend the service life of the core catalyst.

Method used

Through chemical connection, the carrier shell and the core form a cross-linking reaction to form a mesh structure, enhancing the connection stability between the core and the shell and preventing the shell from falling off. The specific steps include preparing the active seed liquid, the carrier core and the shell, forming a core-shell structure through a coupling agent and an initiator, and finally impregnating and calculating with the MMP solution.

Benefits of technology

The stable connection between the core and the shell is achieved, the service life of the catalyst is extended, the number of catalyst recycling times is increased, and the conversion rate of methyl acrylate synthesized by MMP is increased.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the field of chemical synthesis, and particularly relates to a preparation method and application of a catalyst for MMP synthesis, and the preparation method comprises the following steps: S1, preparing an active seed solution: adding sodium methoxide and a monomer into water, and stirring to form the active seed solution; s2, preparing a carrier inner core: adding the inner layer shell into a seed solution for dipping, drying and roasting to obtain the carrier inner core containing an active component; s3, preparing a carrier shell: adding alumina powder and a monomer into water, then adding the carrier core, a coupling agent and an initiator to react, and then roasting to form a carrier with a core-shell structure; and S4, adding the carrier with the core-shell structure into a mixed solution of methanol, methyl acrylate and MMP, dipping, drying and roasting to obtain the final catalyst. Through a chemical connection mode, the phase carrier shell and the inner core form a cross-linking reaction and form a net-shaped structure to bind the shell and the inner core, and the connection between the inner core and the shell is more stable, so that the problem that the shell layer falls off is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical synthesis, and in particular relates to a preparation method and application of a catalyst for MMP synthesis. Background Art

[0002] Methyl 3-methoxypropionate (MMP) is a colorless liquid with a special aroma. It is an important organic solvent and organic synthesis intermediate. The preparation process of MMP generally uses methanol and methyl acrylate as raw materials, and then adds sodium methoxide catalyst to react. In order to improve the activity and service life of the catalyst, the structure of the catalyst is currently improved to prepare a core-shell structured supported catalyst. At present, the preparation method of core-shell structure catalyst generally comprises first preparing a seed core, then using an adhesive to adhere a shell material to the outside of the seed core to form a core-shell structure, and finally calcining to form a core-shell structure catalyst.

[0003] However, during the calcination and application process of the catalyst prepared by the above method, the shell layer is easy to fall off due to the low degree of bonding between the core and the shell, thereby failing to achieve the purpose of extending the service life of the core catalyst. Summary of the invention

[0004] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a method for preparing a catalyst for MMP synthesis and its application. Through chemical connection, the outer shell of the phase carrier will form a cross-linking reaction with the inner core and form a network structure to bind the two, and the connection between the inner core and the outer shell is more stable, thereby avoiding the problem of shell shedding.

[0005] The specific technical solution adopted by the present invention is: A method for preparing a catalyst for MMP synthesis comprises the following steps: S1. preparing an active seed solution: adding sodium methoxide, octyl acrylate, acrylic acid, an emulsifier and water into a reaction container, and then stirring to form a suspension to form an active seed solution; S2. Preparation of carrier core: dissolving dopamine hydrochloride in a Tris-HCL buffer solution, then adding porous silica to the buffer solution, reacting at room temperature for 8-12 hours, drying to obtain an inner shell, adding the inner shell to a seed solution for immersion, drying, and calcining to obtain a carrier core containing an active component; S3, preparing a carrier shell: adding alumina powder, octyl acrylate, acrylic acid, an emulsifier and water into a reaction container, then adding a carrier core, a coupling agent and an initiator, heating to 60-80° C. and keeping the temperature for 60-90 minutes, and then calcining to form a carrier with a core-shell structure; S4. Add the core-shell structure carrier into a mixed solution of methanol, methyl acrylate and MMP, immerse, dry and calcine to obtain the final catalyst.

[0006] The active seed solution in step S1 includes, by weight, 5-10 parts of sodium methoxide, 3-5 parts of octyl acrylate, 1-2 parts of acrylic acid, and 0.2-0.5 parts of emulsifier.

[0007] The carrier core in step S2 includes, by weight, 4-6 parts of dopamine hydrochloride, 0.5-1 parts of Tris-HCL buffer solution, and 10-15 parts of porous silica.

[0008] The carrier shell in step S3 includes, by mass, 20-30 parts of alumina powder, 3-4 parts of carrier core, 3-5 parts of octyl acrylate, 1-2 parts of acrylic acid, 1-2 parts of emulsifier, 0.05-0.1 parts of coupling agent, and 0.05-0.1 parts of initiator.

[0009] The coupling agent is a silane coupling agent of an organic silicon monomer having an allyl group.

[0010] The initiator is any one of ammonium persulfate, sodium persulfate and potassium persulfate.

[0011] An application of a catalyst for MMP synthesis comprises the following steps: A. preparing catalyst; B. synthesizing MMP using the catalyst; Step A includes the following steps: S1. preparing an active seed solution: adding sodium methoxide, octyl acrylate, acrylic acid, an emulsifier and water into a reaction container, and then stirring to form a suspension to form an active seed solution; S2. Preparation of carrier core: dissolving dopamine hydrochloride in a Tris-HCL buffer solution, then adding porous silica to the buffer solution, reacting at room temperature for 8-12 hours, drying to obtain an inner shell, adding the inner shell to a seed solution for immersion, drying, and calcining to obtain a carrier core containing an active component; S3, preparing a carrier shell: adding alumina powder, octyl acrylate, acrylic acid, an emulsifier and water into a reaction container, then adding a carrier core, a coupling agent and an initiator, heating to 60-80° C. and keeping the temperature for 60-90 minutes, and then calcining to form a carrier with a core-shell structure; S4, adding the core-shell structure carrier to a mixed solution of methanol, methyl acrylate and MMP, immersing for 4-8 hours, drying and calcining for 4 hours to obtain the final catalyst; Step B includes the following steps: S5, adding methanol and methyl acrylate into a reaction kettle, adding hydroquinone monomethyl ether and a catalyst, mixing evenly, and reacting at 70-80° C. for 2-3 hours to obtain a reaction solution; S6. Add ammonium carbonate to the reaction solution and stir evenly. After reacting for 10-20 minutes, filter the solution and put the filtrate into a distillation kettle for vacuum distillation to obtain a finished MMP product.

[0012] The temperature of the reduced pressure distillation is 150-160° C., and the vacuum degree is -0.85 to 0.1 MPa.

[0013] The MMP finished product comprises, by weight, 100-120 parts of methanol, 240-260 parts of methyl acrylate, 30-40 parts of catalyst, 0.1-0.2 parts of hydroquinone monomethyl ether, and 2.5-3 parts of ammonium carbonate.

[0014] The beneficial effects of the present invention are: 1. The core and shell of the core-shell catalyst in the present invention are chemically connected. Compared with the traditional physical connection method, since the core of the carrier contains a cross-linking monomer, the carrier shell will form a cross-linking reaction with the core and form a network structure to bind the two. The chemical connection method will make the connection between the core and the shell more stable, thereby avoiding the problem of shell shedding.

[0015] 2. The core-shell catalyst of the present invention has a double-layer porous structure, which can form a larger surface area. At the same time, the outer shell layer can provide good protection for the inner core, which is beneficial to prolong the service life of the catalyst and increase its recycling times. DETAILED DESCRIPTION

[0016] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. 1. Specific embodiments Example 1 S1. Prepare active seed solution: add 8 parts of sodium methoxide, 4 parts of octyl acrylate, 1.5 parts of acrylic acid, 0.3 parts of emulsifier and water into a reaction container, and then stir to form a suspension to form an active seed solution; S2. Preparation of carrier core: dissolving 5 parts of dopamine hydrochloride in 0.8 parts of Tris-HCL buffer solution, then adding 12 parts of porous silica to the buffer solution, reacting at room temperature for 10 hours, drying to obtain an inner shell, adding the inner shell to the seed solution for immersion for 6 hours, drying, and calcining at 550° C. for 5 hours to obtain a carrier core containing active components; S3, preparing a carrier shell: adding 25 parts of alumina powder, 4 parts of octyl acrylate, 1.5 parts of acrylic acid, 1.5 parts of an emulsifier and water into a reaction container, then adding 3.5 parts of a carrier core, 0.08 parts of a coupling agent and 0.08 parts of an initiator, heating to 70°C and keeping the temperature for 80 minutes, and then calcining at 600°C for 5 hours to form a core-shell structure carrier; S4. Add the core-shell structure carrier into a mixed solution of methanol, methyl acrylate and MMP, immerse for 6 hours, dry and calcine for 4 hours to obtain the final catalyst.

[0018] Example 2 S1, preparing active seed solution: adding 5 parts of sodium methoxide, 3 parts of octyl acrylate, 1 part of acrylic acid, 0.2 parts of emulsifier and water into a reaction container, and then stirring to form a suspension to form an active seed solution; S2. Preparation of carrier core: dissolving 4 parts of dopamine hydrochloride in 0.5 parts of Tris-HCL buffer solution, then adding 10 parts of porous silica to the buffer solution, reacting at room temperature for 8 hours, drying to obtain an inner shell, adding the inner shell to the seed solution for immersion for 6 hours, drying, and calcining at 550° C. for 5 hours to obtain a carrier core containing active components; S3, preparing a carrier shell: adding 20 parts of alumina powder, 3 parts of octyl acrylate, 1 part of acrylic acid, 1 part of emulsifier and water into a reaction container, then adding 3 parts of carrier core, 0.05 parts of coupling agent and 0.05 parts of initiator, heating to 60°C and keeping warm for 90 minutes, and then calcining at 600°C for 5 hours to form a core-shell structure carrier; S4. Add the core-shell structure carrier into a mixed solution of methanol, methyl acrylate and MMP, immerse for 6 hours, dry and calcine for 4 hours to obtain the final catalyst.

[0019] Example 3 S1. Prepare active seed solution: add 10 parts of sodium methoxide, 5 parts of octyl acrylate, 2 parts of acrylic acid, 0.5 parts of emulsifier and water into a reaction container, and then stir to form a suspension to form an active seed solution; S2. Preparation of carrier core: 6 parts of dopamine hydrochloride are dissolved in 1 part of Tris-HCL buffer solution, and then 15 parts of porous silica are added to the buffer solution, reacted at room temperature for 12 hours, dried to obtain an inner shell, added the inner shell to the seed solution for immersion for 6 hours, dried, and calcined at 550° C. for 5 hours to obtain a carrier core containing active components; S3, preparing a carrier shell: adding 30 parts of alumina powder, 5 parts of octyl acrylate, 2 parts of acrylic acid, 2 parts of emulsifier and water into a reaction container, then adding 4 parts of carrier core, 0.1 parts of coupling agent and 0.1 parts of initiator, heating to 80°C and keeping warm for 60 minutes, and then calcining at 600°C for 5 hours to form a core-shell structure carrier; S4. Add the core-shell structure carrier into a mixed solution of methanol, methyl acrylate and MMP, immerse for 6 hours, dry and calcine for 4 hours to obtain the final catalyst.

[0020] Example 4 S1. Prepare active seed solution: add 7.8 parts of sodium methoxide, 4.6 parts of octyl acrylate, 1.8 parts of acrylic acid, 0.4 parts of emulsifier and water into a reaction container, and then stir to form a suspension to form an active seed solution; S2. Preparation of carrier core: 4.8 parts of dopamine hydrochloride were dissolved in 0.7 parts of Tris-HCL buffer solution, and then 13 parts of porous silica were added to the buffer solution, reacted at room temperature for 10 hours, dried to obtain an inner shell, added the inner shell to the seed solution for immersion for 9 hours, dried, and calcined at 650° C. for 6 hours to obtain a carrier core containing active components; S3, preparing a carrier shell: adding 28 parts of alumina powder, 4.6 parts of octyl acrylate, 1.8 parts of acrylic acid, 1.8 parts of emulsifier and water into a reaction container, then adding 3.6 parts of carrier core, 0.08 parts of coupling agent and 0.08 parts of initiator, heating to 72°C and keeping warm for 75 minutes, and then calcining at 600°C for 5 hours to form a core-shell structure carrier; S4. Add the core-shell structure carrier into a mixed solution of methanol, methyl acrylate and MMP, immerse for 6 hours, dry and calcine for 4 hours to obtain the final catalyst.

[0021] Example 5 S1. Prepare active seed solution: add 24 parts of sodium methoxide, 3.2 parts of octyl acrylate, 1.2 parts of acrylic acid, 0.2 parts of emulsifier and water into a reaction container, and then stir to form a suspension to form an active seed solution; S2. Preparation of carrier core: 4.2 parts of dopamine hydrochloride were dissolved in 0.6 parts of Tris-HCL buffer solution, and then 10 parts of porous silica were added to the buffer solution, reacted at room temperature for 8 hours, dried to obtain an inner shell, added the inner shell to the seed solution for immersion for 6 hours, dried, and calcined at 700° C. for 5 hours to obtain a carrier core containing active components; S3, preparing a carrier shell: adding 22 parts of alumina powder, 3.2 parts of octyl acrylate, 1.2 parts of acrylic acid, 1.1 parts of an emulsifier and water into a reaction container, then adding 3.2 parts of a carrier core, 0.06 parts of a coupling agent and 0.06 parts of an initiator, heating to 65°C and keeping the temperature for 85 minutes, and then calcining at 600°C for 5 hours to form a core-shell structure carrier; S4. Add the core-shell structure carrier into a mixed solution of methanol, methyl acrylate and MMP, immerse for 6 hours, dry and calcine for 4 hours to obtain the final catalyst.

[0022] Comparative Example 1 S1. preparing an active seed solution: adding 8 parts of sodium methoxide and water into a reaction container, and then stirring to form a solution to form an active seed solution; S2. Preparation of carrier core: dissolving 5 parts of dopamine hydrochloride in 0.8 parts of Tris-HCL buffer solution, then adding 12 parts of porous silica to the buffer solution, reacting at room temperature for 10 hours, drying to obtain an inner shell, adding the inner shell to the seed solution for immersion for 6 hours, drying, and calcining at 550° C. for 5 hours to obtain a carrier core containing active components; S3, preparing a carrier shell: adding 25 parts of alumina powder, 8 parts of aluminum sol and water into a reaction container, then adding 3.5 parts of a carrier core and dispersing them evenly to obtain a slurry, and then calcining at 600° C. for 5 h to form a core-shell structure carrier; S4. Add the core-shell structure carrier into a mixed solution of methanol, methyl acrylate and MMP, immerse for 6 hours, dry and calcine for 4 hours to obtain the final catalyst.

[0023] 2. Performance Test The catalysts prepared in Examples 1-5 and Comparative Example 1 were used to prepare MMP. After the preparation, the catalysts were taken out, and then the MMP was prepared again. The process was repeated several times, and the conversion rate of methyl acrylate in each reaction was tested. The test results are shown in Table 1. The preparation process of MMP is as follows: 100g of methanol and 250g of methyl acrylate are added to a reactor, 0.1g of hydroquinone monomethyl ether and 30g of a catalyst are added, the mixture is evenly mixed and reacted at 75°C for 2h to obtain a reaction solution, 2.8g of ammonium carbonate is added to the reaction solution and stirred evenly, the reaction is performed for 15min and then filtered, the filtrate is kneaded into a distillation kettle for reduced pressure distillation to obtain a finished MMP product.

[0024] Table 1 It can be seen from Table 1 that the catalysts prepared in Examples 1-5 not only have a high conversion rate of methyl acrylate in the initial use, but also have a low rate of decrease in the conversion rate of methyl acrylate, and the catalysts still have high activity after five uses.

[0025] However, for the catalyst prepared in Comparative Example 1, although its core-shell structure can slow down the decline rate of its active components in the initial stage, its activity decline rate increases sharply after repeated use. This is because its shell layer falls off after repeated use.

[0026] In addition, by comparing the initial methyl acrylate conversion rates of Example 1 and Comparative Example 1, it can be seen that when the catalyst in Example 1 is used to prepare MMP, the conversion rate of methyl acrylate is higher. This is because the monomers and emulsifiers in the seed solution make the active components more evenly distributed and increase the adhesion between the active components and the silica carrier.

[0027] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a catalyst for MMP synthesis, characterized in that: The following steps are involved: S1. preparing an active seed solution: adding sodium methoxide, octyl acrylate, acrylic acid, an emulsifier and water into a reaction container, and then stirring to form a suspension to form an active seed solution; S2. Preparation of carrier core: dissolving dopamine hydrochloride in a Tris-HCL buffer solution, then adding porous silica to the buffer solution, reacting at room temperature for 8-12 hours, drying to obtain an inner shell, adding the inner shell to a seed solution for immersion, drying, and calcining to obtain a carrier core containing an active component; S3, preparing a carrier shell: adding alumina powder, octyl acrylate, acrylic acid, an emulsifier and water into a reaction container, then adding a carrier core, a coupling agent and an initiator, heating to 60-80° C. and keeping the temperature for 60-90 minutes, and then calcining to form a carrier with a core-shell structure; S4. Add the core-shell structure carrier into a mixed solution of methanol, methyl acrylate and MMP for immersion, dry and then calcine to obtain the final catalyst.

2. The method for preparing a catalyst for MMP synthesis according to claim 1, characterized in that: The active seed solution in step S1 includes, by weight, 5-10 parts of sodium methoxide, 3-5 parts of octyl acrylate, 1-2 parts of acrylic acid, and 0.2-0.5 parts of emulsifier.

3. The method for preparing a catalyst for MMP synthesis according to claim 1, characterized in that: The carrier core in step S2 includes, by weight, 4-6 parts of dopamine hydrochloride, 0.5-1 parts of Tris-HCL buffer solution, and 10-15 parts of porous silica.

4. The method for preparing a catalyst for MMP synthesis according to claim 1, characterized in that: The carrier shell in step S3 includes, by mass, 20-30 parts of alumina powder, 3-4 parts of carrier core, 3-5 parts of octyl acrylate, 1-2 parts of acrylic acid, 1-2 parts of emulsifier, 0.05-0.1 parts of coupling agent, and 0.05-0.1 parts of initiator.

5. The method for preparing a catalyst for MMP synthesis according to claim 1, characterized in that: The coupling agent is a silane coupling agent of an organic silicon monomer having an allyl group.

6. The method for preparing a catalyst for MMP synthesis according to claim 1, characterized in that: The initiator is any one of ammonium persulfate, sodium persulfate and potassium persulfate.

7. An application of a catalyst for MMP synthesis, characterized in that, The following steps are involved: A. preparing catalyst; B. synthesizing MMP using the catalyst; Step A includes the following steps: S1. preparing an active seed solution: adding sodium methoxide, octyl acrylate, acrylic acid, an emulsifier and water into a reaction container, and then stirring to form a suspension to form an active seed solution; S2. Preparation of carrier core: dissolving dopamine hydrochloride in a Tris-HCL buffer solution, then adding porous silica to the buffer solution, reacting at room temperature for 8-12 hours, drying to obtain an inner shell, adding the inner shell to a seed solution for immersion, drying, and calcining to obtain a carrier core containing an active component; S3, preparing a carrier shell: adding alumina powder, octyl acrylate, acrylic acid, an emulsifier and water into a reaction container, then adding a carrier core, a coupling agent and an initiator, heating to 60-80° C. and keeping the temperature for 60-90 minutes, and then calcining to form a carrier with a core-shell structure; S4, adding the core-shell structure carrier into a mixed solution of methanol, methyl acrylate and MMP, impregnating, drying and calcining to obtain the final catalyst; Step B includes the following steps: S5, adding methanol and methyl acrylate into a reaction kettle, adding hydroquinone monomethyl ether and a catalyst, mixing evenly, and reacting at 70-80° C. for 2-3 hours to obtain a reaction solution; S6. Add ammonium carbonate to the reaction solution and stir evenly. After reacting for 10-20 minutes, filter the solution and put the filtrate into a distillation kettle for vacuum distillation to obtain a finished MMP product.

8. The use of a catalyst for MMP synthesis according to claim 7, characterized in that: The temperature of the reduced pressure distillation is 150-160° C., and the vacuum degree is -0.85 to 0.1 MPa.

9. The use of a catalyst for MMP synthesis according to claim 7, characterized in that: The MMP finished product comprises, by weight, 100-120 parts of methanol, 240-260 parts of methyl acrylate, 30-40 parts of catalyst, 0.1-0.2 parts of hydroquinone monomethyl ether, and 2.5-3 parts of ammonium carbonate.